Flame-retardant antistatic fiber and preparation method thereof
By adding composite antistatic agents, flame retardants and modified fly ash to the polyester fiber, the poor antistatic and flammability problems of polyester fibers are solved, and its flame retardancy and mechanical properties are improved. It is suitable for high-demand Application field.
Patent Information
- Application Number
- CN202411390492.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyester fibers have poor antistatic properties due to their tightly arranged molecules and lack of hydrophilic groups, and have problems such as flammability and poor dispersion of fillers, which limits its application in the fields of aviation, transportation, medical care, etc.
Polyester is used as the main material, and composite antistatic agents, flame retardants, antibacterial agents and modified fly ash are added. By synthesizing modified phosphate compounds and modified fly ash, the flame retardancy and antistatic properties of the fiber are improved. and mechanical properties.
It achieves good flame retardancy, antistatic properties and mechanical properties of the fiber, and is suitable for high-demand application areas, enhancing its commercial application value.
Smart Images

Figure BDA0005072273730000081 
Figure BDA0005072273730000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of fibers, and in particular to a flame-retardant antistatic fiber and a preparation method thereof. Background Art
[0002] Polyester fiber, commonly known as "polyester", is a synthetic fiber obtained by spinning polyester formed by the condensation of organic dibasic acids and diols. It is one of the most widely used chemical fibers at present. It has excellent physical and chemical properties, such as high strength, excellent hydrolysis resistance and heat resistance, etc., and low cost. It is widely used in people's production and life. At the same time, polyester fiber also has strong wear resistance and is one of the materials with high strength requirements for making sportswear, canvas, backpacks, etc.
[0003] Although polyester fiber has many excellent characteristics mentioned above, with the expansion of its application fields, in some special fields, such as aviation, transportation, medical and other fields, the polyester fiber used needs to meet certain anti-static requirements, but the polyester fiber has poor anti-static properties due to its tight molecular arrangement and lack of hydrophilic groups; and polyester fiber is a flammable fiber, which makes the products made of polyester fiber have certain safety hazards; in addition, some filler components are often added to polyester fiber to improve the mechanical properties and heat resistance of the fiber, but these fillers may have poor dispersion problems, resulting in a decrease in fiber performance. These reasons will limit the application and development of polyester fiber.
[0004] Patent CN 104278349B discloses an antistatic-flame-retardant copolyester fiber and a preparation method thereof, comprising components such as polybutylene terephthalate / adipate, an antistatic agent, a phosphorus-based flame retardant and an inorganic nanopowder, and having good antistatic, flame-retardant and mechanical properties. However, the inorganic nanopowder selected in the application is nano-scale silicon dioxide, calcium carbonate or magnesium carbonate or barium sulfate, which has the problem of easy agglomeration and poor dispersion, and may cause a decrease in the mechanical properties of the fiber.
[0005] Therefore, there is an urgent need in the market for a fiber with good flame retardancy, antistatic properties and mechanical properties. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention uses polyester as the main material, adds a composite antistatic agent, a flame retardant, an antibacterial agent and modified fly ash to synthesize a flame retardant antistatic fiber, which has good flame retardancy, antistatic and mechanical properties.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] On one hand, the present invention provides a flame retardant antistatic fiber, which comprises the following raw materials by weight: 90-110 parts of polyester, 5-15 parts of composite antistatic agent, 5-10 parts of flame retardant, 4-10 parts of antibacterial agent and 1-4 parts of modified fly ash.
[0009] The flame retardant is tripolyphosphate or ammonium polyphosphate; and the antibacterial agent is a silver ion antibacterial agent.
[0010] In some embodiments of the present invention, the polyester is any one of polyethylene terephthalate, polytrimethylene terephthalate, and polybutylene terephthalate.
[0011] In some embodiments of the present invention, the composite antistatic agent is a mixture of a modified phosphate ester compound and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1:(0.8-2).
[0012] Preferably, the mass ratio of the modified phosphate ester compound to isomeric tridecyl alcohol polyoxyethylene ether sodium sulfate is 1:1.5.
[0013] In some embodiments of the present invention, the method for preparing the modified phosphate ester compound comprises the following steps:
[0014] (1) epichlorohydrin is added dropwise to a sodium hydrogen phosphate aqueous solution, heated to 80-90° C., stirred for 3.5-4.5 hours, rotary evaporated, anhydrous ethanol is added, stirred, filtered, recrystallized, and dried to obtain product 1 for later use;
[0015] (2) adding myristic acid to a reaction vessel, introducing an inert gas, heating to 115-125° C., adding (3-amino-2,2-difluoropropyl)dimethylamine, continuing to heat to 145-155° C., stirring, distilling under reduced pressure, recrystallizing, and drying to obtain product 2 for later use;
[0016] (3) adding the product 1 of step (1) and the product 2 of step (2) to an ethanol solution in sequence, heating to 80-90° C., stirring, distilling, extracting, distilling, drying, adding anhydrous ethanol, stirring, filtering, and drying to obtain a modified phosphate ester compound.
[0017] Wherein, in the step (1), the molar ratio of epichlorohydrin to disodium hydrogen phosphate in the disodium hydrogen phosphate aqueous solution is 1:(1-1.4).
[0018] Preferably, in step (1), the molar ratio of epichlorohydrin to disodium hydrogen phosphate in the disodium hydrogen phosphate aqueous solution is 1:1.2.
[0019] In some embodiments of the present invention, in step (2), the molar ratio of myristic acid to (3-amino-2,2-difluoropropyl)dimethylamine is 1:(1-2).
[0020] Preferably, in step (2), the molar ratio of myristic acid to (3-amino-2,2-difluoropropyl)dimethylamine is 1:1.5.
[0021] In some embodiments of the present invention, in step (3), the mass ratio of product 1 to product 2 is 1:(1.5-2).
[0022] Preferably, in step (3), the mass ratio of product 1 to product 2 is 1:1.875.
[0023] Polyester fiber has many advantages such as good wear resistance, good wrinkle resistance, easy care and good elasticity. It is one of the most widely used chemical fibers. However, due to the tight molecular arrangement and lack of hydrophilic groups, polyester fiber generally has poor antistatic properties.
[0024] On the one hand, the applicant uses disodium hydrogen phosphate and epichlorohydrin as raw materials to synthesize product 1. On the other hand, the applicant uses myristic acid and (3-amino-2,2-difluoropropyl) dimethylamine as raw materials, and utilizes the condensation reaction of carboxyl and amino groups to synthesize a tertiary amine (product 2) having a fatty long chain and an amide bond structure. Product 1 and product 2 are further combined through a quaternization reaction to synthesize a modified phosphate ester compound. The modified phosphate ester compound contains both cationic head groups and anionic head groups in its structure, which makes up for the shortcomings of simple cationic surfactants that easily discolor the fiber and have poor compatibility with other additives, and has good antistatic and bactericidal properties. In addition, the structure has both amide groups and phosphate groups, which can have good compatibility with the skin, mild performance and easy biodegradation, and the amide bonds and fluorine bonds also improve the thermal stability of the modified phosphate ester compound and improve the durability of the modified phosphate ester compound.
[0025] Furthermore, the applicant mixed the modified phosphate ester compound and isomeric tridecanol polyoxyethylene ether sodium sulfate in a specific mass ratio, which can synergistically enhance the spreading and wetting ability of the composite antistatic agent, and has a good synergistic effect on emulsification, wetting and foaming properties.
[0026] In some embodiments of the present invention, the method for preparing the modified fly ash comprises the following steps:
[0027] 1) adding fly ash to anhydrous ethanol, stirring, heating to 55-65° C., adding stearic acid and 11-aminoundecyltriethoxysilane in sequence, stirring, cooling to room temperature, filtering, and drying to obtain activated fly ash for later use;
[0028] 2) The activated fly ash, acrylamide, ammonium persulfate and N,N-methylenebisacrylamide in step 1) are mixed, stirred, deionized water is added, stirred, molded, and demolded to obtain modified fly ash.
[0029] In some embodiments of the present invention, in step 1), the mass ratio of fly ash, stearic acid and 11-aminoundecyltriethoxysilane is 1:(0.08-0.12):(0.1-0.2).
[0030] Preferably, in step 1), the mass ratio of fly ash, stearic acid and 11-aminoundecyltriethoxysilane is 1:0.1:0.15.
[0031] In some embodiments of the present invention, in step 2), the mass ratio of activated fly ash to acrylamide is 1:(0.2-0.3).
[0032] Preferably, in step 2), the mass ratio of activated fly ash to acrylamide is 1:0.25.
[0033] Fly ash is an industrial waste and a fine powdery substance. Its main components are silicon oxide, aluminum oxide, iron oxide, calcium oxide and other ingredients. Adding it to fibers can improve the mechanical properties and heat resistance. Fly ash also has certain flame retardancy. However, fly ash itself has certain limitations in terms of dispersibility and toughness.
[0034] On the one hand, the applicant uses stearic acid and 11-aminoundecyltriethoxysilane to modify the surface of fly ash for activation. The carboxyl structure in stearic acid and the amino structure in 11-aminoundecyltriethoxysilane enrich the active groups on the surface of fly ash, improve the dispersibility of fly ash in fiber, and thus improve the strength and heat resistance of fiber, and the long-chain alkyl structure in 11-aminoundecyltriethoxysilane can further improve the dispersibility of fly ash in fiber; on the other hand, the applicant introduces acrylamide to modify the activated fly ash, so that acrylamide is polymerized in situ to generate polyacrylamide gel with a network structure, and fly ash particles are embedded in the network structure of polyacrylamide gel, thereby effectively improving the toughness of fly ash; further, the amide bond in the polyacrylamide structure may form hydrogen bonds with the carboxyl group in stearic acid, thereby improving the stability of the modified fly ash; further, fly ash can also play a role in stabilizing the modified phosphate compound foam in the composite antistatic agent, making the fiber more stable as a whole.
[0035] Another aspect of the present invention further provides a method for preparing the flame retardant antistatic fiber described in the above technical solution, comprising the following steps:
[0036] The polyester, composite antistatic agent, flame retardant, antibacterial agent and modified fly ash are mixed, stirred at 110-130° C. for 20-40 minutes, extruded, and melt-spun to obtain flame retardant antistatic fiber.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) The present invention uses polyester as the main material, adds a composite antistatic agent, a flame retardant, an antibacterial agent and modified fly ash to synthesize a flame retardant antistatic fiber. Through the synergistic effect of the components, the flame retardant antistatic fiber has good flame retardancy, antistatic properties and mechanical properties.
[0039] (2) The present invention uses disodium hydrogen phosphate, epichlorohydrin, myristic acid and (3-amino-2,2-difluoropropyl) dimethylamine as raw materials to prepare a modified phosphate ester compound, which has good antistatic properties, bactericidal properties and thermal stability, and is mixed with isomeric tridecanol polyoxyethylene ether sodium sulfate in a specific mass to form a composite antistatic agent, which plays a synergistic antistatic role.
[0040] (3) The present invention uses stearic acid and 11-aminoundecyltriethoxysilane to perform surface activation modification on fly ash, and then introduces acrylamide to modify the fly ash, so that the dispersibility and toughness of the fly ash are improved, thereby improving the mechanical properties and flame retardant properties of the fiber.
[0041] (4) The flame-retardant and antistatic fiber prepared by the present invention has good flame retardancy, antistatic properties and mechanical properties, can be widely used in the fiber field, and has good commercial application value. DETAILED DESCRIPTION
[0042] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0043] In the following embodiments and comparative examples, except for modified phosphate compounds and modified fly ash, the other compound monomers and related reagents used can be purchased from the market. Among them, tripolyphosphate was purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.; ammonium polyphosphate was purchased from Jinan Fuming Chemical Co., Ltd.; polyethylene terephthalate was purchased from Suzhou Chenzhituo Polymer Materials Co., Ltd.; polypropylene terephthalate was purchased from Dongguan Yingxiang Plastic Raw Materials Co., Ltd.; polybutylene terephthalate was purchased from Hubei Xinghengye Technology Co., Ltd.; and silver ion antibacterial agent was purchased from Dongguan Zhonghui Plastic Additive Co., Ltd.
[0044] Preparation Example 1
[0045] The synthesis method of the modified phosphate ester compound A comprises the following steps:
[0046] (1) 0.3 mol of epichlorohydrin was added dropwise to 0.36 mol of 50 wt% sodium dihydrogen phosphate aqueous solution, heated to 85° C., stirred for 4 h, rotary evaporated, 40 ml of anhydrous ethanol was added, stirred for 15 min, filtered, recrystallized three times with ethyl acetate and anhydrous ethanol in sequence, and dried at 40° C. for 12 h to obtain product 1 for use;
[0047] (2) 0.2 mol of myristic acid was added to a reaction vessel, nitrogen was introduced, the reaction vessel was heated to 120° C., 0.3 mol of (3-amino-2,2-difluoropropyl)dimethylamine was added, the reaction vessel was heated to 150° C., the reaction vessel was stirred for 8 h, the reaction vessel was distilled under reduced pressure, the reaction vessel was recrystallized from petroleum ether for 3 times, and the reaction vessel was dried at 40° C. for 48 h to obtain product 2 for later use;
[0048] (3) 32 g of the product 1 of step (1) and 60 g of the product 2 of step (2) were added to 105 g of a 25 wt% ethanol solution in sequence, heated to 85°C, stirred for 36 h, distilled, extracted with ether three times, distilled, dried at 40°C for 24 h, added with 50 ml of anhydrous ethanol, stirred for 15 min, filtered, and dried at 40°C for 48 h to obtain a modified phosphate ester compound A.
[0049] Preparation Example 2
[0050] The specific implementation manner of the modified phosphate ester compound B is the same as that of the modified phosphate ester compound A, except that in step (2), the molar number of (3-amino-2,2-difluoropropyl)dimethylamine is replaced with 0.18 mol.
[0051] Preparation Example 3
[0052] The specific implementation method of the modified phosphate ester compound C is the same as that of the modified phosphate ester compound A, except that in step (3), the mass of the product 2 is replaced by 41 g.
[0053] Preparation Example 4
[0054] The synthetic method of modified fly ash A comprises the following steps:
[0055] 1) Add 10 g of fly ash to 50 ml of anhydrous ethanol, stir for 15 min, heat to 60° C., add 1 g of stearic acid and 1.5 g of 11-aminoundecyltriethoxysilane in sequence, stir for 1 h, cool to room temperature, filter, and dry at 60° C. for 12 h to obtain activated fly ash for later use;
[0056] 2) 8 g of the activated fly ash prepared in step 1), 2 g of acrylamide, 0.08 g of ammonium persulfate and 0.16 g of N,N-methylenebisacrylamide were mixed and stirred for 30 s, 4.4 g of deionized water was added, and the mixture was stirred for 90 s. The mixture was molded (wrapped in plastic wrap and placed in a curing box at 20° C. and a relative humidity of 96% for 2 h), and demolded to obtain modified fly ash A.
[0057] Preparation Example 5
[0058] The specific implementation manner of modified fly ash B is the same as that of modified fly ash A, except that in step 1), the mass of stearic acid is replaced with 0.6 g.
[0059] Preparation Example 6
[0060] The specific implementation manner of modified fly ash C is the same as that of modified fly ash A, except that in step 1), the mass of 11-aminoundecyltriethoxysilane is replaced with 0.8 g.
[0061] Preparation Example 7
[0062] The specific implementation manner of modified fly ash D is the same as that of modified fly ash A, except that in step 2), the mass of acrylamide is replaced with 1.4 g.
[0063] Example 1
[0064] The invention discloses a flame retardant antistatic fiber, which comprises the following raw materials by weight: 100 parts of polyethylene terephthalate, 10 parts of composite antistatic agent, 7.5 parts of tripolyphosphate, 7 parts of silver ion antibacterial agent and 2.5 parts of modified fly ash A.
[0065] The composite antistatic agent is a mixture of modified phosphate ester compound A and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1:1.5.
[0066] The preparation method of the flame retardant antistatic fiber in this embodiment comprises the following steps:
[0067] Polyethylene terephthalate, composite antistatic agent, tripolyphosphate, silver ion antibacterial agent and modified fly ash A are mixed, stirred at 120°C for 30 minutes, extruded, and melt-spun at 280°C to obtain flame-retardant antistatic fibers.
[0068] Example 2
[0069] The invention discloses a flame retardant antistatic fiber, which comprises the following raw materials by weight: 90 parts of polytrimethylene terephthalate, 5 parts of composite antistatic agent, 5 parts of ammonium polyphosphate, 4 parts of silver ion antibacterial agent and 2.5 parts of modified fly ash A.
[0070] The composite antistatic agent is a mixture of modified phosphate ester compound A and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1:0.8.
[0071] The preparation method of the flame retardant antistatic fiber in this embodiment comprises the following steps:
[0072] Polytrimethylene terephthalate, a composite antistatic agent, ammonium polyphosphate, a silver ion antibacterial agent and modified fly ash A are mixed, stirred at 110° C. for 40 minutes, extruded, and melt-spun at 270° C. to obtain a flame-retardant antistatic fiber.
[0073] Example 3
[0074] The invention discloses a flame retardant antistatic fiber, which comprises the following raw materials by weight: 110 parts of polybutylene terephthalate, 15 parts of composite antistatic agent, 10 parts of ammonium polyphosphate, 10 parts of silver ion antibacterial agent and 2.5 parts of modified fly ash A.
[0075] The composite antistatic agent is a mixture of modified phosphate ester compound A and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1:2.
[0076] The preparation method of the flame retardant antistatic fiber in this embodiment comprises the following steps:
[0077] Polybutylene terephthalate, composite antistatic agent, ammonium polyphosphate, silver ion antibacterial agent and modified fly ash A are mixed, stirred at 130°C for 20 minutes, extruded, and melt-spun at 290°C to obtain flame-retardant antistatic fibers.
[0078] Example 4
[0079] The invention discloses a flame retardant antistatic fiber, which comprises the following raw materials by weight: 95 parts of polyethylene terephthalate, 10 parts of a composite antistatic agent, 6 parts of tripolyphosphate, 6 parts of a silver ion antibacterial agent and 1 part of modified fly ash A.
[0080] The composite antistatic agent is a mixture of modified phosphate ester compound A and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1:1.5.
[0081] The preparation method of the flame retardant antistatic fiber in this embodiment is the same as that in Embodiment 1.
[0082] Example 5
[0083] The invention discloses a flame retardant antistatic fiber, which comprises the following raw materials by weight: 105 parts of polyethylene terephthalate, 10 parts of a composite antistatic agent, 9 parts of tripolyphosphate, 8 parts of a silver ion antibacterial agent and 4 parts of modified fly ash A.
[0084] The composite antistatic agent is a mixture of modified phosphate ester compound A and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1:1.5.
[0085] The preparation method of the flame retardant antistatic fiber in this embodiment is the same as that in Embodiment 1.
[0086] Example 6
[0087] This embodiment provides a flame-retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified phosphate ester compound A is replaced by an equal amount of the modified phosphate ester compound B.
[0088] Example 7
[0089] This embodiment provides a flame-retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified phosphate ester compound A is replaced by an equal amount of the modified phosphate ester compound C.
[0090] Example 8
[0091] This embodiment provides a flame retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that modified fly ash B replaces modified fly ash A in equal amounts.
[0092] Example 9
[0093] This embodiment provides a flame retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified fly ash A is replaced by the modified fly ash C in equal amounts.
[0094] Example 10
[0095] This embodiment provides a flame retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Embodiment 1, except that modified fly ash D replaces modified fly ash A in equal amounts.
[0096] Comparative Example 1
[0097] This comparative example provides a flame retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that a conventional phosphate antistatic agent OP-10 is used to replace the modified phosphate type compound A in an equal amount.
[0098] Comparative Example 2
[0099] This comparative example provides a flame retardant antistatic fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that a modified phosphate ester compound A is used to replace an equal amount of the composite antistatic agent.
[0100] Comparative Example 3
[0101] This comparative example provides a flame-retardant antistatic fiber and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of isomeric tridecanol polyoxyethylene ether sodium sulfate is used to replace the composite antistatic agent.
[0102] Comparative Example 4
[0103] This comparative example provides a flame retardant antistatic fiber and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that fly ash is used in an equal amount to replace modified fly ash A.
[0104] Performance Testing
[0105] The flame retardancy, antistatic properties and mechanical properties of the flame retardant and antistatic fibers of Examples 1-10 and Comparative Examples 1-4 were tested. The test results are shown in Table 1.
[0106] (1) Flame retardancy
[0107] Flame retardancy is determined by testing the flame retardancy level. Referring to the standard UL-94, the flame retardancy of V-0 level is better than that of V-1 level.
[0108] (2) Antistatic properties
[0109] The antistatic property is judged by the half-life method, referring to the standard GB / T 12703-1991. The smaller the half-life, the better the antistatic property.
[0110] (3) Mechanical properties
[0111] The mechanical properties are determined by testing the breaking strength of the fiber, with reference to standard GB / T 9997-1988.
[0112] Table 1
[0113]
[0114]
[0115] It can be seen from the data in Table 1 that the flame retardant antistatic fibers in Examples 1-5 of the present invention have good flame retardancy, antistatic properties and mechanical properties as a whole. Among them, Examples 6-7 respectively changed the addition ratio of the main components in the synthesis process of the modified phosphate ester compound, which reduced the antistatic properties of the modified phosphate ester compound itself and the synergistic antistatic properties with isomeric tridecanol polyoxyethylene ether sodium sulfate, resulting in a significant increase in the half-life of the fiber, while other properties were not significantly affected; Examples 8-10 changed the addition amounts of stearic acid, 11-aminoundecyl triethoxysilane and acrylamide during the preparation of the modified fly ash, so that the dispersibility and toughness of the modified fly ash were not well improved, which in turn resulted in the strength of the fiber. The mechanical properties and flame retardancy of the fibers decreased; in Comparative Examples 1-3, conventional phosphate antistatic agent OP-10 was used to replace the modified phosphate compound A in equal amounts, and modified phosphate compound A and isomeric tridecyl alcohol polyoxyethylene ether sodium sulfate were used to replace the composite antistatic agent in equal amounts. The test found that the antistatic property of the fiber showed poor results, but had no significant effect on the flame retardancy and mechanical properties; in Comparative Example 4, fly ash was used to replace the modified fly ash A in equal amounts. The test found that the flame retardancy and mechanical properties of the fiber showed poor results, but had no significant effect on the antistatic property.
[0116] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A flame retardant antistatic fiber, characterized in that: The flame retardant antistatic fiber comprises the following raw materials by weight: 90-110 parts of polyester, 5-15 parts of composite antistatic agent, 5-10 parts of flame retardant, 4-10 parts of antibacterial agent and 1-4 parts of modified fly ash.
2. The flame retardant and antistatic fiber according to claim 1, characterized in that: The polyester is any one of polyethylene terephthalate, polypropylene terephthalate and polybutylene terephthalate.
3. The flame retardant and antistatic fiber according to claim 1, characterized in that: The composite antistatic agent is a mixture of modified phosphate ester compound and isomeric tridecanol polyoxyethylene ether sodium sulfate, with a mass ratio of 1: (0.8-2).
4. The flame retardant and antistatic fiber according to claim 3, characterized in that: The preparation method of the modified phosphate ester compound comprises the following steps: (1) epichlorohydrin is added dropwise to a sodium hydrogen phosphate aqueous solution, heated to 80-90° C., stirred for 3.5-4.5 hours, rotary evaporated, anhydrous ethanol is added, stirred, filtered, recrystallized, and dried to obtain product 1 for later use; (2) adding myristic acid to a reaction vessel, introducing an inert gas, heating to 115-125° C., adding (3-amino-2,2-difluoropropyl)dimethylamine, continuing to heat to 145-155° C., stirring, distilling under reduced pressure, recrystallizing, and drying to obtain product 2 for later use; (3) adding the product 1 of step (1) and the product 2 of step (2) to an ethanol solution in sequence, heating to 80-90° C., stirring, distilling, extracting, distilling, drying, adding anhydrous ethanol, stirring, filtering, and drying to obtain a modified phosphate ester compound.
5. The flame retardant and antistatic fiber according to claim 4, characterized in that: In the step (2), the molar ratio of myristic acid to (3-amino-2,2-difluoropropyl)dimethylamine is 1:(1-2).
6. The flame retardant and antistatic fiber according to claim 4, characterized in that: In the step (3), the mass ratio of product 1 to product 2 is 1:(1.5-2).
7. The flame retardant and antistatic fiber according to claim 1, characterized in that: The preparation method of the modified fly ash comprises the following steps: 1) adding fly ash to anhydrous ethanol, stirring, heating to 55-65° C., adding stearic acid and 11-aminoundecyltriethoxysilane in sequence, stirring, cooling to room temperature, filtering, and drying to obtain activated fly ash for later use; 2) The activated fly ash, acrylamide, ammonium persulfate and N,N-methylenebisacrylamide in step 1) are mixed, stirred, deionized water is added, stirred, molded, and demolded to obtain modified fly ash.
8. The flame retardant and antistatic fiber according to claim 7, characterized in that: In the step 1), the mass ratio of fly ash, stearic acid and 11-aminoundecyltriethoxysilane is 1:(0.08-0.12):(0.1-0.2).
9. The flame-retardant antistatic fiber according to claim 7, characterized in that: In the step 2), the mass ratio of activated fly ash to acrylamide is 1:(0.2-0.3).
10. A method for preparing the flame-retardant antistatic fiber according to any one of claims 1 to 9, characterized in that: The following steps are involved: The polyester, composite antistatic agent, flame retardant, antibacterial agent and modified fly ash are mixed, stirred at 110-130° C. for 20-40 minutes, extruded, and melt-spun to obtain flame retardant antistatic fiber.
Citation Information
Patent Citations
Flame-retardant antistatic polyester fiber
CN106087101A
Preparation method of anti-static agent for high-stability dacron fabric
CN108442116A
Viscosespinning oil and preparation method thereof
CN108755141A
Flame-retardant colored antistatic polyester fiber and preparation method thereof
CN111893596A
Multi-type charging and discharging connector of electric vehicle
KR1020240141663A