Paper capable of delaying light aging and yellowing and preparation method thereof
By applying biodielectric material and PET film layer on the surface of the paper and combining the structure of the adhesive layer, the problem of paper aging and yellowing under ultraviolet light is solved, and the sun resistance and service life of the paper are significantly improved.
Patent Information
- Application Number
- CN202411386982.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
AI Technical Summary
Paper is prone to aging and yellowing under ultraviolet radiation, resulting in a decline in mechanical properties, and the prior art is difficult to effectively prevent photoaging.
Biodie materials are used to coat the paper surface, combined with the PET film layer and the adhesive layer to form a paper structure that delays photoaging and turns yellowing, simplifying the processing steps through the coating process and improving the UV shielding characteristics.
It effectively reduces the fluorescence whiteness and color difference changes of paper, extends the service life of paper, improves its tensile strength and elongation, slows down the photoaging process, and significantly improves the sun resistance of paper.
Smart Images

Figure CN119061730A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to paper capable of delaying yellowing due to light aging and a preparation method thereof, belonging to the technical field of functional paper. Background Art
[0002] Paper is a sheet of cellulose that is formed by the association of hydrogen bonds and has a certain strength after pulping, papermaking and drying of raw materials such as bark, trunk, rice straw and wheat straw. As a carrier of cultural information, paper has invaluable humanistic and artistic value. Paper is a natural organic substance containing plant fiber, which is more difficult to preserve than inorganic substances. Its main components are cellulose, hemicellulose and lignin. During the preservation process, it is easy to produce proton autocatalytic hydrolysis to produce acidic substances. Cellulose is a long-chain polymer compound that is easily hydrolyzed under the catalysis of acid and alkali to produce hydrolyzed cellulose, which reduces the degree of polymerization and causes the paper to turn yellow. Fillers in the papermaking process and acidic substances such as nitrogen and sulfur oxides in the air during the preservation process will also cause the paper fibers to become acidified, and irreversible aging changes such as hydrolysis and oxidation, mildew, acidification, yellowing and embrittlement will inevitably occur. After hemicellulose and lignin are oxidized, colored groups will be generated, the color of the paper will turn yellow, the brittleness will increase, and it will eventually become powdery and damaged, which will greatly reduce the mechanical properties of the paper.
[0003] Paper is sensitive to the external environment. When exposed to the natural environment, it will be exposed to ultraviolet radiation, pollutants in the air, and fungi. The ultraviolet rays in the sun have the characteristics of high energy, which is particularly destructive to paper. Ultraviolet radiation will accelerate the aging of paper fibers. Under the action of ultraviolet rays, molecules will directly produce chemical reactions such as chain breaking, cross-linking and decomposition, thereby initiating the degradation reaction of paper, causing the appearance of paper to turn yellow, the strength to decrease, and the brittleness to increase. Certain substances in the air will generate strong oxidants under the irradiation of ultraviolet rays, thereby oxidizing and degrading cellulose, hemicellulose and lignin, causing paper to age. In addition, the infrared rays in the light will heat the paper, increase the temperature of the paper, and accelerate the internal reaction rate, thereby accelerating the aging of the paper. There are three main forms of paper photodegradation: anaerobic photodegradation, photooxidation degradation and catalytic photooxidation. Lignin, sizing agents, fillers or white pigments contained in paper are all photosensitizers, which can catalyze the photodegradation of paper. Therefore, in the protection of paper materials, protection against ultraviolet rays is also a very important part.
[0004] Based on the above situation, it is necessary to propose a method for delaying the yellowing of paper due to light aging to solve the above problem. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a paper that delays yellowing due to light aging and a preparation method thereof. By applying biological medium materials in the paper printing industry, the ultraviolet shielding properties of the paper itself can be greatly improved, thereby improving the yellowing phenomenon of the paper.
[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solution:
[0007] In a first aspect, a paper for delaying yellowing due to light aging is provided, comprising a base paper layer 1, a mixed layer 2, an adhesive layer 3, and a PET film layer 4; one side of the base paper layer 1 is coated with the mixed layer 2, and the PET film layer 4 is bonded to the side of the base paper layer 1 coated with the mixed layer 2 through the adhesive layer 3.
[0008] In a second aspect, a method for preparing paper that delays yellowing due to light aging is provided, comprising: step 1: taking out the base paper to be processed and drying it for later use; step 2: weighing 1.5g-2g of the biological medium material and 40mL of ethyl acetate, stirring and mixing them to obtain a mixed solution; step 3: applying the mixed solution obtained in step 2 on the surface of the base paper to be processed and drying it naturally; step 4: applying glue on the PET film to form an adhesive layer; step 5: bonding one side of the base paper to be processed obtained in step 3 coated with the mixed solution and one side of the PET film obtained in step 4 coated with glue together and then drying; step 6: after drying, taking it out for later use.
[0009] Furthermore, in step 2, 2 g of biological medium material and 40 mL of ethyl acetate are weighed and stirred and mixed.
[0010] Furthermore, in step 4, the coating amount of the glue is 110 g / m 2 .
[0011] The beneficial effects of the present invention are as follows: the present invention adopts a coating process to place the biological medium material on paper, which simplifies the paper processing steps, has strong operability, simple processing methods and low costs; further, the method of the present invention broadens the scope of use of the biological medium material, and applying it to the field of paper protection can achieve a good effect of delaying light aging and yellowing of paper. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Schematic diagram of a paper structure for delaying light aging and yellowing provided by an embodiment of the present invention;
[0013] The numbers in the figure are: base paper layer-1, mixed layer-2, adhesive layer-3, PET film layer-4. DETAILED DESCRIPTION
[0014] The invention will be further described below in conjunction with the accompanying drawings and embodiments, but the content of the invention is not limited to the scope of the embodiments.
[0015] Embodiment 1:
[0016] like Figure 1 As shown, according to the first aspect of an embodiment of the present invention, a paper for delaying yellowing due to light aging is provided, comprising a base paper layer 1, a mixed layer 2, an adhesive layer 3, and a PET film layer 4; one side of the base paper layer 1 is coated with the mixed layer 2, and the PET film layer 4 is bonded to the side of the base paper layer 1 coated with the mixed layer 2 through the adhesive layer 3.
[0017] According to a second aspect of an embodiment of the present invention, a method for preparing paper for delaying light aging and yellowing is provided, comprising the following steps:
[0018] Step 1: Take out the base paper to be processed and dry it for later use, and cut out a piece of base paper with a size of about 300mm×210mm for later use;
[0019] Step 2: Weigh 2 g of biological medium material and 40 mL of ethyl acetate and stir and mix; the biological medium material is composed of the following raw materials in percentage by mass: 61% to 65% synthetic fluorphlogopite, 35% to 39% titanium dioxide, and 0% to 1% tin dioxide; in this embodiment, the biological medium material is specifically composed of 64% synthetic fluorphlogopite, 35% titanium dioxide, and 1% tin dioxide in percentage by mass;
[0020] Step 3: Apply the mixed liquid to the front of the base paper to be processed by manual coating and dry naturally;
[0021] Step 4: Manually apply glue on the PET film to form an adhesive layer. The amount of glue applied is about 110g / m 2 ;
[0022] Step 5: Bond one side of the base paper to be processed obtained in step 3 coated with the mixed liquid and one side of the PET film obtained in step 4 coated with the glue together, and dry them in a cool place indoors for 24 hours;
[0023] Step 6: After drying, take it out and set it aside.
[0024] The paper for delaying light aging and yellowing prepared by the preparation method of the present invention and the paper prepared without coating the mixed solution (i.e., the paper prepared without coating the mixed solution is used as the blank control group, and the method omits steps 2 and 3 compared with the present invention, i.e., directly bonding the base paper to the one side of the PET film coated with glue and then drying) are compared and discussed:
[0025] Measurement of basic parameters: Take out the paper and use the paper sampler to obtain a 100cm 2 The basic parameters of the paper samples were measured by using paper testing instruments such as a smoothness meter, a whiteness meter, and a thickness meter, as shown in Table 1 below.
[0026] Table 1 Basic parameters of paper that delays light aging and yellowing
[0027]
[0028] Through the basic parameter measurement of the blank control group and the paper for delaying light aging and yellowing as shown in Table 1, it is found that the fluorescent whiteness of the blank control group is higher, while the paper for delaying light aging and yellowing made by the present invention has lower fluorescent whiteness in the paper. It should be noted that people are often exposed to fluorescent whitening agents in their daily life activities, which generally do not cause harm to the human body. However, if exposed in excess, since fluorescent whitening agents are easily accumulated in the human body, they will have many harmful effects on the human body over time, greatly reducing the human body's immunity. Obviously, the paper of the present invention has more application advantages.
[0029] Light fastness test: Four samples of paper produced by the method of the present invention and the paper of the blank control group were selected and cut into samples with a specification of 60 mm×200 mm for numbering and testing, and the light fastness of the paper was tested using a light fatigue test device to observe the change in color difference, and the aging result of a paper that delays light aging and yellowing was objectively characterized by data using a colorimeter. The test results are shown in Tables 2 to 9 (L is brightness, a is redness, b is yellowness, ΔL represents the change in brightness after aging, Δa represents the change in redness, and Δb represents the change in yellowness).
[0030] Table 2 Color quality test data of the blank control group in the initial state
[0031] Sample No. L a b Whiteness 1 91.11 -0.73 5.46 72.54 2 90.85 -0.75 5.71 71.69 3 90.82 -0.81 5.54 71.85 4 91.26 -0.69 5.37 72.95
[0032] Table 3 Test data of color quality of paper in initial state for delaying yellowing due to light aging
[0033] Sample No. L a b Whiteness 1 88.74 -1.02 2.82 70.57 2 89.86 -0.8 2.92 71.84 3 88.74 -1.05 3.56 69.36 4 89.95 -0.76 2.7 69.85
[0034] Table 4 Color quality test data of blank control group aging for 24 hours
[0035] Sample No. L a b Whiteness △L △a △b △E*ab 1 90.81 0.55 6.71 70.24 -0.3 1.28 1.25 1.814 2 90.66 0.51 7 70.31 -0.19 1.26 1.29 1.813 3 90.48 0.49 6.89 70.18 -0.34 1.3 1.35 1.905 4 90.7 0.32 6.89 69.17 -0.56 1.01 1.52 1.909 average value 90.6625 0.4675 6.8725 69.975 -0.3475 1.2125 1.3525 1.860 Maximum 90.81 0.55 7 70.31 -0.19 1.3 1.52 1.909 Minimum 90.48 0.32 6.71 69.17 -0.56 1.01 1.25 1.813 Standard Deviation 0.137 0.101 0.120 0.539 0.155 0.136 0.119 0.054 Coefficient of variation 0.002 0.217 0.017 0.008 -0.447 0.112 0.088 0.029
[0036] Table 5 Color quality test data of paper that delays yellowing after light aging for 24 hours
[0037] Sample No. L a b Whiteness △L △a △b △E*ab 1 88.62 -0.69 3.58 69.12 -0.12 0.33 0.76 0.837 2 89.35 -0.75 3.7 69.29 -0.51 0.05 0.78 0.933 3 88.44 -0.67 4.36 68.44 -0.3 0.38 0.8 0.935 4 89.55 -0.7 3.56 68.17 -0.4 0.06 0.86 0.950 average value 88.99 -0.7025 3.8 68.755 -0.3325 0.205 0.8 0.914 Maximum 89.55 -0.67 4.36 69.29 -0.12 0.38 0.86 0.950 Minimum 88.44 -0.75 3.56 68.17 -0.51 0.05 0.76 0.837 Standard Deviation 0.542 0.034 0.378 0.536 0.166 0.174 0.043 0.052 Coefficient of variation 0.006 -0.048 0.100 0.008 -0.498 0.851 0.054 0.057
[0038] Table 6 Color quality test data of blank control group after aging for 48 hours
[0039] Sample No. L a b Whiteness △L △a △b △E*ab 1 90.16 0.45 7.38 69.5 -0.95 1.18 1.92 2.446 2 89.73 0.46 7.76 68.86 -1.12 1.21 2.05 2.631 3 89.61 0.36 7.66 68.62 -1.21 1.17 2.12 2.707 4 89.69 0.51 7.3 69.48 -1.57 1.2 1.93 2.762 average value 89.7975 0.445 7.525 69.115 -1.2125 1.19 2.005 2.636 Maximum 90.16 0.51 7.76 69.5 -0.95 1.21 2.12 2.762 Minimum 89.61 0.36 7.3 68.62 -1.57 1.17 1.92 2.446 Standard Deviation 0.247 0.062 0.220 0.444 0.262 0.018 0.097 0.138 Coefficient of variation 0.003 0.140 0.029 0.006 -0.216 0.015 0.048 0.052
[0040] Table 7 Color quality test data of paper that delays yellowing after light aging for 48 hours
[0041] Sample No. L a b Whiteness △L △a △b △E*ab 1 88.49 -0.17 3.97 69.04 -0.25 0.85 1.15 1.452 2 89.18 -0.18 4.27 68.22 -0.68 0.62 1.35 1.634 3 88.04 -0.33 4.82 67.89 -0.7 0.72 1.26 1.611 4 89.77 -0.26 4.04 67.66 -0.18 0.5 1.34 1.442 average value 88.87 -0.235 4.275 68.2025 -0.4525 0.6725 1.275 1.535 Maximum 89.77 -0.17 4.82 69.04 -0.18 0.85 1.35 1.634 Minimum 88.04 -0.33 3.97 67.66 -0.7 0.5 1.15 1.442 Standard Deviation 0.761 0.075 0.385 0.604 0.276 0.149 0.093 0.102 Coefficient of variation 0.009 -0.319 0.090 0.009 -0.610 0.221 0.073 0.066
[0042] Table 8 Color quality test data of blank control group aging for 72 hours
[0043]
[0044] Table 9 Color quality test data of paper that delays yellowing after light aging for 72 hours
[0045] Sample No. L a b Whiteness △L △a △b △E*ab 1 87.62 -0.35 5.22 68.1 -1.12 0.67 2.4 2.732 2 88.9 -0.17 5.4 68.27 -0.96 0.63 2.48 2.733 3 87.63 -0.32 5.71 67.85 -1.11 0.73 2.15 2.527 4 88.89 -0.09 4.94 68.01 -1.06 0.67 2.24 2.567 average value 88.26 -0.2325 5.3175 68.0575 -1.0625 0.675 2.3175 2.640 Maximum 88.9 -0.09 5.71 68.27 -0.96 0.73 2.48 2.733 Minimum 87.62 -0.35 4.94 67.85 -1.12 0.63 2.15 2.527 Standard Deviation 0.733 0.123 0.323 0.175 0.073 0.041 0.150 0.108 Coefficient of variation 0.008 -0.531 0.061 0.003 -0.069 0.061 0.065 0.041
[0046] It should be noted that color difference refers to the difference in color perception between two colors expressed in numerical form. The larger the ΔE*ab value, the more significant the color difference between samples, and the smaller the ΔE*ab value, the smaller the color difference between samples. Through the above light accelerated aging experimental data, it is found that during the three groups of aging processes of 24 hours, 48 hours, and 72 hours, the color difference of a paper that delays light aging and yellowing at the same time is smaller than that of the blank control group, which shows that the paper that delays light aging and yellowing of the present invention can resist the damage of ultraviolet rays to the paper to a certain extent, and prolong the service life of the paper itself.
[0047] Furthermore, the blank control group and the paper produced by the method of the present invention were tested for the change in indentation stiffness, tensile strength and elongation at the initial stage and after aging for 24 hours, 48 hours and 72 hours, and the experimental results are shown in Tables 10 to 13.
[0048] Table 10 Blank control group aging 72 hours indentation stiffness change test
[0049] 0 24 48 72 Vertical / gf 184.55 154.05 121.63 109.5 Horizontal / gf 151.42 133.42 103.5 89.64
[0050] Table 11 Test on the change of indentation stiffness of paper after aging for 72 hours to delay yellowing due to light aging
[0051] 0 24 48 72 Vertical / gf 209.74 192.93 188.86 169.1 Horizontal / gf 162.68 143.9 130.57 115.28
[0052] Table 12 Test on changes in tensile strength and elongation of the blank control group after aging for 72 hours
[0053]
[0054] Table 13 Test on the change of tensile strength and elongation of paper after aging for 72 hours to delay yellowing due to light aging
[0055]
[0056] It should be noted that the mechanical properties of paper mainly depend on the strength of the fiber itself and the bonding strength between the fibers. At the same time, the fiber length and fiber flexibility also affect the mechanical strength of the paper. Studies have shown that the indentation stiffness is related to the length of the paper fiber and the bonding force between the fibers. The main reason for paper aging is that the degradation of cellulose, hemicellulose and lignin causes the paper fiber to break. With the increase of light aging time, the aging reaction rate of the paper accelerates, causing the paper fibers to become brittle and hard, and the paper to become yellow and brittle, so the mechanical strength of the paper decreases. In order to slow down these degradation processes, it is necessary to carry out preventive protection. It can be seen from the above experiments that the indentation stiffness of the blank control group paper and the paper made by the present invention that delays light aging and yellowing in the longitudinal and transverse directions decreases with the increase of aging time, but it is obvious that the reduction of the paper that delays light aging and yellowing is smaller than that of the blank paper; at the same time, the tensile strength and elongation performance of the present invention are better than those of the blank control group.
[0057] Furthermore, in order to better prove the lightfastness effect of a paper that delays light aging and yellowing, samples were taken from the prepared paper that delays light aging and yellowing and the blank control group, and bronze ink was manually applied on the two papers to conduct light aging experiments again, to compare and explain whether the lightfastness effect of the ink printed on the paper changes with or without the paper preparation method that delays light aging and yellowing. The test results are shown in Tables 14 to 21.
[0058] Table 14 Blank control group initial state color quality test data
[0059] Sample No. L a b Whiteness 1 29.13 24.12 27.28 1.64 2 28.98 23.44 27.36 1.61 3 30.14 24.14 26.96 1.84 4 29.76 24.09 27.58 1.71
[0060] Table 15 Test data of color quality of paper in initial state for delaying yellowing due to light aging
[0061] Sample No. L a b Whiteness 1 38.28 29.22 31.86 2.96 2 34.61 28.05 30.19 2.35 3 29.7 21.89 24.41 2.04 4 39.21 24.83 27.79 3.86
[0062] Table 16 Color quality test data of blank control group aging for 24 hours
[0063] Sample No. L a b Whiteness △L △a △b △E*ab 1 29.04 22.95 24.4 2.12 -0.09 -1.17 -2.88 3.11 2 28.35 21.6 24.6 1.99 -0.63 -1.84 -2.76 3.376 3 29.08 23.12 24.9 2.08 -1.06 -1.02 -2.06 2.531 4 29.34 22.35 25.48 2.17 -0.42 -1.74 -2.1 2.759 average value 28.953 22.505 24.845 2.09 -0.55 -1.443 -2.45 2.944 Maximum 29.34 23.12 25.480 2.170 -0.09 -1.02 -2.06 3.376 Minimum 28.35 21.6 24.4 1.99 -1.06 -1.84 -2.88 2.531 Standard Deviation 0.423 0.688 0.471 0.076 0.406 0.408 0.43 0.374 Coefficient of variation 0.015 0.031 0.019 0.036 -0.739 -0.283 -0.176 0.127
[0064] Table 17 Color quality test data of paper aging for 24 hours to delay yellowing due to light aging
[0065] Sample No. L a b Whiteness △L △a △b △E*ab 1 38.17 28.32 31.74 2.96 -0.11 -0.9 -0.12 0.915 2 33.68 27.79 28.2 2.89 -0.93 -0.26 -1.99 2.212 3 28.97 21.29 23.27 2.22 -0.73 -0.6 -1.14 1.481 4 37.83 24.3 26.43 2.43 -1.38 -0.53 -1.36 2.009 average value 34.663 25.425 27.41 2.625 -0.788 -0.573 -1.153 1.654 Maximum 38.17 28.32 31.74 2.96 -0.11 -0.26 -0.12 2.212 Minimum 28.97 21.29 23.27 2.22 -1.38 -0.9 -1.990 0.915 Standard Deviation 4.309 3.283 3.534 0.358 0.527 0.263 0.777 0.581 Coefficient of variation 0.124 0.129 0.129 0.136 -0.669 -0.459 -0.674 0.351
[0066] Table 18 Color quality test data of blank control group aging for 48 hours
[0067] Sample No. L a b Whiteness △L △a △b △E*ab 1 28.57 22.91 24.96 1.76 -0.56 -1.21 -2.32 2.676 2 27.55 21.98 24.47 1.63 -1.43 -1.46 -2.89 3.54 3 28.17 20.97 23.33 1.95 -1.97 -3.17 -3.63 5.206 4 27.93 20.88 25.06 1.94 -1.83 -3.21 -2.52 4.473 average value 28.055 21.685 24.455 1.820 -1.448 -2.263 -2.840 3.974 Maximum 28.570 22.91 25.06 1.95 -0.56 -1.21 -2.32 5.206 Minimum 27.550 20.880 23.330 1.630 -1.970 -3.210 -3.630 2.676 Standard Deviation 0.428 0.957 0.793 0.154 0.634 1.076 0.577 1.102 Coefficient of variation 0.015 0.044 0.032 0.085 -0.438 -0.476 -0.203 0.277
[0068] Table 19 Color quality test data of paper that delays yellowing after light aging for 48 hours
[0069] Sample No. L a b Whiteness △L △a △b △E*ab 1 37.17 28.66 29.56 2.26 -1.11 -0.56 -2.3 2.615 2 32.68 27.56 27.89 1.93 -1.93 -0.49 -2.3 3.042 3 29.53 21.3 22.77 2.17 -0.17 -0.59 -1.64 1.751 4 37.39 23.4 26.35 2.23 -1.82 -1.43 -1.44 2.726 average value 34.193 25.23 26.643 2.148 -1.258 -0.768 -1.92 2.533 Maximum 37.390 28.66 29.56 2.26 -0.17 -0.490 -1.44 3.042 Minimum 29.53 21.3 22.77 1.93 -1.93 -1.43 -2.3 1.751 Standard Deviation 3.791 3.464 2.895 0.15 0.811 0.444 0.446 0.552 Coefficient of variation 0.111 0.137 0.109 0.07 -0.645 -0.578 -0.232 0.218
[0070] Table 20 Color quality test data of blank control group aging for 72 hours
[0071] Sample No. L a b Whiteness △L △a △b △E*ab 1 28.12 22.41 23.04 1.87 -1.01 -1.71 -4.24 4.682 2 28.11 20.89 21.75 2 -0.87 -2.55 -5.61 6.223 3 29.1 21.98 22.92 2.07 -1.04 -2.16 -4.04 4.698 4 27.85 21.82 23.4 1.79 -1.91 -2.27 -4.18 5.126 average value 28.295 21.775 22.778 1.933 -1.208 -2.173 -4.518 5.182 Maximum 29.1 22.41 23.4 2.07 -0.87 -1.71 -4.04 6.223 Minimum 27.85 20.890 21.75 1.79 -1.91 -2.550 -5.61 4.682 Standard Deviation 0.551 0.640 0.715 0.126 0.474 0.349 0.733 0.724 Coefficient of variation 0.019 0.029 0.031 0.065 -0.393 -0.161 -0.162 0.14
[0072] Table 21 Color quality test data of paper that delays yellowing after light aging for 72 hours
[0073]
[0074]
[0075] From the above experimental results, it can be seen that the paper that delays light aging and yellowing prepared by introducing the method for preparing paper that delays light aging and yellowing can reduce the change of ink color (mainly using △E*ab as an evaluation index) for products with ink printed on the surface, and can also slow down the change process of ink light aging. Based on this research premise, a paper that delays light aging and yellowing is used to produce paper printed products with paper and ink as the base material to improve the light fastness of the printed products.
[0076] By applying the above technical solution, it can be known that compared with the light-fast biomass paper and its preparation method disclosed in the existing patent application, a coating capable of molding a laser effect is applied during the processing, and through a series of processing processes, the finished product has decorative effects such as laser colorful effects and metallic three-dimensional effects. The paper processed in this way can add icing on the cake for the paper packaging and printing industry, and extend the optional scope of paper used in the packaging and printing industry. The present invention adopts a coating process to place the biological medium material on the paper, which simplifies the paper processing steps, has strong operability, simple processing methods, and low costs; further, the method of the present invention broadens the scope of use of the biological medium material, and applies it to the field of paper protection, which can achieve a good effect of delaying light aging and yellowing of paper.
[0077] In summary, the present invention focuses on expanding the scope of use of the method for preparing light-fast paper that delays light aging and yellowing, and refers the paper with decorative effects used in the processing packaging and printing industry to other fields, and observes whether the method for preparing paper that delays light aging and yellowing can achieve good light-fastness effects by using the processing technology involved in the present invention. Through a series of experiments, it is proved that a paper that delays light aging and yellowing can improve the amplitude of changes in paper color parameters, and a paper that delays light aging and yellowing can improve the ultraviolet shielding properties of paper. From the research ideas and design perspectives of the present invention, the light-fastness effect of the method for preparing paper that delays light aging and yellowing can be introduced and used in combination with other reagents (such as: paper deacidification and reinforcement agent to replace ethyl acetate in this application) to observe changes in paper protection effectiveness.
[0078] Embodiment 2:
[0079] A method for preparing paper that delays yellowing due to light aging, comprising:
[0080] Step 1: Take out the base paper to be processed and dry it for later use;
[0081] Step 2: Weigh 1.5 g of a biological medium material and 40 mL of ethyl acetate, stir and mix, and obtain a mixed solution; the biological medium material is composed of the following raw materials in percentage by mass: 63% of synthetic fluorphlogopite, 36.5% of titanium dioxide, and 0.5% of tin dioxide;
[0082] Step 3: Use a coating device to coat the mixed solution obtained in step 2 on the surface of the base paper to be processed, and dry it naturally; for example, the coating experiment is carried out on a rod coater, the paper to be coated is placed flat on the press of the coater, the prepared biological medium material mixed solution is adjusted to the coating concentration, the biological medium material coating solution is measured with a dropper and placed on the top of the coater, the speed and coating amount of the coating rod are strictly controlled, and the paper is dried naturally after coating;
[0083] Step 4: Place the PET film to be coated flat on the press of the coating machine, use a dropper to measure the glue and place it on the top of the coating machine, and then coat it to form an adhesive layer;
[0084] Step 5: bonding one side of the base paper to be processed obtained in step 3 coated with the mixed liquid and one side of the PET film obtained in step 4 coated with the glue together and then drying;
[0085] Step 6: After drying, take it out and set it aside.
[0086] Furthermore, the bio-medium material is composed of the following raw materials in percentage by mass: 61% of synthetic fluorphlogopite, 38.5% of titanium dioxide, and 0.5% of tin dioxide.
[0087] Embodiment 3:
[0088] A method for preparing paper that delays yellowing due to light aging, comprising:
[0089] Step 1: Take out the base paper to be processed and dry it for later use;
[0090] Step 2: Weigh 1.6 g of biological medium material and 40 mL of ethyl acetate, stir and mix to obtain a mixed solution; the biological medium material is composed of the following raw materials in the following mass percentages: 62.5% of synthetic fluorphlogopite, 37% of titanium dioxide, and 0.5% of tin dioxide.
[0091] Step 3: Use a coating device to coat the mixed solution obtained in step 2 on the surface of the base paper to be processed, and dry it naturally; for example, the coating experiment is carried out on a rod coater, the paper to be coated is placed flat on the press of the coater, the prepared biological medium material mixed solution is adjusted to the coating concentration, the biological medium material coating solution is measured with a dropper and placed on the top of the coater, the speed and coating amount of the coating rod are strictly controlled, and the paper is dried naturally after coating;
[0092] Step 4: Place the PET film to be coated flat on the press of the coating machine, use a dropper to measure the glue and place it on the top of the coating machine, and then coat it to form an adhesive layer;
[0093] Step 5: bonding one side of the base paper to be processed obtained in step 3 coated with the mixed liquid and one side of the PET film obtained in step 4 coated with the glue together and then drying;
[0094] Step 6: After drying, take it out and set it aside.
[0095] Furthermore, the bio-medium material is composed of the following raw materials in percentage by mass: 65% of synthetic fluorphlogopite and 35% of titanium dioxide.
[0096] The present invention applies the bio-medium material to the surface of paper by a coating method, so as to achieve the effect of reinforcing the paper; the surface of the fiber in the paper-based material that is easily decomposed and broken by ultraviolet light is evenly coated with titanium dioxide particles with a shielding effect, and the precipitated fibers are either coated on the synthetic fluorphlogopite and the short-cut surface, or filled in the gaps of the material, which can effectively prevent the ultraviolet light from decomposing and destroying the structure of the paper-based material; the appropriate polymer material can not only make the paper fiber thicker and increase the fiber bonding force, thereby enhancing the strength of the paper, but also have the effects of toughening and anti-aging, thereby improving the service life of the paper.
[0097] The specific implementation modes of the present invention have been described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A paper for delaying yellowing due to light aging, characterized in that: The invention comprises a base paper layer (1), a mixed layer (2), an adhesive layer (3), and a PET film layer (4); one side of the base paper layer (1) is coated with the mixed layer (2), and the PET film layer (4) is bonded to the side of the base paper layer (1) coated with the mixed layer (2) through the adhesive layer (3).
2. A method for preparing paper that delays yellowing due to light aging, characterized in that: include: Step 1: Take out the base paper to be processed and dry it for later use; Step 2: Weigh 1.5 g to 2 g of the biological medium material and 40 mL of ethyl acetate, stir and mix to obtain a mixed solution; Step 3: Apply the mixed solution obtained in step 2 to the surface of the base paper to be processed and dry it naturally; Step 4: Apply glue on the PET film to form an adhesive layer; Step 5: bonding one side of the base paper to be processed obtained in step 3 coated with the mixed liquid and one side of the PET film obtained in step 4 coated with the glue together and then drying; Step 6: After drying, take it out and set it aside.
3. The method for preparing paper that delays yellowing due to light aging according to claim 2, characterized in that: In the step 2, 2 g of biological medium material and 40 mL of ethyl acetate were weighed and stirred and mixed.
4. The method for preparing paper that delays yellowing due to light aging according to claim 2, characterized in that: In step 4, the coating amount of glue is 110g / m 2 .
Citation Information
Patent Citations
Masking paper with anti-aging capability and preparation method thereof
CN115522408A
Sun-proof biomass paper and preparation method thereof
CN117364530A
Anti-aging paperboard and preparation method thereof
CN117926639A
Paper is scribbled with connecing no aluminium of dress to help to highlight cigarette