Preparation method of fiber hybrid composite bulletproof helmet and composite bulletproof helmet
Through fiber hybrid composite technology, the hot pressing composite of ultra-high molecular weight polyethylene fiber and reinforced fibers is used to solve the shortcomings of existing bulletproof helmets in durability and bulletproof performance, and achieve efficient bulletproof performance improvement and structural strength enhancement. Engineering application.
Patent Information
- Application Number
- CN202411417981.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-03
AI Technical Summary
The engineering application of existing bulletproof helmets is limited. Aramid helmets are not light-resistant and have short lifespan. Ultra-high molecular weight polyethylene helmets are not resistant to high temperatures and have low bulletproof performance, which is easy to cause blunt injuries.
Using the preparation method of fiber hybrid composite bulletproof helmets, the ultra-high molecular weight polyethylene fiber weft fabric is cut and pre-paved to heat-press and reinforcing fibers (such as carbon fiber, aramid fiber, glass fiber, PBO fiber) is formed to form vacuum hot pressure Or non-vacuum hot pressing composite structure to improve bulletproof performance and structural strength.
It has achieved improvements in elastic resistance, reduced the height of the elastic marks, enhanced the interface bonding strength and composite uniformity, suitable for engineering applications, and improved production efficiency.
Smart Images

Figure CN119063578A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of bulletproof protective equipment, and in particular to a preparation method of a fiber-mixed composite bulletproof helmet and a composite bulletproof helmet. Background Art
[0002] Bulletproof helmets are protective equipment that protect the human head from high-speed projectiles or fragments. They are crucial to improving soldiers' survivability, reducing casualties and enhancing combat effectiveness. Since World War II, various countries have conducted in-depth research on the bulletproof performance and wearing comfort of bulletproof helmets, including bulletproof materials, helmet-shaped structures, composite structures, and molding processes. Through continuous technological innovation, traditional metal helmets have been gradually replaced.
[0003] At present, the most widely used bulletproof helmets are aramid helmets and ultra-high molecular weight polyethylene helmets. However, aramid helmets are not light-resistant, have poor weather resistance, have a short lifespan, and have high manufacturing costs, so their applicable markets are limited, which limits their engineering applications. Ultra-high molecular weight polyethylene bulletproof helmets are not resistant to high temperatures, and when bullets penetrate, the bullet marks are high, which can easily cause blunt injuries, resulting in low bulletproof performance. Summary of the invention
[0004] The purpose of the embodiments of the present invention is to provide a method for preparing a fiber-mixed composite bullet-proof helmet and a composite bullet-proof helmet, so as to solve the problems of limited engineering applications and low bulletproof performance.
[0005] To solve the above technical problems, the embodiments of the present invention provide the following technical solutions:
[0006] A first aspect of the present invention provides a method for preparing a fiber hybrid composite bulletproof helmet, the preparation method comprising:
[0007] Cutting the multi-layer ultra-high molecular weight polyethylene fiber non-woven fabric according to the preset cutting size;
[0008] Multiple layers of cut ultra-high molecular weight polyethylene fiber non-woven fabrics are stacked one on top of the other and pre-laid in the mold cavity of the helmet female mold to obtain a pre-laid helmet;
[0009] The pre-laid helmet is placed in a pre-pressing mold for pre-pressing and shaping to obtain a pre-pressed helmet;
[0010] The pre-pressed helmet is placed in a forming mold for forming and pressing to obtain a bulletproof main body helmet;
[0011] Cutting and pre-laying the multi-layer reinforced fiber prepreg in sequence to obtain a pre-laid reinforced fiber helmet, wherein the fibers used in the multi-layer reinforced fiber prepreg are reinforcing fibers, and the reinforcing fibers are a combination of one or more of carbon fibers, aramid fibers, glass fibers, and PBO fibers;
[0012] Placing the pre-laid reinforced fiber helmet in a forming mold and performing forming pressing to obtain a reinforced fiber helmet;
[0013] The bulletproof main body helmet and the reinforced fiber helmet are hot-pressed and composited using a film to obtain a fiber hybrid composite bulletproof helmet. When the hot-pressing composite is vacuum hot-pressing, the vacuum hot-pressing temperature is 110-130° C., the holding pressure is 2-5 MPa, and the holding time is 15-30 min.
[0014] In some modified embodiments of the first aspect of the present invention, the fibers used in the ultra-high molecular weight polyethylene non-woven fabric are ultra-high molecular weight polyethylene fibers, and the mixing ratio of the ultra-high molecular weight polyethylene fibers to the reinforcing fibers is 4:1 to 6.8:1.
[0015] In some modified embodiments of the first aspect of the present invention, when the hot pressing composite is non-vacuum hot pressing, the temperature of the non-vacuum hot pressing is 110-130° C., the holding pressure is 5-15 MPa, and the holding time is 15-30 min.
[0016] In some modified embodiments of the first aspect of the present invention, the constant pressure holding temperature of the molding pressing of the pre-pressed helmet is 128-133°C, the constant temperature holding time is 15-30 minutes, and the constant temperature holding pressure is 15 MPa.
[0017] In some modified embodiments of the first aspect of the present invention, the constant pressure holding temperature for molding and pressing of the pre-laid reinforced fiber helmet is 135-155°C, the constant temperature holding time is 30-50 minutes, and the constant temperature holding pressure is 3-7 MPa.
[0018] In some modified embodiments of the first aspect of the present invention, multiple layers of cut ultra-high molecular weight polyethylene fiber non-woven fabrics are overlapped layer by layer and pre-laid in the mold cavity of the helmet female mold to obtain a pre-laid helmet, comprising:
[0019] Obtaining a preset number of layers of first-cut ultra-high molecular weight polyethylene fiber non-woven fabric;
[0020] The positions of the first sharp corners of each layer of the first-cut ultra-high molecular weight polyethylene fiber non-woven fabric are kept consistent, and each layer of the first-cut ultra-high molecular weight polyethylene fiber non-woven fabric is overlapped at multiple inner cutting line positions, and pre-laid in the mold cavity of the helmet female mold;
[0021] Obtaining a preset number of layers of second-cut ultra-high molecular weight polyethylene fiber non-woven fabric;
[0022] Place the second sharp corner positions of the second cut ultra-high molecular weight polyethylene fiber non-woven fabrics of each layer into the corresponding first sharp corner positions, and rotate the second sharp corner positions by a preset angle;
[0023] The layers of the second cut ultra-high molecular weight polyethylene fiber non-woven fabric are overlapped at multiple inner cutting line positions and pre-laid in the mold cavity of the helmet female mold;
[0024] Return to the step of obtaining a preset number of layers of the second cut ultra-high molecular weight polyethylene fiber non-woven fabric, and stop pre-laying when the number of pre-laying reaches the preset number, to obtain a pre-laid helmet.
[0025] In some modified implementations of the first aspect of the present invention, the preset number of layers is 2 to 4 layers, the preset number of times is 10 to 30 times, and the preset angle is 30±5°.
[0026] In some modified embodiments of the first aspect of the present invention, the multi-layer ultra-high molecular weight polyethylene fiber non-woven fabric is used as the bulletproof material, and the surface density of the bulletproof material is 80 to 160 g / m 2 .
[0027] In some modified embodiments of the first aspect of the present invention, the adhesive film is a hot melt adhesive, and the surface density of the hot melt adhesive film is 60 to 120 g / m 2 .
[0028] The second aspect of the present invention provides a composite bulletproof helmet, which includes a bulletproof main body helmet and a reinforced fiber helmet. The fiber used in the bulletproof main body helmet is ultra-high molecular weight polyethylene fiber, and the fiber used in the reinforced fiber helmet is a combination of one or more of carbon fiber, aramid fiber, glass fiber, and PBO fiber. The mixing ratio of the ultra-high molecular weight polyethylene fiber to the reinforced fiber is 4:1 to 6.8:1.
[0029] Compared with the prior art, the present invention provides a preparation method of a fiber-mixed composite bulletproof helmet and a composite bulletproof helmet. According to a preset cutting size, multiple layers of ultra-high molecular weight polyethylene fiber non-weft cloth are cut, and the multiple layers of cut ultra-high molecular weight polyethylene fiber non-weft cloth are overlapped layer by layer, and pre-laid in the mold cavity of the helmet female mold to obtain a pre-laid helmet; the pre-laid helmet is placed in a pre-pressing mold for pre-pressing and shaping to obtain a pre-pressed helmet; the pre-pressed helmet is placed in a molding mold for molding and pressing to obtain a bulletproof main body helmet; multiple layers of reinforcing fiber prepreg cloth are cut and pre-laid in sequence to obtain To the pre-laid reinforced fiber helmet, the fiber used in the multi-layer reinforced fiber prepreg is the reinforcing fiber, and the reinforcing fiber is a combination of one or more of carbon fiber, aramid fiber, glass fiber, and PBO fiber; the pre-laid reinforced fiber helmet is placed in a molding mold for molding and pressing to obtain a reinforced fiber helmet; the bulletproof main body helmet and the reinforced fiber helmet are hot-pressed and composited with a film to obtain a fiber hybrid composite bulletproof helmet, and when the hot-pressing composite is vacuum hot-pressing, the vacuum hot-pressing temperature is 110-130°C, the holding pressure is 2-5MPa, and the holding time is 15-30min. In this way, ultra-high molecular weight polyethylene fiber, carbon fiber, aramid fiber, glass fiber, and PBO fiber are selected as the hybrid fiber materials of the composite bulletproof helmet, and the performance advantages of different fiber materials are comprehensively utilized to achieve the positive unification of the anti-ballistic performance and structural strength of the bulletproof helmet, so that the bullet mark height value of the mixed fiber material helmet is small, and the bulletproof performance of the fiber hybrid composite bulletproof helmet is effectively improved. The process of hot pressing and compounding the adhesive films at the interfaces of the bulletproof main helmet and the reinforced fiber helmet adopts vacuum hot pressing to effectively improve the interface bonding strength and interface compounding uniformity, while greatly improving the production efficiency, which is conducive to engineering application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] By reading the detailed description below with reference to the accompanying drawings, the above and other objects, features and advantages of the exemplary embodiments of the present invention will become readily understood. In the accompanying drawings, several embodiments of the present invention are shown in an exemplary and non-limiting manner, and the same or corresponding reference numerals represent the same or corresponding parts, wherein:
[0031] Figure 1 A flow chart schematically shows a method for preparing a fiber hybrid composite bulletproof helmet;
[0032] Figure 2 A schematic diagram schematically shows the preset cutting size of the ultra-high molecular weight polyethylene non-woven fabric;
[0033] Figure 3 A schematic diagram schematically shows the cutting size of the reinforcing fiber prepreg;
[0034] Figure 4 The structure of a composite bulletproof helmet is schematically shown. DETAILED DESCRIPTION
[0035] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0036] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in the present invention should have the common meanings understood by those skilled in the art to which the present invention belongs.
[0037] The method in the embodiment of the present invention is described in detail below.
[0038] Figure 1 The flowchart schematically shows the method for preparing the fiber hybrid composite bulletproof helmet in the embodiment of the present invention, see Figure 1 As shown, the preparation method may include:
[0039] S101, cutting the multi-layer ultra-high molecular weight polyethylene fiber non-woven fabric according to a preset cutting size.
[0040] As an optional implementation, the fiber used in the ultra-high molecular weight polyethylene non-woven fabric is ultra-high molecular weight polyethylene fiber, and the mixing ratio of the ultra-high molecular weight polyethylene fiber to the reinforcing fiber is 4:1 to 6.8:1.
[0041] As an optional embodiment, multi-layer ultra high molecular weight polyethylene fiber (UHMWPEF) non-woven fabric is used as the bulletproof material, and the surface density of the bulletproof material is 80 to 160 g / m 2 .
[0042] Specifically, the bulletproof material is subjected to cutting, pre-laying, pre-pressing, hot pressing and other processes in sequence to prepare a bulletproof main body helmet. The bulletproof material is a UHMWPEF non-woven fabric prepared by mixing UHMWPEF and impregnating a thermoplastic resin binder, wherein the thermoplastic resin binder is polyurethane with a content of 10% to 20%.
[0043] The cutting process is to lay the UHMWPEF non-woven fabric and cut it into the preset cutting size by an automatic cutting machine. The radius of the circular part of the ultra-high molecular weight polyethylene non-woven fabric with the preset cutting size is 260-350 mm, the length of the straight part of the outer shape is 260-350 mm, the length of the inner cutting line is 180-300 mm, and the distance between the two inner cutting lines on the same straight line is 142-232 mm.
[0044] Figure 2 Schematic diagram showing the preset cutting size of ultra-high molecular weight polyethylene non-woven fabric, see Figure 2 As shown, the radius of the circular part of the ultra-high molecular weight polyethylene non-woven fabric with preset cutting size is 260mm, the length of the straight line part is 260, the length of the inner cutting line is 189mm and 297mm, and the distance between the two inner cutting lines on the same straight line is 143mm.
[0045] S102, overlapping multiple layers of cut ultra-high molecular weight polyethylene fiber non-woven fabrics layer by layer, pre-laying them in the mold cavity of the helmet female mold to obtain a pre-laid helmet.
[0046] Specifically, multiple layers of cut ultra-high molecular weight polyethylene fiber non-woven fabrics are overlapped layer by layer and pre-laid in the mold cavity of the helmet female mold to obtain a pre-laid helmet, including:
[0047] Step A1: obtaining a first cut ultra-high molecular weight polyethylene fiber non-woven fabric with a preset number of layers.
[0048] Among them, the preset number of layers is 2 to 4 layers.
[0049] Obtain 2 to 4 layers of first cut ultra-high molecular weight polyethylene fiber non-woven fabric.
[0050] Step A2: keep the first sharp corner positions of each layer of the first cut ultra-high molecular weight polyethylene fiber non-woven fabric consistent, and overlap each layer of the first cut ultra-high molecular weight polyethylene fiber non-woven fabric at multiple inner cutting line positions, and pre-lay them in the mold cavity of the helmet female mold.
[0051] Specifically, when 2 to 4 layers of first-cut ultra-high molecular weight polyethylene fiber non-woven fabrics, i.e., cut pieces, are laid together, it is necessary to keep the first sharp corner positions of each layer of the first-cut ultra-high molecular weight polyethylene fiber non-woven fabrics consistent, and overlap each layer of the first-cut ultra-high molecular weight polyethylene fiber non-woven fabrics at the four inner cutting line positions to avoid material voids or excessive overlap, and pre-lay them in the mold cavity of the helmet female mold to ensure that each layer of the first-cut ultra-high molecular weight polyethylene fiber non-woven fabrics is pre-laid to fit the mold shape of the helmet female mold.
[0052] Step A3: obtaining a preset number of layers of second-cut ultra-high molecular weight polyethylene fiber non-woven fabric.
[0053] A second cut ultra-high molecular weight polyethylene fiber non-woven fabric having 2 to 4 layers is obtained from the multi-layer cut ultra-high molecular weight polyethylene fiber non-woven fabric cut in S101.
[0054] Step A4: placing the second sharp corner positions of each layer of the second cut ultra-high molecular weight polyethylene fiber non-woven fabric to the corresponding first sharp corner positions, and rotating the second sharp corner positions by a preset angle.
[0055] Among them, the preset angle is 30±5°.
[0056] The second sharp angle position of each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth is placed at the corresponding first sharp angle position, that is, the second sharp angle position coincides with the first sharp angle position, and the second sharp angle position is rotated 30±5° clockwise or counterclockwise, that is, on the basis of the first sharp angle position, the corresponding second sharp angle position is rotated 30±5° clockwise or counterclockwise, and the sharp angle position after rotating 30±5° clockwise or counterclockwise is the final sharp angle position of each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth.
[0057] Step A5: overlapping each layer of the second cut ultra-high molecular weight polyethylene fiber non-woven fabric at multiple inner cutting line positions, and pre-laying in the mold cavity of the helmet female mold.
[0058] Specifically, when 2 to 4 layers of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth, i.e., the cut pieces, are laid together, it is necessary to keep the second sharp corner positions of each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth consistent, and overlap each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth at the four inner cutting line positions to avoid material voids or excessive overlap, and pre-lay them in the mold cavity of the helmet female mold to ensure that each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth is pre-laid to fit the mold shape of the helmet female mold.
[0059] Step A6: Return to the step of obtaining a preset number of layers of the second cut ultra-high molecular weight polyethylene fiber non-woven fabric, and stop pre-laying when the number of pre-laying reaches the preset number, to obtain a pre-laid helmet.
[0060] Among them, the preset number of times is 10 to 30 times.
[0061] Specifically, return to step A3, and continue to execute steps A3, A4 and A5, that is, obtain a preset number of layers of second cut ultra-high molecular weight polyethylene fiber non-weft cloth, place the second sharp corner position of each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth to the corresponding first sharp corner position, and rotate the second sharp corner position by a preset angle, overlap each layer of the second cut ultra-high molecular weight polyethylene fiber non-weft cloth at multiple inner cutting line positions, and pre-lay them in the mold cavity of the helmet female mold until the pre-laying is stopped when the number of pre-laying reaches 10 to 30 times, to obtain a pre-laid helmet.
[0062] S103, placing the pre-laid helmet into a pre-pressing mold for pre-pressing and shaping to obtain a pre-pressed helmet.
[0063] Specifically, the pre-pressing process is to put the pre-laid helmet into the pre-pressing mold, ensure that the female mold is at the bottom and the male mold is at the top, start pre-pressing and shaping, and obtain the pre-pressed helmet. The temperature of the pre-pressing process is 25-55°C, the pressure is 10MPa, and the time is 5-15s.
[0064] S104, placing the pre-pressed helmet into a molding die for molding and pressing to obtain a bulletproof main body helmet.
[0065] As an optional implementation, the constant pressure holding temperature of the molding pressing of the pre-pressed helmet is 128-133°C, the constant temperature holding time is 15-30 minutes, and the constant temperature holding pressure is 15MPa.
[0066] Specifically, step S104 is a hot pressing process, in which the pre-pressed helmet is placed in a molding mold for hot pressing. The constant pressure holding temperature is 128-133°C, the constant temperature holding time is 15-30 minutes, the constant temperature holding pressure is 15MPa, and the mold opening temperature is 30-50°C. During the molding and pressing process, 3-6 exhaust operations are performed, the exhaust temperature is 50-100°C, and the helmet mold is raised by 30-50mm during exhaust.
[0067] S105, cutting and pre-laying the multiple layers of reinforcing fiber prepreg in sequence to obtain a pre-laid reinforcing fiber helmet.
[0068] The fibers used in the multi-layer reinforced fiber prepreg are reinforcing fibers, and the reinforcing fibers are a combination of one or more of carbon fibers, aramid fibers, glass fibers, and PBO fibers.
[0069] The multi-layer reinforced fiber prepreg is a composite material made of resin-based reinforced fiber material. The reinforced fiber helmet is prepared by cutting, pre-laying, hot pressing and other processes on the multi-layer reinforced fiber prepreg.
[0070] The resin-based materials are epoxy resin, acrylic resin, polyimide resin and the like.
[0071] The composite material is a prepreg fabric prepared by dipping carbon fiber, aramid fiber and glass fiber in glue, and the resin content is 30-50%.
[0072] The cutting process of the multi-layer reinforced fiber prepreg is to cut the reinforced fiber prepreg into a reinforced fiber prepreg with a set cutting size, wherein the set cutting size includes a circle with a preset radius and four inner cutting lines are opened in the circle.
[0073] Figure 3 A schematic diagram schematically shows the cutting size of the reinforcing fiber prepreg, see Figure 3 As shown, the cutting process of the multi-layer reinforced fiber prepreg is to cut the reinforced fiber prepreg into a circle with a radius of 250 mm, and at the same time open four inner cutting lines, and the length of the four inner cutting lines is 170 mm.
[0074] Specifically, the pre-laying process is to place the cut reinforced fiber prepreg cloth, i.e., the cut pieces, on the pre-laying mold, and each cut piece is overlapped up and down at the position of the inner cutting line to ensure that the cut piece is close to the mold surface. According to the value of the mixing ratio of ultra-high molecular weight polyethylene fiber and reinforcing fiber, after all the cut pieces are laid, they are removed from the pre-laying mold and shaped to ensure that there is no opening at the inner cutting line seam and the cut pieces are tightly fitted.
[0075] The pre-laid mold is designed according to the mixed structure, which can be the female mold or male mold of the forming mold, or other objects whose forming surface conforms to the female mold or male mold.
[0076] S106, placing the pre-laid reinforced fiber helmet in a forming mold, performing forming and pressing, and obtaining a reinforced fiber helmet.
[0077] Specifically, step S106 is a hot pressing process, in which the pre-laid reinforced fiber helmet is placed in a molding die and molding and pressing is started. The constant pressure and heat preservation temperature of the molding and pressing of the pre-laid reinforced fiber helmet is 135-155°C, the constant temperature and heat preservation is 30-50 minutes, the constant temperature and heat preservation pressure is 3-7MPa, and the mold opening temperature is 30-50°C.
[0078] S107, hot-pressing and compounding the bulletproof main body helmet and the reinforced fiber helmet using an adhesive film to obtain a fiber hybrid composite bulletproof helmet.
[0079] Wherein, when the hot pressing composite is vacuum hot pressing, the temperature of vacuum hot pressing is 110-130° C., the holding pressure is 2-5 MPa, and the holding time is 15-30 min.
[0080] As an optional implementation, when the hot pressing composite is non-vacuum hot pressing, the temperature of the non-vacuum hot pressing is 110-130° C., the holding pressure is 5-15 MPa, and the holding time is 15-30 min.
[0081] As an optional implementation, the adhesive film is a hot melt adhesive, and the surface density of the hot melt adhesive film is 60 to 120 g / m 2 .
[0082] Specifically, the formed bulletproof main body helmet and the reinforced fiber helmet are hot-pressed and laminated, and the interlayer interface between the bulletproof main body helmet and the reinforced fiber helmet is laminated using an adhesive film.
[0083] Hot pressing composite can be vacuum hot pressing or non-vacuum mold hot pressing. The vacuum hot pressing process is preferred. The use of the vacuum hot pressing process can improve the uniformity of the adhesive at the interlayer interface.
[0084] The composite adhesive film used at the interface between the layers can be a hot melt adhesive of vinyl or polyethylene type. It is preferred to select a colloid with high affinity to materials such as polyethylene and aramid, and with excellent resistance to high and low temperature, weathering and moisture and heat aging. The surface density of the adhesive film is 60-120g / m 2 The size of the film is 500×500mm. The size of the film is freely variable, mainly covering the entire helmet composite interface.
[0085] The present invention selects different hybrid fiber materials, fiber hybrid structures, fiber hybrid ratios, etc. according to the overall structure and bulletproof performance requirements of the bulletproof helmet and different damage modes, so as to comprehensively exert the performance advantages of each fiber material, obtain hybrid positive effects and optimal bulletproof performance; including the selection of main bulletproof fiber, hybrid reinforcing fiber, hybrid structure and hybrid ratio of each fiber, etc. The bulletproof fiber is UHMWPE fiber, and the reinforcing fiber is a combination of one or more of carbon fiber, aramid fiber, glass fiber and PBO fiber.
[0086] The mixed structure of bulletproof fiber and reinforcing fiber can be designed as follows: the bullet-facing surface is bulletproof fiber and the back-to-back surface is reinforcing fiber; or the bullet-facing surface is reinforcing fiber and the back-to-back surface is bulletproof fiber; or the bullet-facing surface and the back-to-back surface are one or two of the reinforcing fibers, with bulletproof fiber in the middle.
[0087] Through the above steps S101 to S107, a fiber hybrid composite helmet made of one or more composite materials made of ultra-high molecular weight polyethylene fiber, aramid fiber, carbon fiber, glass fiber, etc. can be obtained. The fiber hybrid composite helmet has excellent bulletproof performance and structural rigidity, and can resist 51-type 7.62mm lead-core bullets fired from 54-type pistols, with a bullet mark height of less than or equal to 25mm.
[0088] The present invention is based on the preparation process of ultra-high molecular weight polyethylene bulletproof helmets, and comprehensively utilizes fiber hybrid preparation technology, multi-structure material composite technology, and vacuum hot pressing technology to propose a preparation method for fiber hybrid composite bulletproof helmets. Using this preparation method, a composite bulletproof helmet with both structural rigidity and bulletproof performance can be prepared, which improves the bulletproof performance while reducing the product weight.
[0089] As an optional embodiment: Step 1, select ultra-high molecular weight polyethylene fiber as the main bulletproof material, and carbon fiber as the reinforcing mixed fiber material. The mixed structure is that the bullet-facing surface is ultra-high molecular weight polyethylene material, the back-bounce surface is carbon fiber material, and the fiber mixing ratio is 6.5:1.
[0090] Step 2: Select a surface density of 160g / m 2 , ultra-high molecular weight polyethylene non-woven fabric with a resin content of 15% is used as a bulletproof material, and is cut into pieces of preset cutting size. Take 3 pieces, and pre-lay the helmet in a way that the pieces are overlapped and repeated, and lay them in a cycle for 15 times, with a total of 45 pieces laid. Put the pre-laid helmet into the pre-pressing mold and start pre-pressing, the process is 50℃, 10MPa, 5s. Then transfer it to the molding mold for hot pressing, with a constant pressure insulation temperature of 128℃, a insulation time of 800s, an insulation pressure of 15MPa, a mold opening temperature of 40℃, and 4 exhausts during the pressing process, with an exhaust temperature of 80℃. After the pressing is completed, the bulletproof main body helmet shell of ultra-high molecular weight polyethylene is obtained.
[0091] Step 3: Select a surface density of 200g / m 2 , 3K carbon fiber prepreg with an epoxy resin content of 30%, cut it into pieces with set cutting sizes. According to the laying method of overlapping each piece up and down at the position of the inner cutting line, lay 3 carbon fiber prepregs flat on the helmet male mold. After the laying and shaping is completed, select high-temperature resistant polytetrafluoroethylene demolding cloth as the demolding material and start pressing. The pressing temperature is 140°C, constant temperature and pressure holding for 30 minutes, constant temperature and pressure holding pressure is 5MPa, and the mold opening temperature is 40°C. After the hot pressing is completed, a carbon fiber reinforced helmet shell with a frosted surface is obtained.
[0092] Step 4: Use the ultra-high molecular weight polyethylene bulletproof main body helmet prepared in step 2 as the bullet-facing surface, and use the carbon fiber reinforced helmet prepared in step 3 as the back-bombing surface. The surface density of the composite adhesive at the interface of the two materials is selected to be 120g / m 2 , a vinyl film with a size of 500×500mm, and the three components are placed in a molding mold for hot pressing according to the structure of "anti-bullet surface + film + anti-bullet surface". The process parameters are: temperature of 130℃, pressure of 15MPa, and time of 15min. Thus, a bulletproof helmet made of ultra-high molecular weight polyethylene fiber and carbon fiber with both anti-bullet performance and structural rigidity is obtained, and the bare helmet weighs 1040g.
[0093] The 51-type 7.62mm lead core bullet fired by the 54-type pistol was selected for live ammunition shooting test, and the product test results are shown in Table 1. It can be seen that the bullet mark height is less than or equal to 25mm, which meets the requirements of GA 293-2012, Level 2 standard.
[0094] Table 1 Test results of protective performance of fiber hybrid bulletproof helmet shell
[0095]
[0096] The embodiment of the present invention cuts multiple layers of ultra-high molecular weight polyethylene fiber non-weft cloth according to preset cutting sizes, overlaps multiple layers of cut ultra-high molecular weight polyethylene fiber non-weft cloth layer by layer, and pre-lays them in the mold cavity of the helmet female mold to obtain a pre-laid helmet; puts the pre-laid helmet into a pre-pressing mold for pre-pressing and shaping to obtain a pre-pressed helmet; puts the pre-pressed helmet into a forming mold for molding and pressing to obtain a bulletproof main body helmet; cuts and pre-lays multiple layers of reinforcing fiber prepreg cloth in sequence to obtain a pre-laid reinforced fiber helmet, the fibers used in the multiple layers of reinforcing fiber prepreg cloth are reinforcing fibers, and the reinforcing fibers are one or more combinations of carbon fiber, aramid fiber, glass fiber, and PBO fiber; places the pre-laid reinforced fiber helmet in a forming mold for molding and pressing to obtain a reinforced fiber helmet; hot-presses the bulletproof main body helmet and the reinforcing fiber helmet using a film to obtain a fiber mixed composite bulletproof helmet, and when the hot-pressing and compounding is vacuum hot-pressing, the temperature of the vacuum hot-pressing is 110-130° C., the holding pressure is 2-5 MPa, and the holding time is 15-30 min. In this way, ultra-high molecular weight polyethylene fiber, carbon fiber, aramid fiber, glass fiber, and PBO fiber are selected as the mixed fiber materials of the composite bulletproof helmet, and the performance advantages of different fiber materials are comprehensively utilized to achieve the positive unification of the anti-ballistic performance and structural strength of the bulletproof helmet, so that the bullet mark height value of the mixed fiber material helmet is small, and the anti-ballistic performance of the fiber mixed composite bulletproof helmet is effectively improved. The step-by-step process of bulletproof main body helmet molding, reinforced fiber helmet molding, and composite molding of the bulletproof main body helmet and reinforced fiber helmet is adopted to ensure the quality stability of the molding process of helmets of different materials. The process of hot pressing and compounding the adhesive films at the interfaces of the bulletproof main body helmet and the reinforced fiber helmet adopts vacuum hot pressing to effectively improve the interface bonding strength and interface composite uniformity, and at the same time greatly improves the production efficiency, which is conducive to the engineering application of the invention.
[0097] Figure 4 The structure of a composite bulletproof helmet is schematically shown. The composite bulletproof helmet includes a bulletproof main body helmet and a reinforced fiber helmet. The fiber used in the bulletproof main body helmet is ultra-high molecular weight polyethylene fiber, and the fiber used in the reinforced fiber helmet is a combination of one or more of carbon fiber, aramid fiber, glass fiber, and PBO fiber. The mixing ratio of ultra-high molecular weight polyethylene fiber to reinforced fiber is 4:1 to 6.8:1.
[0098] It should be pointed out here that the description of the above composite bulletproof helmet embodiment is similar to the description of the above fiber hybrid composite bulletproof helmet preparation method embodiment, and has similar beneficial effects as the fiber hybrid composite bulletproof helmet preparation method embodiment. For technical details not disclosed in the embodiment of the composite bulletproof helmet of the embodiment of the present invention, please refer to the description of the fiber hybrid composite bulletproof helmet preparation method embodiment of the present invention for understanding.
[0099] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a fiber hybrid composite bulletproof helmet, characterized in that: The preparation method comprises: Cutting the multi-layer ultra-high molecular weight polyethylene fiber non-woven fabric according to the preset cutting size; Multiple layers of cut ultra-high molecular weight polyethylene fiber non-woven fabrics are stacked one on top of the other and pre-laid in the mold cavity of the helmet female mold to obtain a pre-laid helmet; The pre-laid helmet is placed in a pre-pressing mold for pre-pressing and shaping to obtain a pre-pressed helmet; The pre-pressed helmet is placed in a forming mold for forming and pressing to obtain a bulletproof main body helmet; Cutting and pre-laying multiple layers of reinforcing fiber prepreg in sequence to obtain a pre-laid reinforced fiber helmet, wherein the fibers used in the multiple layers of reinforcing fiber prepreg are reinforcing fibers, and the reinforcing fibers are a combination of one or more of carbon fibers, aramid fibers, glass fibers, and PBO fibers; Placing the pre-laid reinforced fiber helmet in a forming mold and performing forming and pressing to obtain a reinforced fiber helmet; The bulletproof main body helmet and the reinforced fiber helmet are hot-pressed and composited using a film to obtain a fiber hybrid composite bulletproof helmet. When the hot-pressing composite is vacuum hot-pressing, the temperature of the vacuum hot-pressing is 110-130° C., the holding pressure is 2-5 MPa, and the holding time is 15-30 min.
2. The preparation method according to claim 1, characterized in that: The fiber used in the ultra-high molecular weight polyethylene non-woven fabric is ultra-high molecular weight polyethylene fiber, and the mixing ratio of the ultra-high molecular weight polyethylene fiber to the reinforcing fiber is 4:1 to 6.8:
1.
3. The preparation method according to claim 1, characterized in that: When the hot pressing composite is non-vacuum hot pressing, the temperature of the non-vacuum hot pressing is 110-130° C., the holding pressure is 5-15 MPa, and the holding time is 15-30 min.
4. The preparation method according to claim 1, characterized in that: The constant pressure and heat preservation temperature of the molding and pressing of the pre-pressed helmet is 128-133° C., the constant temperature and heat preservation time is 15-30 minutes, and the constant temperature and heat preservation pressure is 15 MPa.
5. The preparation method according to claim 1, characterized in that: The constant pressure holding temperature of the molding and pressing of the pre-laid reinforced fiber helmet is 135-155° C., the constant temperature holding time is 30-50 minutes, and the constant temperature holding pressure is 3-7 MPa.
6. The preparation method according to claim 1, characterized in that: The method comprises: overlapping multiple layers of cut ultra-high molecular weight polyethylene fiber non-woven fabrics layer by layer, and pre-laying them in the mold cavity of the helmet female mold to obtain a pre-laid helmet, comprising: Obtaining a preset number of layers of first-cut ultra-high molecular weight polyethylene fiber non-woven fabric; Keeping the first sharp corner positions of each layer of first-cut ultra-high molecular weight polyethylene fiber non-woven fabrics consistent, overlapping each layer of first-cut ultra-high molecular weight polyethylene fiber non-woven fabrics at multiple inner cutting line positions, and pre-laying them in the mold cavity of the helmet female mold; Obtaining the preset number of layers of second-cut ultra-high molecular weight polyethylene fiber non-woven fabric; Placing the second sharp corner positions of the second cut ultra-high molecular weight polyethylene fiber non-woven fabrics of each layer to the corresponding first sharp corner positions, and rotating the second sharp corner positions by a preset angle; The layers of the second cut ultra-high molecular weight polyethylene fiber non-woven fabrics are overlapped at multiple inner cutting line positions and pre-laid in the mold cavity of the helmet female mold; Return to the step of obtaining the preset number of layers of the second cut ultra-high molecular weight polyethylene fiber non-woven fabric, and stop pre-laying when the number of pre-laying reaches the preset number, to obtain the pre-laid helmet.
7. The preparation method according to claim 6, characterized in that: The preset number of layers is 2 to 4 layers, the preset number of times is 10 to 30 times, and the preset angle is 30±5°.
8. The preparation method according to claim 1, characterized in that: The multi-layer ultra-high molecular weight polyethylene fiber non-woven fabric is used as a bulletproof material, and the surface density of the bulletproof material is 80 to 160 g / m 2 .
9. The preparation method according to claim 1, characterized in that: The adhesive film is a hot melt adhesive, and the surface density of the hot melt adhesive film is 60-120 g / m 2 .
10. A composite bulletproof helmet, characterized in that: The composite bulletproof helmet comprises a bulletproof main body helmet and a reinforced fiber helmet, the fiber used in the bulletproof main body helmet is ultra-high molecular weight polyethylene fiber, the fiber used in the reinforced fiber helmet is a combination of one or more of carbon fiber, aramid fiber, glass fiber, and PBO fiber, and the mixing ratio of the ultra-high molecular weight polyethylene fiber to the reinforced fiber is 4:1 to 6.8:1.
Citation Information
Patent Citations
Ballistic resistant article, semi-finished product for and method of making a shell for a ballistic resistant article
CN104136878A
Preparation method of bulletproof helmet
CN109795132A
Bulletproof helmet body and preparation method thereof
CN112428630A
Forming method of light high-protection PE bulletproof helmet
CN115891202A
High-performance bulletproof helmet shell and preparation method thereof
CN117341232A
Cited By
Lightweight hybrid fiber bulletproof flashboard and preparation method thereof
CN120941838A
Lightweight hybrid fiber bulletproof plugboard and preparation method
CN120941838B
Novel ceramic fiber composite high-strength helmet and preparation method thereof
CN121498476A