Full-transparent flexible strain sensor based on ITO (indium tin oxide) cluster disordered densely-arranged dot matrix
Patent Information
- Application Number
- CN202310629266.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
Smart Images

Figure CN119063615A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fully transparent flexible strain sensors, in particular to a fully transparent flexible strain sensor based on an ITO cluster randomly densely arranged dot matrix. Background Art
[0002] Fully transparent flexible strain sensors have important application value for the next generation of electronic skin and optical touch screens. The above work has shown that ITO cluster lattices can achieve real-time response to strain, but the electrodes used in the sensing unit are metal materials. In order to realize fully transparent strain sensor devices, the metal electrode materials need to be replaced with transparent electrode materials.
[0003] For strain sensors, if ITO bulk thin film is used to make transparent electrodes, the reliability of the sensor under large strain can be guaranteed due to the brittleness of the ITO film. In addition, the preparation process of bulk ITO transparent conductive film includes high-temperature annealing process, which is also difficult for the flexible substrate used in strain sensors to withstand.
[0004] To this end, we designed an all-ITO-based transparent strain sensing unit with PU as the flexible substrate and ITO clusters deposited on both the electrodes and the sensitive medium. Summary of the invention
[0005] The object of the present invention is to provide a fully transparent flexible strain sensor based on a disordered and densely arranged array of ITO clusters, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a fully transparent flexible strain sensor based on a disordered and dense array of ITO clusters, comprising a substrate, an electrode and a cluster conductive network, a fully ITO-based transparent strain sensing unit with PU as a flexible substrate and electrodes and a sensitive medium both deposited with ITO clusters;
[0007] One is the dense lattice of ITO clusters between electrodes; the other is the ITO cluster thin film electrode. There is a certain proportion of pores inside the conductive film assembled by ITO clusters. Under high deposition, the number of stacking layers of clusters also increases accordingly, and it has a three-dimensional stacking structure.
[0008] Preferably, the fully ITO-based transparent strain sensing unit uses metal materials as conductive interdigital electrodes and ITO clusters with disordered close-packed lattices as sensitive media. By controlling the cluster coverage, a group of flexible strain sensing units with different initial resistances are prepared.
[0009] Preferably, a layer of metal electrode is prepared on the flexible substrate, and the metal electrode is made of a molybdenum sheet engraved with an interdigital electrode pattern as a mask.
[0010] Preferably, the dimensions of the flexible substrate are 24 mm in length, 15 mm in width and 0.4 mm in thickness.
[0011] Preferably, the electrodes are metal silver fingers, each finger is 4 mm long and 40 μm wide, the electrode spacing is 40 μm, and there are 48 fingers on one side.
[0012] Preferably, a mask having the same interdigital electrode pattern as that used to prepare the metal electrode is used in the magnetron plasma gas cluster beam instrument;
[0013] Using high deposition amount to deposit multiple layers of ITO clusters to form a conductive film;
[0014] Then, the mask was removed and an ITO conductive electrode was prepared after annealing at 120°C for 1 h in a vacuum environment;
[0015] The same method as above was used to deposit a conductive network consisting of a densely packed lattice of sub-monolayer ITO clusters between the interdigitated electrodes.
[0016] Preferably, in order to achieve real-time monitoring of the conductivity of the sample during the deposition process, a certain amount of quick-drying silver glue still needs to be applied before depositing the cluster lattice conductive network to achieve the connection between the wire and the electrode.
[0017] Preferably, the calculation formula of the film resistivity ρ is:
[0018] Where R is the resistance of the film, which can be obtained from the slope of the fitting curve by linear fitting of the I–V curve of the film, A is the total cross-sectional area perpendicular to the current direction in the equivalent film, w is the electrode length of a single stripe, t is the film thickness, L is the width between electrodes, that is, the length of the film in the current direction, and N is the number of stripes.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] First, the present invention uses PU as a flexible substrate, and the electrodes and sensitive media are all deposited with ITO clusters to form an all-ITO-based transparent strain sensing unit;
[0021] The first is the dense array of ITO clusters between electrodes; the second is the ITO cluster thin film electrode. There is a certain proportion of pores inside the conductive film assembled by ITO clusters. Under high deposition, the number of stacking layers of clusters also increases accordingly, and it has a three-dimensional stacking structure, which ensures the reliability of the sensor under large strain.
[0022] Second, the present invention makes an ITO conductive electrode after annealing at 120°C for 1h in a vacuum environment; using the same method as above, a conductive network consisting of a sub-monolayer ITO cluster densely packed lattice is deposited between the interdigitated electrodes, achieving the effect of heat resistance of the flexible substrate used in the strain sensor. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a schematic diagram of the preparation process of the transparent strain sensing unit based on ITO clusters of the present invention;
[0024] Figure 2 This is the real-time response curve of the transparent strain sensing unit based on all-ITO clusters under small strain (the change of current with stretching, the value marked in the figure is the strain value corresponding to the stretching);
[0025] Figure 3 The present invention is a transparent strain sensing unit based on all-ITO clusters, and the curve of the conductivity and resistance change rate with strain under small strain (a) and its gauge coefficient (b);
[0026] Figure 4 (a) Demonstration photo of the application of the strain sensing unit for monitoring finger joints of the present invention; (b) Real-time response diagram of the all-ITO cluster transparent strain sensing unit to the bending of finger joints;
[0027] Figure 5 It is a schematic diagram showing the change of the conductivity of the ITO cluster conductive film of the present invention with the deposition time;
[0028] Figure 6 A schematic diagram of a thin film structure between two adjacent electrodes in an interdigitated electrode of the present invention;
[0029] Figure 7 The SEM images of the ITO cluster conductive film prepared at a sputtering power of 25 W (a) and 55 W (b) according to the present invention; and the cross-sectional SEM images of the ITO cluster conductive film prepared at a sputtering power of 25 W (c) and 55 W (d);
[0030] Figure 8 (a) I–V curves of ITO cluster films after annealing at different temperatures; (b) changes in resistivity ρ with annealing temperature T (the inset is a graph showing the relationship between lnρ and 1 / T);
[0031] Fig. 9 This is a schematic diagram of the structure of a flexible strain sensing unit based on an ITO cluster disordered close-packed lattice in the present invention;
[0032] Fig.10 (a) The change of conductivity and resistance rate of the ITO cluster close-packed lattice strain sensing unit with strain; (b) The change of gauge coefficient with strain (the inset is a local enlarged view under small strain);
[0033] Fig.11(a) The linear fitting of the resistance change rate of the ITO cluster close-packed lattice strain sensing unit versus strain change curve of the present invention; (b) The residual diagram of the relative resistance change of the sensor calculated according to the linear fitting curve and the measurement result;
[0034] Fig.12 The strain response curves of the ITO cluster close-packed dot matrix sensor unit samples with different basic conductivities of the present invention. (a) The relative change of resistance and (c) the relative change of conductivity with strain; (b) and (d) are the graphs of the change of gauge coefficient with strain calculated based on the data of (a) and (c);
[0035] Fig.13 This is the I–V curve of the sample with a basic conductivity of 100nS under different strains of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] See also Figure 1-13 A fully transparent flexible strain sensor based on a disordered and dense array of ITO clusters, including a substrate, an electrode and a cluster conductive network, a fully ITO-based transparent strain sensing unit with PU as a flexible substrate and electrodes and sensitive media deposited with ITO clusters;
[0038] One is the dense lattice of ITO clusters between electrodes; the other is the ITO cluster thin film electrode. There is a certain proportion of pores inside the conductive film assembled by ITO clusters. Under high deposition, the number of stacking layers of clusters also increases accordingly, and it has a three-dimensional stacking structure.
[0039] Fabrication of fully transparent flexible strain sensing unit
[0040] like Figure 1 As shown, a mask plate with the same interdigital electrode pattern as that used to prepare the metal electrode is used in a magnetron plasma gas cluster beam instrument, and a multilayer ITO cluster is deposited with a high deposition amount to form a conductive film. The mask plate is then removed, and an ITO conductive electrode is made after annealing at 120°C for 1h in a vacuum environment. The conductive network consisting of a sub-monolayer ITO cluster densely packed lattice is deposited between the interdigital electrodes using the same method as above;
[0041] It should be noted that in order to achieve real-time monitoring of the conductivity of the sample during the deposition process, a certain amount of quick-drying silver glue still needs to be applied before depositing the cluster lattice conductive network to achieve the connection between the wire and the electrode.
[0042] Response of transparent flexible strain sensing unit based on all-ITO clusters to strain
[0043] like Figure 2 Shown: The tensile response test results of the transparent strain sensing unit based on all-ITO clusters under small strain. Within the small strain range (ε<1%), the current shows a step change with the increase of tensile strain, which is similar to the metal electrode sample used in the previous article, indicating that the all-ITO cluster-based transparent strain sensing unit can respond well to small strains.
[0044] Unlike strain sensing units based on metal electrodes, the current of the all-ITO transparent strain sensing unit suddenly changes downward at the moment when a tensile force is applied. No obvious tailing phenomenon is observed in the post-deformation stage, but instead a downward protruding peak is observed. This phenomenon is more obvious when ε>1% and in a large strain range.
[0045] In addition, the amplitude of current change gradually decreases under large tensile strain. After one stretching, the current size can gradually recover to 80% to 90% of the current size before stretching, which limits its performance under large strain.
[0046] This may be related to the internal particle movement of the high coverage ITO cluster thin film electrode under large strain. During the stretching process of the fully transparent flexible strain sensor unit, there are two parts that actually participate in the strain response: one is the dense lattice of ITO clusters between the electrodes, which should theoretically contribute to the strain response in the same way as the dense lattice of ITO clusters deposited between metal electrodes discussed above; the other is the ITO cluster thin film electrode. There is a certain proportion of pores inside the conductive film assembled by ITO clusters, and the number of stacked layers of clusters increases accordingly under high deposition, with a certain three-dimensional stacking structure.
[0047] Under a large strain amplitude, in the longitudinal arrangement, the gap between the clusters with good contact with the substrate at the bottom layer and the adjacent clusters is first widened at the moment of external force, resulting in a decrease in current. The adjacent clusters in the upper layer gradually fill the enlarged particle spacing due to the change of the pores in the lower layer, causing the current to slowly recover. In the transverse arrangement, in addition to the deformation in the same direction as the pulling force, there is also a contraction deformation in the direction perpendicular to the pulling force in the middle area of the flexible substrate, which will cause the spacing of some particles in the cluster electrode to shrink under large strain. Properly increasing the annealing temperature of the ITO electrode may help improve the stability of the transparent electrode.
[0048] The response sensitivity of the full ITO cluster transparent strain sensing unit in the small strain range is analyzed, and the relative change of its resistance (or conductivity) and the calculated gauge coefficient with the change of strain are shown as follows: Figure 3As shown in (a) and (b), under small strains of 0<ε<0.5%, the response curves and gauge factors of conductivity and resistance to strain are similar. In the strain range of 0.5%<ε<1.4%, although there are certain differences between the two response curves and gauge factors, the two response curves can keep pace with the strain change, and both have good linearity.
[0049] Among them, the gauge factor measured with resistance as the response signal reached 19 when the strain was 0.9%, which is close to the sample with metal materials as interdigital electrodes.
[0050] Application demonstration of all-ITO cluster transparent strain sensing unit
[0051] Bending strain monitoring is one of the most common detection functions of strain sensors in human body detection. It can be used to monitor human joint activities and has application value in fields such as health monitoring and human body sensing electronic devices. The previous results show that the prepared fully transparent strain sensing unit has a certain detection ability for small strains and is suitable for monitoring joint activities. This section takes the motion detection of finger joints as an example to demonstrate the application of the prepared fully transparent strain sensor based on ITO clusters in joint monitoring.
[0052] Figure 4 (a) is a photo showing the application of finger joint monitoring. The flexible strain sensing unit is placed directly above the finger joint and fixed with tape.
[0053] It should be noted that in actual application, the part deposited with ITO cluster particles needs to be placed on the upper surface, and the direction of the electrode stripes of the interdigitated electrode is perpendicular to the direction of the fingers. On the one hand, this can make the elongation direction of the sensor unit consistent with the current direction, and on the other hand, it is beneficial to increase the response sensitivity of the sensor unit during bending.
[0054] When the finger bends, the flexible substrate bound at the joint bends synchronously. Assuming that the length of the central layer of the substrate remains unchanged, the total length of the upper surface will increase, forming a tensile strain. At this time, the spacing between the ITO clusters on the upper surface is enlarged, and the resistance of the sensor unit increases, and the increase increases with the increase in the bending amplitude; when the degree of bending of the finger weakens or straightens again, the spacing between the clusters decreases until it returns to the level when it was not bent, and the resistance of the sensor unit decreases.
[0055] Figure 4(b) is the response curve of the sensor unit under different degrees of finger bending. The response of the finger in three states: straight, relaxed and bent is selected. The rising and falling edges of the response signal can be clearly identified from the figure, and response platforms of different heights corresponding to the finger movements are presented, indicating that the fully transparent strain sensor unit has good response characteristics for small movements of the finger joints.
[0056] Figure 4 In (b), area 2 shows the response of the sensor unit when the finger is flicked four times with an interval of about 1 s, which shows the response ability of the prepared strain sensor unit during rapid strain.
[0057] To summarize: This chapter studies the response characteristics of the flexible strain sensing unit with disordered close-packed ITO clusters as the sensitive medium to tensile strain, and realizes a fully transparent strain sensing unit with both electrodes and sensitive medium being ITO clusters. The main research results are as follows:
[0058] 1) Using metal materials as conductive interdigital electrodes and ITO clusters as the sensitive medium, a group of flexible strain sensing units with different initial resistances were prepared by controlling the cluster coverage, and their response characteristics to tensile strain were studied. The test shows that the sensing unit can quantitatively respond to small changes in strain, and a lower cluster coverage can obtain a higher sensitivity (gauge factor). For samples with a basic conductivity of 1ns, the gauge factor can be greater than 100; but appropriately increasing the cluster coverage can improve the linear responsiveness of the device in a large strain range, which is beneficial for the practical application of strain sensors. The response time of the sensing unit in a small strain range (<1%) is maintained in the range of 200 to 600ms, with the shortest response time being 230ms, and the response time in a large strain range is increased.
[0059] 2) In view of the limitations of film brittleness and high-temperature annealing process when transparent flexible electrodes are made of ITO bulk films, ITO cluster multilayer densely packed films are used to make electrodes, realizing a fully transparent flexible strain sensing unit with ITO cluster sub-monolayer densely packed dot matrix as the sensitive medium. Its preparation process can be carried out at a low annealing temperature of 120°C and can be adapted to flexible devices using organic substrates. The prepared strain sensor device can reach a gauge factor of 19 under small strains, and can identify strains caused by straightening, relaxing, bending, and rapid tapping of fingers.
[0060] Preparation of ITO Cluster Conductive Film
[0061] Using a quartz glass sheet covered with interdigitated electrodes as the substrate, by significantly extending the deposition time while keeping the deposition parameters stable, an ITO cluster conductive film based on disordered close-packed multilayer ITO clusters can be prepared. We used the relevant parameters in Chapter 2 to prepare the corresponding ITO cluster films based on spherical and multi-branched ITO clusters. Figure 5 This is the curve of the conductivity of the ITO cluster conductive film changing with time during the experiment. It can be seen that the conductivity is very sensitive to the change of the ITO cluster coverage, and the adjustable range is wide, realizing the change process from high resistance state (under low deposition amount) to high conductivity state (under high deposition amount). During the deposition time from 450s to 1h, the conductivity increased by nearly two orders of magnitude, indicating that the number of percolation channels continued to increase during this process.
[0062] In this work, we focus on:
[0063] 1) The influence of cluster morphology on the conductive properties of ITO cluster films;
[0064] 2) The influence of annealing process on the conductive properties of ITO cluster films.
[0065] Sheet resistance is one of the key physical quantities that reflect the conductive properties of thin film materials. The size of the sheet resistance value has nothing to do with the shape but is related to the thickness. Since the sheet resistance is greatly affected by the film thickness, it is appropriate to use resistivity to compare samples of different thicknesses. Here we briefly introduce the calculation method of resistivity when preparing cluster films with interdigitated electrodes as substrates. Figure 6 The figure shows the schematic diagram of the thin film structure between two adjacent electrodes in the interdigitated electrode used. There are 120 such conductive stripe units in the interdigitated electrode used in the experiment. According to the calculation formula of resistance, the calculation formula of the film resistivity ρ can be derived as follows:
[0066]
[0067] Among them, R is the resistance of the film, which can be linearly fitted to the I–V curve of the film and obtained from the slope of the fitting curve, A is the total cross-sectional area perpendicular to the current direction in the equivalent film, w is the electrode length of a single stripe, t is the film thickness, L is the width between electrodes, that is, the length of the film in the current direction, and N is the number of stripes, which is 120 here. Microscopic characterization and thickness estimation of ITO cluster conductive films
[0068] In order to analyze the prepared ITO cluster conductive film microscopically and measure its thickness, the film samples based on multi-branched and spherical ITO clusters were characterized by scanning electron microscopy (SEM) to observe their surface morphology and cross-section.
[0069] Figure 7 (a) and (b) are SEM images of ITO cluster conductive films prepared at sputtering powers of 25W and 55W, respectively. It can be observed from the figure that the surface of the ITO cluster film presents an irregular undulating morphology, indicating whether the film is formed by dense accumulation of nano-sized clusters. This is because the deposition process in this experiment is a completely random process, and the formed ITO cluster particles are directly deposited on the substrate in a manner perpendicular to the substrate. Therefore, the formed ITO cluster film does not have obvious orientation characteristics, and a film is finally formed after multiple layers of disordered stacking. Figure 7 (c) and (d) show that controlling the deposition time can make the cluster films prepared at different sputtering powers have similar thicknesses, and the thicknesses of the two samples are about 93nm and 90nm respectively. The film composed of multi-branched ITO clusters prepared at a sputtering power of 25W has pores of about several nanometers, while the pore diameter in the film composed of spherical ITO clusters prepared at a sputtering power of 55W is slightly reduced, which is consistent with the size of the cluster particles themselves.
[0070] ITO clusters with multi-branch morphology are large in size (about 6nm) and have relatively random branch orientations. When randomly stacked, the branches are prone to spatial hindrance, resulting in larger pores. Spherical ITO clusters are small in size (about 3nm) and have regular shapes, which are conducive to reducing pores when randomly stacked. However, the presence of high porosity also shows that the film thickness measured by the cross-section method cannot accurately reflect the equivalent thickness of the preparation, and the measured value is larger than the actual value. To this end, we need to use the deposition rate measured by the crystal oscillator to estimate the thickness.
[0071] In the experiment, since the cluster beam will form an angle centered on the nozzle, the deposition rate at different distances from the nozzle is not uniform, so the deposition rate reading of the crystal oscillator cannot reflect the actual deposition rate when the cluster beam reaches the substrate. However, using the geometric similarity relationship, the reading in the crystal oscillator can be proportionally converted according to the length of the substrate from the nozzle. The conversion formula is rclc=rsls, where rc and lc represent the deposition rate reading of the quartz crystal detector and its distance from the nozzle, respectively, and rs and ls represent the actual deposition rate at the substrate and the distance from the substrate to the nozzle, respectively. Therefore, the estimated results of the film thickness can be summarized as shown in the following table:
[0072] The thickness of the ITO cluster film estimated from the deposition rate measured by the quartz crystal oscillator
[0073]
[0074] Highly conductive ITO cluster-dense thin films obtained by finite temperature annealing
[0075] The ITO cluster films (equivalent thickness of 46nm to 49nm) prepared at 25W and 55W sputtering powers were annealed at 250℃ for 1h in a vacuum environment, and then the samples were characterized by I–V. The I–V curves of the samples before and after annealing were observed. The central symmetry of the I–V curves of the two ITO cluster films before and after annealing did not change, but the shapes changed significantly. Compared with before annealing, the I–V curves of the samples after annealing showed good linear characteristics, and the conductive properties were significantly improved. The resistivity of the spherical ITO cluster film was reduced to 6.5×10-4Ω·cm, while the resistivity of the multi-branched ITO cluster film was more significantly reduced. After annealing, the resistivity was only 3.1×10-4Ω·cm, which was more than an order of magnitude lower than before annealing. This resistivity value is close to the level of industrial-grade bulk ITO films prepared by standard vapor deposition process (industrial-grade bulk ITO films are usually hundreds of nanometers thick and need to be heat treated at a high temperature above 600°C. The resistivity of the obtained high-grade films is 0.7×10-4Ω·cm to 5.0×10-4Ω·cm). Obviously, the multi-branched cluster morphology is more conducive to making the deposited film obtain high conductivity. Under the same deposition amount, the multi-branched cluster morphology is conducive to achieving close contact between clusters, thereby generating more electron percolation channels in the cluster film.
[0076] At the same time, the highly conductive ITO cluster film also shows excellent transparency in the visible light region. The transmittance of the annealed ITO cluster film in the visible wavelength range of 400nm to 800nm remains above 85%, and can even reach above 90% in some bands. It can be found that the transmittance of the ITO film obtained by the dense stacking of multi-branched clusters is slightly lower than that of the ITO film obtained by the dense stacking of spherical clusters in the short wavelength region. This difference can be attributed to the larger size and irregular shape of the multi-branched ITO clusters, which causes light to experience more scattering losses in the film, thereby reducing the transmittance.
[0077] Effect of annealing temperature on resistivity of ITO cluster conductive films
[0078] In order to analyze the relationship between the resistivity of ITO cluster conductive film and annealing temperature, we prepared a multi-branched ITO cluster densely packed film (equivalent thickness of about 46nm) on the interdigitated electrode under the same conditions, annealed at 50, 100, 150, 200, and 250℃ for 1h each in a vacuum environment and cooled to room temperature. After each annealing, the I–V characteristics of the film were characterized. The results are shown in Figure 2. Figure 8 (a) shown.
[0079] It can be seen that with the increase of annealing temperature, the slope of the I-V curve of the cluster film gradually increases, indicating that the conductivity gradually improves, but the linearity and symmetry of the shape still do not change much. This shows that in uniform annealing, the increase of annealing temperature will not significantly change the density of cluster arrangement in the cluster film, and therefore does not significantly change the transmission mode of electrons between clusters. Figure 8 The I–V curves at each temperature in (a) are linearly fitted and the resistivity is calculated. The relationship between the resistivity and the annealing temperature is plotted as shown in Figure 8 (b) When the annealing temperature is higher than 50°C, the resistivity decreases exponentially with the annealing temperature. It is generally believed that in the high temperature range, the relationship between resistivity and annealing temperature roughly satisfies the Arrhenius equation:
[0080]
[0081] Among them, ρ0 is the pre-exponential factor, ΔE is the thermal activation energy, kB is the Boltzmann constant, and T is the annealing temperature. For the convenience of analysis, take the logarithm of both sides of the equation and get:
[0082]
[0083] Based on this, we plotted the relationship between lnρ and 1 / T (such as Figure 8 (b) The thermal activation energy under annealing can be calculated based on the slope of the figure. According to the linear fitting results, the annealing thermal activation energy of the ITO cluster film is about 310 eV. This result is basically consistent with the thermal activation energy of the ITO cluster dense lattice in the high temperature region under low coverage discussed in the previous section. It is generally believed that the improvement in the conductivity of ITO film is mainly attributed to the effect of high-temperature annealing on oxygen vacancy defects in the film. Higher annealing temperatures will lead to more oxygen vacancies, resulting in a higher concentration of carriers.
[0084] ITO cluster lattice strain sensor
[0085] Flexible strain sensors are a hot topic in current research on materials and devices. According to their working principles, strain sensors can be mainly divided into resistive, piezoelectric and capacitive types, which are used to convert the strain generated by external forces into resistance signals, voltage signals and capacitance signals, respectively, to achieve sensing and response to strain. Among them, resistive strain sensors have a simpler structure and are more convenient to use. They can provide more reliable, more sensitive and faster strain response feedback over a larger strain range, and are widely used in various flexible electronic devices.
[0086] At present, the working principles of nanostructured flexible strain sensors mainly include two categories: crack extension mechanism and quantum tunneling mechanism. The core of the crack mechanism is a series of microcracks artificially created in the nanofilm. The brittleness of the film material is used to make the two ends of the microcracks disconnect or contact with the magnitude of the strain during the strain process, thereby changing the resistance of the film. Flexible strain sensors based on the quantum tunneling mechanism are based on the electron tunneling penetration between the nanostructure units that make up the film. The spacing between adjacent structural units increases or decreases with the magnitude of the strain during the strain process, thereby changing the resistance of the film. Flexible strain sensors based on the quantum tunneling mechanism have more advantages in response sensitivity and response range, especially in terms of controllability. The performance of flexible sensors can be well controlled by controlling the shape, size and spacing of the nanostructure units.
[0087] This chapter is based on the tunneling mechanism and uses ITO clusters densely packed lattices as the sensitive medium to prepare a flexible strain sensing unit, and detects the real-time response characteristics of the sensing unit to tensile strain; compares the tensile properties of the flexible strain sensor under different cluster coverage, and analyzes the relationship between sensor sensitivity and cluster deposition. A fully transparent strain sensor with electrodes and sensitive media based on ITO clusters densely packed lattices is prepared, and demonstrated for several typical application scenarios.
[0088] Structure and response principle of ITO clusters disordered close-packed lattice flexible strain sensing unit
[0089] The flexible strain sensing unit based on the disordered close-packed lattice of ITO clusters prepared in the experiment is mainly divided into three parts, namely the substrate, the electrode and the cluster conductive network. Fig. 9 As shown. Among them, the bottom layer is a transparent flexible substrate. Commonly used materials include polyethylene glycol terephthalate (PET), polyurethane (PU) and polyimide (PI). Such polymer materials have mature industrial products and can be purchased directly on the market. A layer of metal electrode is prepared on the polymer flexible substrate by thermal evaporation mask deposition technology. In this work, silver is selected as the electrode material, and the interdigital electrode is used to improve the sensitivity of the flexible strain sensing unit. In the preparation of the electrode, a molybdenum sheet engraved with an interdigital electrode pattern is used as a mask. The interdigital electrode pattern on the mask is prepared by a wire cutting process and can be reused. When preparing the electrode, the mask is covered on the flexible substrate and placed above the evaporation source of the coating instrument. The silver particles in the evaporation source are heated by electric current to evaporate silver vapor and deposited on the substrate. After the mask is removed, the interdigital electrode can be obtained. ITO clusters are deposited between the interdigital electrodes to form a conductive network.
[0090] In this work, we used a PU material with a length of about 24 mm, a width of about 15 mm, and a thickness of about 0.4 mm as a flexible substrate, and deposited metal silver interdigital electrodes on its surface. Each interdigital electrode was 4 mm long, 40 μm wide, and the electrode spacing was 40 μm. There were 48 interdigital electrodes on one side. During the deposition process, the conductivity of the cluster lattice was monitored and controlled in real time to obtain the predetermined basic conductivity of the sensing unit. In this work, the basic conductivity was set between 1 nS and 100 nS.
[0091] The key to the flexible strain sensing unit responding to strain based on the tunneling effect lies in the use and regulation of the inter-cluster spacing. When the flexible substrate is deformed under the action of external force, the inter-cluster spacing will change. For example, during the stretching process, as the flexible substrate is stretched, the inter-cluster spacing is enlarged; during the bending process of the flexible substrate with the curvature radius as the direction pointing to one side of the cluster conductive network, the clusters are close together due to being in the concave part of the bend, and the particle spacing is reduced. At this time, the tunneling process of electrons between clusters is affected, which is manifested in that the resistance of the cluster conductive network will increase with the increase of cluster spacing and decrease with the decrease of cluster spacing. By measuring the change in resistance of the cluster conductive network during substrate deformation, the actual strain size of the substrate can be obtained. Strain response sensitivity and linearity of ITO cluster close-packed dot matrix sensor unit
[0092] Sensitivity is the most important indicator of the flexible sensor's response to strain, and it also reflects the resolution of the device. For strain sensors, the gauge factor (GF) is usually used to measure sensitivity. The gauge factor is defined as the rate of change of conductivity (or resistance) per unit strain, and the mathematical expression is:
[0093]
[0094] or
[0095]
[0096] Among them, ε is strain (or length change rate), G0 and R0 are the conductivity or resistance of the material when it is not deformed, and ΔG and ΔR are the changes in conductivity or resistance under strain ε. There is no essential difference between these two formulas in mathematics, and both express the evolution of the conductive characteristics of the sensing unit with strain. However, in practical applications, the calculation results of the same device using different formulas will be different, which is mainly affected by the design parameters of the device (such as: working current size, stretching range, etc.). Select one of the measurement methods according to the actual situation, or switch when necessary.
[0097] Fig.10(a) is the conductivity and resistance change rate of the strain sensing unit based on ITO cluster lattice under different strains. Under a small strain of ε<0.6%, the relative change of conductivity and resistance increases slowly with the increase of tensile strain, and the two are almost the same in value; there is an obvious inflection point at ε=0.6%, and the change rate increases rapidly with the increase of strain. At this time, the relative change curves of conductivity and resistance gradually separate, and the relative change of resistance is much greater than the relative change of conductance. The relative change of resistance continues to increase with the increase of strain, and shows a good linear change in the strain range of 0.6% to 7%, until a certain deviation from the linear relationship appears around ε=7%; the relative change of conductance gradually slows down with the increase of strain after ε=2%, and does not show an obvious linear relationship with strain. According to the formula
[0098] and Get as Fig.10 (b) shows the relationship between the gauge factor and strain. Fig.10 (b) It can be seen that in the strain range below 2%, the gauge factor rises rapidly, and the gauge factor can reach GF=32 when resistance is the response signal, and it remains stable in the range of 30 to 35 in the subsequent large strain stretching; the gauge factor with conductivity as the response signal reaches a peak value (GF=18) at ε=2%, and then shows a significant decline.
[0099] Comparing the two methods of calculating the gauge coefficient, under the condition of small strain of ε<0.6%, the performance characterization of the strain sensor unit using resistance or conductivity as the response signal is not significantly different, but in a larger strain range, it is difficult to obtain a high sensitivity using conductivity as the response signal, especially in the strain range of ε>2%, using resistance as the response signal can obtain good linearity and sensitivity. Better linearity is conducive to reducing the error generated when linear calibration is given to the sensor. Linear fitting of data with resistance as the response signal (such as Fig.11 (a)), the residuals of each data point and the fitted value are as follows Fig.11 (b) It can be found that most of the residual values fall within the range of ±0.1, indicating that the obtained data has good linearity. Influence of cluster coverage on the strain response sensitivity of ITO cluster dense array sensing unit
[0100] The sensitivity of the cluster-based conductive network strain sensing unit is directly related to the coverage of the cluster dense lattice, which can be quantified by the basic conductance of the sample when it is deposited. We prepared three ITO cluster dense lattices with basic conductances of 1nS, 10nS, and 100nS, and prepared flexible strain sensing units as described above, and conducted tensile strain response tests with the same parameters under the same electrical conditions.
[0101] Fig.12 (a) (c) are the curves of the relative changes in resistance and conductance of samples with different basic conductivity as a function of strain. It can be seen from the figure that within a smaller strain range (ε<1%), as the basic conductivity decreases, the relative changes in resistance and conductance of the sample caused by strain increase accordingly. Fig.12 (b)(d) show the and The calculated gauge coefficient shows that the low coverage sample with a base conductivity of 1nS has the highest sensitivity (gauge coefficient), and its gauge coefficient reaches 101 (with resistance as the response signal) at a strain of ε=7%. At a larger coverage (initial deposition conductivity of 10nS), the gauge coefficient of the sensing unit is significantly reduced. By comparing the gauge coefficients calculated with resistance and conductivity as the response signal, it can be found that the gauge coefficients with resistance as the response signal in the three samples are significantly higher than the gauge coefficients with conductivity as the response signal. The relative change in resistance maintains a good linear correspondence with the strain over a large strain range, which is more beneficial for practical applications.
[0102] Depend on Fig.12 (b) It can be seen that when the sample with a basic conductivity of 100 nS is stretched to around ε=1.7%, its gauge factor is equivalent to the gauge factor of the sample with a basic conductivity of 1 nS when ε=0.1%. Fig.13 is the I–V curve of the high coverage sample under different strains. It can be observed that the nonlinearity of the curve shape gradually increases with strain, indicating that the cluster particle spacing increases with stretching. Therefore, assuming that the average particle spacing changes with coverage, after stretching, the average particle spacing dM of the high coverage cluster close-packed lattice increases to the average particle spacing dm in the low coverage lattice. From this, the mathematical relationship 1.17dM=1.01dm can be obtained, based on which the relationship between cluster spacing under different cluster coverage can be estimated: dM / dm=01 / 117.
[0103] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A fully transparent flexible strain sensor based on a disordered and dense array of ITO clusters, comprising a substrate, an electrode and a cluster conductive network, characterized in that: The fully ITO-based transparent strain sensing unit uses PU as a flexible substrate, and both the electrode and the sensitive medium are deposited with ITO clusters; One is the dense lattice of ITO clusters between electrodes; The second is the ITO cluster thin film electrode. There is a certain proportion of pores inside the conductive film assembled by ITO clusters. Under high deposition amount, the number of stacking layers of clusters also increases accordingly, and it has a three-dimensional stacking structure.
2. A fully transparent flexible strain sensor based on disordered and densely arranged ITO clusters according to claim 1, characterized in that: The fully ITO-based transparent strain sensing unit uses metal materials as conductive interdigital electrodes and ITO clusters with disordered close-packed lattices as sensitive media. By controlling the cluster coverage, a group of flexible strain sensing units with different initial resistances are prepared.
3. The fully transparent flexible strain sensor based on the disordered and densely arranged ITO clusters according to claim 1 is characterized in that: A layer of metal electrode is prepared on a flexible substrate, and the metal electrode is made of a molybdenum sheet engraved with a cross-finger electrode pattern as a mask.
4. The fully transparent flexible strain sensor based on the disordered and densely arranged ITO clusters according to claim 1 is characterized by: The dimensions of the flexible substrate are 24 mm in length, 15 mm in width, and 0.4 mm in thickness.
5. The fully transparent flexible strain sensor based on the disordered and densely arranged ITO clusters according to claim 3 is characterized by: The electrodes are metal silver fingers, each of which is 4 mm long and 40 μm wide. The electrode spacing is 40 μm, and there are 48 fingers on one side.
6. The method for preparing ITO clusters in a fully transparent flexible strain sensor based on a disordered and dense array of ITO clusters according to claim 1, characterized in that: Using a mask having the same interdigital electrode pattern as that used to prepare the metal electrode in a magnetron plasma gas cluster beam instrument; Using high deposition amount to deposit multiple layers of ITO clusters to form a conductive film; Then, the mask was removed and an ITO conductive electrode was prepared after annealing at 120°C for 1 h in a vacuum environment; The same method as above was used to deposit a conductive network consisting of a densely packed lattice of sub-monolayer ITO clusters between the interdigitated electrodes.
7. The method for preparing ITO clusters in a fully transparent flexible strain sensor based on a disordered and dense array of ITO clusters according to claim 6, characterized in that: In order to achieve real-time monitoring of sample conductivity during the deposition process, a certain amount of quick-drying silver glue still needs to be applied before depositing the cluster lattice conductive network to connect the wires to the electrodes.
8. The method for preparing ITO clusters in a fully transparent flexible strain sensor based on a disordered and dense array of ITO clusters according to claim 6, characterized in that: The calculation formula of film resistivity ρ is: Where R is the resistance of the film, which can be obtained from the slope of the fitting curve by linear fitting of the I–V curve of the film, A is the total cross-sectional area perpendicular to the current direction in the equivalent film, w is the electrode length of a single stripe, t is the film thickness, L is the width between electrodes, that is, the length of the film in the current direction, and N is the number of stripes.
Citation Information
Cited By
Wind pressure measuring device based on intelligent sensing element
CN121230939A
A wind pressure measuring device based on intelligent sensing elements
CN121230939B