Design method for quantifying mix proportion of full-machine-made sand concrete
By quantifying the design method of the comprehensive machine sand concrete mix ratio, comprehensively considering the stone powder content, water reducing agent usage and sand fineness modulus, the detailed raw material usage is calculated, and the accuracy and efficiency of machine sand concrete design in the existing technology is solved. , improves the actual performance of concrete and design reliability.
Patent Information
- Application Number
- CN202411106827.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When designing the mix ratio of machine sand concrete, the existing technology lacks comprehensive considerations for the stone powder content, water reducing agent usage and sand fineness modulus, resulting in a large difference between the actual concrete index and the expected value, low calculation efficiency, and multiple adjustments are required. Match ratio.
The design method for quantitative full-machine sand concrete mix ratio is adopted, and the parameters such as fly ash dosage, ore powder dosage, mineral blending influence coefficient, water glue ratio, water consumption, admixture dosage and other parameters are combined with water reducing agent equivalent The amount of coarse aggregate and fine aggregate is calculated to improve the calculation efficiency and accuracy of the design.
The concrete index is achieved closer to the theoretical value, the number of adjustments of the mix ratio is reduced, the design reliability and calculation efficiency are improved, and the stability of concrete quality is enhanced.
Smart Images

Figure CN119066294A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a design method for quantifying the mix ratio of fully machine-made sand concrete. Background Art
[0002] Artificial sand concrete is widely used in infrastructure construction. The "Ordinary Concrete Mix Design Code" JGJ55-2011 provides the standards and requirements for artificial sand mix ratios. When designing the mix ratio of artificial sand concrete, most operations are carried out in accordance with the above-mentioned design codes.
[0003] The particles of machine-made sand are angular, rough and not smooth, and have a high powder content. The stone powder in machine-made sand, on the one hand, increases the surface area of the sand and the water consumption, but on the other hand, the presence of an appropriate amount of stone powder can improve the grading of the concrete's ultra-fine aggregates, as well as the ball effect produced by the tiny spherical particles, which will improve the workability of the concrete, increase the compactness of the concrete, and thus play a role in improving the overall performance of the concrete. In the relevant technology, there is a defect that the actual indicators of the mixed concrete are far from the expected values due to the lack of consideration of the stone powder content in the machine-made sand when calculating the mix ratio.
[0004] In addition, the amount of water used in the mix ratio of machine-made sand concrete has a direct impact on the workability of fresh cement concrete. In the relevant technology, it is necessary to add a water reducer when mixing concrete to keep the water content of the machine-made sand concrete within the desired range. In the "Ordinary Concrete Mix Design Code" JGJ55-2011, the water amount needs to be retrieved from the table. In actual application, there is a situation where the water amounts corresponding to the mix ratios of C15 to C55 calculated according to the above design code are the same. That is, in the prior art, the method of calculating the water amount is not suitable for the actual application environment.
[0005] When designing the mix ratio, it is also necessary to calculate the sand ratio of sand making. In the "Code for Design of Ordinary Concrete Mix Ratio" JGJ55-2011, the sand ratio is also obtained from the table provided or based on experience. There is a defect that the calculated sand ratio has low accuracy.
[0006] In the related art, when designing the mix ratio, it is necessary to retrieve and obtain it by referring to the table recommended in the "Ordinary Concrete Mix Ratio Design Code" JGJ55-2011, which has the defect of low calculation efficiency of the designed mix ratio. Summary of the invention
[0007] In order to improve the related art, when designing the mix ratio according to the "Ordinary Concrete Mix Design Code" JGJ55-2011, some data need to be obtained by looking up the table, the calculation efficiency of the designed mix ratio is not high, and when designing the mix ratio, there is a lack of comprehensive consideration of the stone powder content, water reducer dosage and sand fineness modulus in the machine-made sand, resulting in a large discrepancy between the actual concrete mix strength and the expected mix strength, and the mix ratio needs to be adjusted many times. This application provides a design method for quantifying the mix ratio of all-machine-made sand concrete to improve the calculation efficiency of the designed mix ratio, and comprehensively considers the stone powder content, water reducer dosage and sand fineness modulus in the all-machine-made sand, so that various indicators of the concrete mixed according to the designed mix ratio are closer to the theoretical values, the reliability of the designed mix ratio is improved, and the calculation efficiency of the designed mix ratio is improved.
[0008] This application provides a quantitative design method for the mix ratio of fully machine-made sand concrete, using the following technical solutions:
[0009] Step S1, obtaining the measured strength of cement f ce and the mix strength of concrete f cu,o According to the fineness modulus of the fully machined sand and the strength grade of the mix ratio, the fly ash dosage β is calculated. f And mineral powder dosage β k , and the fly ash content β f And the mineral powder dosage β k The influence coefficient of mineral admixture γ is calculated, and then the measured strength of cement f ce , the formulation strength f cu,o The water-binder ratio is calculated by using the influence coefficient γ of the mineral admixture
[0010] Step S2, determine the water consumption m of the concrete to be mixed with admixtures wo , according to the water-binder ratio And the water consumption m wo Calculate the amount of adhesive material m bo ;
[0011] Step S3, obtaining the water reduction rate β corresponding to the water reducing agent, according to the water consumption m wo , the amount of the adhesive material m bo The amount of admixture m is calculated by the water reduction rate β ao , and according to the water-binder ratio And the water consumption m wo Calculate the fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co ;
[0012] Step S4, obtaining the sand ratio β of the concrete s, and according to the sand ratio β s , fly ash dosage m fo , Slag powder dosage m ko , the cement dosage m co 、The water consumption m wo , the amount of the admixture m ao and the assumed mass m of concrete mixture per cubic meter cp Calculate the amount of coarse aggregate m go And fine aggregate dosage m so ;
[0013] Step S5, trial mix, adjust and determine the concrete according to the raw material dosage, wherein the raw material dosage includes the fly ash dosage m fo , the amount of slag powder m ko , the amount of the adhesive material m bo , the amount of the admixture m ao , the cement dosage m co , the amount of coarse aggregate m go And the amount of fine aggregate m so .
[0014] Optionally, in step S1, the fly ash content β f The calculation formula is as follows:
[0015] β f =a1·M x -b1·f cu,k +c1;
[0016] Among them, the fineness modulus of machine-made sand is M x The value range of coefficient a1 is not less than 7.6 and not more than 8.4; concrete strength grade f cu,k The value range of coefficient b1 is not less than 0.57 and not more than 0.63; the value range of constant term c1 is not less than 15.2 and not more than 16.8;
[0017] The mineral powder dosage β k The calculation formula is as follows:
[0018] β k =a2·M x +b2·f cu,k +c2;
[0019] Among them, the fineness modulus of machine-made sand is M x The value range of coefficient a2 is not less than 3.80 and not more than 4.20; concrete strength grade f cu,k The value range of the coefficient b2 is not less than 0.019 and not more than 0.021; the value range of the constant term c2 is not less than 3.80 and not more than 4.20.
[0020] Optionally, in step S1, the calculation formula of the mineral admixture influence coefficient γ is as follows:
[0021] γ=-a3·β f -b3·β k +c3;
[0022] Among them, the value range of fly ash content coefficient a3 is not less than 0.898 and not more than 0.993, which is applicable to secondary ash; the value range of slag powder content coefficient b3 is not less than 0.100 and not more than 0.111, which is applicable to S95 slag powder; the value range of constant term c3 is not less than 0.950 and not more than 1.050; β f is the amount of fly ash added; β k is the dosage of mineral powder;
[0023] The water-binder ratio The calculation formula is as follows:
[0024]
[0025] Among them, the value range of coefficient a4 is not less than 0.447 and not more than 0.494, the value range of constant term b4 is not less than 0.008 and not more than 0.010, f cu,o is the mix strength of concrete, f ce It is the actual measured strength of cement and is applicable to the calculation of mix proportion of concrete C55 and below prepared with cement of strength grade 42.5.
[0026] Optionally, step S3 includes:
[0027] Step S31, according to the amount of the adhesive material m bo , the actual slump requirement value H of concrete and the stone powder content N of sand are used to calculate the water consumption m' per cubic meter of concrete without admixture wo , the calculation formula is as follows:
[0028] m' wo =a5·m bo +b5·H+c5·N+d5;
[0029] Among them, the value range of coefficient a5 is not less than 0.2 and not more than 0.3, the value range of coefficient b5 is not less than 160 and not more than 200, the value range of coefficient c5 is not less than 0.80 and not more than 1.00, and the value range of constant term d5 is not less than 115 and not more than 120;
[0030] Step S32, obtaining the water reduction rate β corresponding to the water reducing agent, according to the water consumption m wo , the amount of the adhesive material mbo The amount of admixture m is calculated by the water reduction rate β ao , and according to the water-binder ratio The amount of water to be added after adding the admixture m wo Calculate the fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co .
[0031] Optionally, in step S32, the amount of the additive m ao The calculation formula is as follows:
[0032]
[0033] Wherein, Z is the equivalent value of water reducer, which is used to indicate the amount of water equivalently replaced by 1 kg of water reducer.
[0034] Optionally, the calculation formula of the water reducing agent equivalent value Z is as follows:
[0035] Z = a6·β+b6;
[0036] Wherein, β is the water reduction rate corresponding to the water reducing agent, the value range of the coefficient a6 is not less than 35 and not more than 45, and the value range of the constant term b6 is not less than 0.950 and not more than 1.050.
[0037] Optionally, in step S4, the sand ratio β s The calculation formula is as follows:
[0038] β s =a7·M x -b7·m bo -c7·N+d7;
[0039] Among them, M x is the fineness modulus of sand, m bo is the amount of adhesive; N is the stone powder content of machine-made sand; the value range of coefficient a7 is not less than 9.5 and not more than 10.5, the value range of coefficient b7 is not less than 0.033 and not more than 0.037, the value range of coefficient c7 is not less than 15 and not more than 25, and the value range of constant term d7 is not less than 29.5 and not more than 32.5.
[0040] Optionally, in step S5, the amount of coarse aggregate m go And the amount of fine aggregate m so The calculation formula is as follows:
[0041] m co +m fo +m ko +mso +m go +m wo +m ao =m cp ;
[0042]
[0043] The amount of coarse aggregate m is calculated by the above-mentioned simultaneous equations: go And the amount of fine aggregate m so ; Among them, the assumed mass of concrete mixture per cubic meter is m cp Not less than 2350kg / m 3 And not more than 2450kg / m 3 The value assumed within.
[0044] By adopting the above technical solution, when designing the mix ratio, all data can be obtained through formula calculation, and there is no need to refer to the table retrieval recommended in the "Ordinary Concrete Mix Design Code" JGJ55-2011, thereby improving the calculation efficiency of the design mix ratio.
[0045] When calculating the sand ratio of fully machine-made sand concrete, the stone powder content, fineness modulus and adhesive dosage of the fully machine-made sand are taken into consideration and quantified. The dosage of each raw material in the mix ratio calculated based on the sand ratio is more accurate, and the corresponding indicators of the mixed concrete are closer to the expected values, thereby achieving the purpose of reducing the number of mix ratio adjustments.
[0046] In addition, the concept of water reducer equivalent value has been added, which uses 1kg of water reducer to replace the value of water consumption to achieve the best effect of water reducer.
[0047] By adding the influence coefficients of fly ash and mineral powder on the calculation formulas for the fly ash dosage and mineral powder dosage, the method of obtaining data by referring to the table recommended in the "Ordinary Concrete Mix Design Code" JGJ55-2011 in the existing technology is replaced, so as to further improve the calculation efficiency of the design mix.
[0048] By improving the scientific nature of the mix design of fully machine-made sand concrete, the stability of concrete quality can be improved and the occurrence of quality problems can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be discussed below. Obviously, the technical solutions described in conjunction with the drawings are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments and their drawings can be obtained based on the embodiments shown in these drawings without paying creative work.
[0050] Figure 1 It is a flow chart of the design method for quantifying the mix proportion of fully machine-made sand concrete.
[0051] Figure 2 It is a specific flow chart of step S3. DETAILED DESCRIPTION
[0052] The technical solutions of various embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] The embodiment of the present invention provides a method for designing the mix ratio of fully machine-made sand concrete. Figure 1 to Figure 2 As shown, including:
[0054] Step S1, obtaining the measured strength of cement f ce and the mix strength of concrete f cu,o According to the fineness modulus of the fully machined sand and the strength grade of the mix ratio, the fly ash dosage β is calculated. f And mineral powder dosage β k , and the fly ash content β f And mineral powder dosage β k The influence coefficient of mineral admixture γ is calculated, and then the actual strength of cement f ce , preparation strength f cu,o The water-binder ratio is calculated by the influence coefficient γ of mineral admixtures
[0055] Step S2, determine the water consumption m of the concrete to be mixed with admixtures wo , according to the water-binder ratio And water consumption m wo Calculate the amount of adhesive material m bo ;
[0056] Step S3, obtaining the water reduction rate β corresponding to the water reducing agent, according to the water consumption m wo 、Amount of adhesive material m bo And the water reduction rate β is used to calculate the amount of admixture m ao , and according to the water-binder ratio And water consumption m wo Calculate the fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co ;
[0057] Step S4, obtaining the sand ratio β of the concrete s , and according to the sand ratio βs , fly ash dosage m fo , Slag powder dosage m ko , cement consumption m co , water consumption m wo 、Amount of admixture m ao and the assumed mass m of concrete mixture per cubic meter cp Calculate the amount of coarse aggregate m go And fine aggregate dosage m so ;
[0058] Step S5, trial mix, adjust and determine the concrete according to the raw material dosage, the raw material dosage includes the fly ash dosage m fo , Slag powder dosage m ko 、Amount of adhesive material m bo 、Amount of admixture m ao , cement consumption m co , Coarse aggregate dosage m go And fine aggregate dosage m so
[0059] Specifically, in this embodiment, the water consumption m per cubic meter of concrete is determined according to the concrete strength. wo ; Among them, the water consumption corresponding to C15, C20, C25, C30, C35 and C40 is m wo The value range is not less than 170kg / m 3 And not more than 185kg / m 3 , water consumption corresponding to C50 and C55 m wo The value range is not less than 150kg / m 3 And not more than 165kg / m 3 .
[0060] For step S3, the amount of the adhesive material m bo , fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co , the calculation formula is as follows:
[0061] m fo =β f ·m bo ;m ko =β k ·m bo ;m co =(1-βf-β k )m bo ;
[0062] In a preferred embodiment of the present invention, in step S1, the fly ash content β f The calculation formula is as follows:
[0063] β f =a1·M x -b1·f cu,k +c1;
[0064] Among them, the fineness modulus of machine-made sand is M x The value range of coefficient a1 is not less than 7.6 and not more than 8.4; concrete strength grade f cu,k The value range of coefficient b1 is not less than 0.57 and not more than 0.63; the value range of constant term c1 is not less than 15.2 and not more than 16.8;
[0065] The preferred value of coefficient a1 is 8.0; the preferred value of coefficient b1 is 0.6; the preferred value of constant term c1 is 16.0;
[0066] The optimal equation is obtained:
[0067] β f =8.0·M x -0.6·f cu,k +16.0.
[0068] Mineral powder dosage β k The calculation formula is as follows:
[0069] β k =a2·M x +b2·f cu,k +c2;
[0070] Among them, the fineness modulus of machine-made sand is M x The value range of coefficient a2 is not less than 3.80 and not more than 4.20; concrete strength grade f cu,k The value range of coefficient b2 is not less than 0.019 and not more than 0.021; the value range of constant term c2 is not less than 3.80 and not more than 4.20;
[0071] The preferred value of coefficient a2 is 4.0; the preferred value of coefficient b2 is 0.020; the preferred value of constant term c2 is 4.00;
[0072] The optimal equation is obtained:
[0073] β k =4.0·M x +0.020·f cu,k +4.00.
[0074] In a preferred embodiment of the present invention, in step S1, the calculation formula of the mineral admixture influence coefficient γ is as follows:
[0075] γ=-a3·β f -b3·βk +c3;
[0076] Among them, the value range of fly ash content coefficient a3 is not less than 0.898 and not more than 0.993, which is applicable to secondary ash; the value range of slag powder content coefficient b3 is not less than 0.100 and not more than 0.111, which is applicable to S95 slag powder; the value range of constant term c3 is not less than 0.950 and not more than 1.050; β f is the amount of fly ash added; β k is the dosage of mineral powder;
[0077] Water-cement ratio The calculation formula is as follows:
[0078]
[0079] Among them, the value range of coefficient a4 is not less than 0.447 and not more than 0.494, the value range of constant term b4 is not less than 0.008 and not more than 0.010, f cu,o is the mix strength of concrete, f ce It is the actual measured strength of cement and is applicable to the calculation of mix proportion of concrete C55 and below prepared with cement of strength grade 42.5.
[0080] Specifically, in this embodiment:
[0081] The calculation formula for the influence coefficient γ of mineral admixtures is:
[0082] The preferred value of coefficient a3 is 0.945, the preferred value of coefficient b3 is 0.105, and the preferred value of constant term c3 is 1. Then the preferred equation of the mineral admixture influence coefficient γ is:
[0083] γ=-0.945β f -0.105β k +1.00.
[0084] When actually calculating the influence coefficient γ of mineral admixtures, for the concrete mix ratio using secondary ash and S95 slag powder, the user can directly select the above-mentioned optimal equation and change the fly ash content β f And mineral powder dosage β k Substitute it into the equation and use the calculation tool to quickly obtain the value of the mineral admixture influence coefficient γ.
[0085] Water-cement ratio The calculation formula is as follows, where the preferred value of coefficient a4 is 0.47 and the preferred value of coefficient b4 is 0.009, and the preferred equation is obtained:
[0086]
[0087] In a preferred embodiment of the present invention, step S3 includes:
[0088] Step S31, according to the amount of glue m bo , the actual slump requirement value H of concrete and the stone powder content N of sand are used to calculate the water consumption m' per cubic meter of concrete without admixture wo , the calculation formula is as follows:
[0089] m' wo =a5·m bo +b5·H+c5·N+d5;
[0090] Among them, the value range of coefficient a5 is not less than 0.2 and not more than 0.3, the value range of coefficient b5 is not less than 160 and not more than 200, the value range of coefficient c5 is not less than 0.80 and not more than 1.00, and the value range of constant term d5 is not less than 115 and not more than 120;
[0091] Step S32, obtaining the water reduction rate β corresponding to the water reducing agent, according to the water consumption m wo 、Amount of adhesive material m bo And the water reduction rate β is used to calculate the amount of admixture m ao , and according to the water-binder ratio The amount of water to be added after adding admixtures m wo Calculate the fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co .
[0092] Specifically, in this embodiment, for the water consumption m' wo The calculation formula is:
[0093] The preferred value of coefficient a5 is 0.25, the preferred value of coefficient b5 is 0.18, the preferred value of coefficient c5 is 180, and the preferred value of d5 is 118, and the corresponding preferred equation is obtained:
[0094] m, wo =0.25B+0.18H+180N+118.
[0095] In a preferred embodiment of the present invention, in step S32, the amount of additive m ao The calculation formula is as follows:
[0096]
[0097] Among them, as the water reduction rate β increases, the water reducer equivalent value Z also increases, which is the characteristic of the water reducer itself.
[0098] In a preferred embodiment of the present invention, the calculation formula of the water reducing agent equivalent value Z is as follows:
[0099] Z = a6·β+b6;
[0100] Among them, β is the water reduction rate corresponding to the water reducer, the value range of the coefficient a6 is not less than 35 and not more than 45, and the value range of the constant term b6 is not less than 0.950 and not more than 1.050.
[0101] The preferred value of coefficient a6 is 40, and the preferred value of constant term b6 is 1.00;
[0102] The optimal equation is obtained:
[0103] Z=40β+1.00.
[0104] Specifically, in this embodiment, the water reducing agent equivalent value is used: that is, under given mix ratio conditions, the amount of water reducing agent determined by experiments is used to adjust the water reduction rate of concrete by controlling the amount of water reducing agent.
[0105] According to the JGJ55-2011 standard, when using crushed stone with a particle size of 31.5 to prepare concrete with a slump of 200mm:
[0106] The water consumption without admixture is calculated as
[0107] 205+(200mm-90mm) / 20×5=232.5kg / m 3 ;
[0108] If the water-reducing rate of the admixture is 25%, after adding the recommended admixture of 2%, the water consumption of concrete is 232.5×(1-25%)=174.3kg. The calculated water consumption of the mix ratios C15 to C55 is shown in Table 1. It can be seen that different mix ratios calculate the same water consumption, and the water consumption needs to be adjusted. Therefore, the error in the admixture and water consumption calculated according to the calculation method of JGJ55-2011 is large, which is obviously inappropriate.
[0109] Table 1
[0110]
[0111] In other words, there is a big difference between the calculated value according to JGJ55-2011 and the actual adjusted value of the mix ratio.
[0112] Therefore, redefine the formula for water consumption without admixture:
[0113] m' wo =a5·m bo +b5·H+c5·N+d5;
[0114] The amount of admixture per cubic meter of concrete ao It should be calculated as follows:
[0115]
[0116] In order to calculate the dosage of admixtures, the concept of water reducer equivalent value is introduced. Water reducer equivalent value refers to the amount of water m' minus under given mix ratio conditions. wo -m wo , and then according to the characteristic value Z of the water reducer itself, according to the formula The water reducing agent dosage is calculated and determined so that the concrete reaches the water reducing agent dosage required by the design. By using the water reducing agent equivalent value, the water reducing agent dosage can be reasonably adjusted according to the specific mix ratio requirements to achieve the best use effect of the water reducing agent.
[0117] In a preferred embodiment of the present invention, in step S4, the sand ratio β s The calculation formula is as follows:
[0118] β s =a7·M x -b7·m bo -c7·N+d7;
[0119] Among them, M x is the fineness modulus of sand, m bo is the amount of glue; N is the stone powder content of sand; the value range of coefficient a7 is not less than 9.5 and not more than 10.5, the value range of coefficient b7 is not less than 0.033 and not more than 0.037, the value range of coefficient c7 is not less than 15 and not more than 25, and the value range of constant term d7 is not less than 29.5 and not more than 32.5.
[0120] The preferred value of coefficient a7 is 10, the preferred value of coefficient b7 is 0.035, the preferred value of coefficient c7 is 20, and the preferred value of constant term d7 is 31, resulting in the preferred equation:
[0121] β s =10·M x -0.035 m bo -20·N+31.
[0122] The above sand ratio β s In the calculation formula of , the stone powder content N in the whole machine-made sand is taken as an influencing factor into the sand ratio β s Calculate the amount of coarse aggregate m go And fine aggregate dosage m so The calculation results are more reliable.
[0123] In a preferred embodiment of the present invention, in step S5, the amount of coarse aggregate m go And fine aggregate dosage m so The calculation formula is as follows:
[0124] m co +m fo +m ko +m so +m go +m wo +m ao =m cp ;
[0125]
[0126] The amount of coarse aggregate m is calculated by the above simultaneous equations: go And fine aggregate dosage m so ; Among them, the assumed mass of concrete mixture per cubic meter is m cp Not less than 2350kg / m 3 And not more than 2450kg / m 3 The value assumed within.
[0127] Specifically, in this embodiment, a preparation example of C30 concrete mix ratio is provided:
[0128] Known machine-made sand and gravel powder content N = 10%, fineness modulus M x =2.6, measured strength of cement f ce =49.3, admixture water reduction rate β = 25%, concrete slump H = 200;
[0129] The concrete mix strength f cu,o =f cu,k +1.645σ=30+1.645×5=38.2;
[0130] Fly ash content β f (%):
[0131] β f =a1·M x -b1·f cu,k +c1=8.0×2.6-0.6×30+16.0=18.8;
[0132] Mineral powder dosage β k (%):
[0133] β k =a2·M x +b2·f cu,k +c2=4.0×2.6+0.02×30+4.0=14.4;
[0134] Influence coefficient of mineral admixtures:
[0135] γ=-α3·β f -b3·βk +c3=-0.945×18.8%-0.105×14.4%+1.00=0.8072;
[0136] Subsequently, by Get the equation
[0137] Calculate the water-binder ratio
[0138] The water consumption per cubic meter of C30 concrete is 175kg / m 3 , calculate the amount of adhesive material Fly ash dosage m fo =β f ·m bo =18.8%×361=68;
[0139] Slag powder dosagem ko =β k ·m bo =14.4%×361=52;
[0140] Cement dosage m co =(1-β f -β k )m bo =(1-18.8%-14.4%)×361=241;
[0141] As the water reduction rate β increases, the water reducer equivalent value Z also increases, which is the characteristic of the water reducer itself. In order to calculate the dosage of admixtures, the concept of water reducer equivalent value is introduced. The water reducer equivalent value refers to the amount of water m' minus the water under given mix ratio conditions. wo -m wo , and then according to the characteristic value Z of the water reducer itself, according to the formula Calculate and determine the amount of water reducing agent so that the concrete reaches the design requirements of water reducing agent:
[0142] Calculate the value of equivalent water replacement per kilogram of admixture
[0143] Z=a6·β+b6=40×25%+1=11.0;
[0144] When no admixture is added, the amount of water required for concrete to reach the required slump is m' wo :
[0145] m' wo =a5·m bo +b5·H+c5·N+d5=0.25×361+0.18×200+180×10%+118=262;
[0146] Dosage of admixture m ao :
[0147]
[0148] Sand ratio of concrete with fully machine-made sand β s (%):
[0149] β s =(a7·M x -b7·m bo -c7·N+d7)%=(10×2.6-0.035×361-20×10%+31)%=42.37%;
[0150] Total amount of sand and gravel: m so +m go =2350-241-68-52-7.93-175=1806.07;
[0151] Sand: m so =(m so +m go )×42.37%=765.47,m go =1806.07-765.47=1041.3;
[0152] The corresponding matching ratio is as follows:
[0153] Cement: fly ash: mineral powder: sand: stone: admixture: water = 241:68:52:765:1041:7.93.
[0154] Provide a calculation example of C50 concrete mix ratio:
[0155] The content of fully machined sand and gravel powder is known to be N = 8%, and the fineness modulus is M x =2.7, measured strength of cement f ce =49.3, admixture water reduction rate β = 25%, concrete slump H = 200;
[0156] The concrete mix strength f cu,o =f cu,k +1.645σ=50+1.645×5=59.87;
[0157] Fly ash content β f (%):
[0158] β f =a1·M x -b1·f cu,k +c1=8.0×2.7-0.6×50+16.0=7.6;
[0159] Mineral powder dosage β k (%):
[0160] β k =a2·M x +b2·f cu,k +c2=4.0×2.7+0.02×50+4.0=15.8;
[0161] Influence coefficient of mineral admixtures:
[0162] γ=-a3·β f -b3·β k +c3=-0.945×7.6%-0.105×15.8%+1.00=0.9116;
[0163] Subsequently, by Get the equation Calculate the water-binder ratio
[0164] The water consumption per cubic meter of C50 concrete is 165kg / m 3 , calculate the amount of adhesive material Fly ash dosage m fo =β f ·m bo =7.6%×471=36;
[0165] Slag powder dosagem ko =β k ·m bo =15.8%×471=74;
[0166] Cement dosage m co =(1-β f -β k )m bo =(1-7.6%-15.8%)×471=361;
[0167] As the water reduction rate β increases, the water reducer equivalent value Z also increases, which is the characteristic of the water reducer itself. In order to calculate the dosage of admixtures, the concept of water reducer equivalent value is introduced. The water reducer equivalent value refers to the amount of water m' minus the water under given mix ratio conditions. wo -m wo , and then according to the characteristic value Z of the water reducer itself, according to the formula Calculate and determine the amount of water reducing agent so that the concrete reaches the design requirements of water reducing agent:
[0168] The value of each kilogram of admixture that is equivalent to replacing water is Z = a6·β + b6 = 40×25% + 1 = 11.0.
[0169] The amount of water required to achieve the required slump of concrete without admixtures
[0170] m' wo =a5·m bo +b5·H+c5·N+d5=0.25×471+0.18×200+180×8%+118=286;
[0171] Dosage of admixture
[0172] Sand ratio of concrete with fully manufactured sand (%) β s =(a7·M x -b7·m bo -c7·N+d7)%=(10×2.7-0.035×471-20×8%+31)%=39.9%;
[0173] Total amount of sand and gravel m so +m go =2380-361-36-74-11-165=1733.15;
[0174] Sand so =(m so +m go )×39.9%=691.88,m go =1713.15-671.88=1041.26;
[0175] The corresponding matching ratio is as follows:
[0176] Cement: fly ash: mineral powder: sand: stone: admixture: water = 361:36:74:692:1041:11.
[0177] In a preferred embodiment of the present invention, the amount of coarse aggregate and the amount of fine aggregate are calculated according to the volume method, and the corresponding calculation formula is as follows:
[0178]
[0179] Among them, ρ c is the cement density (kg / m 3 ), should be determined according to the "Determination of cement density" GB / T208, or 2900kg / m 3 ~3100kg / m 3 , ρ f is the density of mineral admixture (kg / m 3 ), can be determined according to the "Determination of cement density" GB / T208-2014, ρ g is the apparent density of coarse aggregate (kg / m 3), should be measured according to the current industry standard "Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete" JGJ52-2006, ρ s is the apparent density of fine aggregate (kg / m 3 ), should be measured according to the current industry standard "Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete" JGJ52-2006, ρ w is the density of water (kg / m 3 ), can be 1000kg / m 3 , α is the percentage of air content in concrete. When no air-entraining admixture is used, α can be taken as 1.
[0180] In summary, when designing the mix ratio, all data can be obtained through formula calculation, without the need to refer to the table retrieval recommended in the "Ordinary Concrete Mix Ratio Design Code" JGJ55-2011, which improves the calculation efficiency of the design mix ratio. In actual calculation, write each formula into the pre-prepared calculation template, substitute each known quantity into the calculation template and calculate, and you can get the calculation results of each raw material amount.
[0181] When calculating the sand ratio, the stone powder content N of the whole machine-made sand is added into the calculation, and the fineness modulus M x Taking the sand ratio and adhesive into consideration, the amount of each raw material in the mix ratio calculated based on the sand ratio is more accurate, and the corresponding indicators of the mixed concrete are closer to the expected values, thereby achieving the purpose of reducing the number of mix ratio adjustments.
[0182] In addition, the concept of water reducer equivalent value has been added, which uses 1kg of water reducer to replace the value of water consumption to achieve the best effect of water reducer.
[0183] By adding the fly ash and mineral powder influence coefficients to the calculation formula for fly ash and mineral powder dosage, the method of obtaining data by referring to the table recommended in the "Ordinary Concrete Mix Design Code" JGJ55-2011 in the existing technology is replaced, and the calculation efficiency of the design mix is further improved. By improving the scientific nature of the mix design of all-machine-made sand concrete, the stability of concrete quality is improved.
Claims
1. A quantitative design method for the mix ratio of fully machine-made sand concrete, characterized by: Step S1, obtaining the measured strength of cement f ce and the mix strength of concrete f cu,o According to the fineness modulus of the fully machined sand and the strength grade of the mix ratio, the fly ash dosage β is calculated. f And mineral powder dosage β k , and the fly ash content β f And the mineral powder dosage β k The influence coefficient of mineral admixture γ is calculated, and then the measured strength of cement f ce , the formulation strength f cu,o The water-binder ratio is calculated by using the influence coefficient γ of the mineral admixture Step S2, determine the water consumption m of the concrete to be mixed with admixtures wo , according to the water-binder ratio And the water consumption m wo Calculate the amount of adhesive material m bo ; Step S3, obtaining the water reduction rate β corresponding to the water reducing agent, according to the water consumption m wo , the amount of the adhesive material m bo The amount of admixture m is calculated by the water reduction rate β ao , and according to the water-binder ratio And the water consumption m wo Calculate the fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co ; Step S4, obtaining the sand content β of the concrete s , and according to the sand ratio β s , the amount of fly ash m fo , the amount of slag powder m ko , the cement dosage m co 、The water consumption m wo , the amount of the admixture m ao and the assumed mass m of concrete mixture per cubic meter cp Calculate the amount of coarse aggregate m go And fine aggregate dosage m so ; Step S5, trial mix, adjust and determine the concrete according to the raw material dosage, wherein the raw material dosage includes the fly ash dosage m fo , the amount of slag powder m ko , the amount of the adhesive material m bo , the amount of the admixture m ao , the cement dosage m co , the amount of coarse aggregate m go And the amount of fine aggregate m so .
2. The design method according to claim 1, characterized in that: In step S1, the fly ash content β f The calculation formula is as follows: β f =a1·M x -b1·f cu,k +c1; Among them, the fineness modulus of machine-made sand is M x The value range of coefficient a1 is not less than 7.6 and not more than 8.4; concrete strength grade f cu,k The value range of the coefficient b1 is not less than 0.57 and not more than 0.63; the value range of the constant term c1 is not less than 15.2 and not more than 16.8; The mineral powder dosage β k The calculation formula is as follows: β k =a2·M x +b2·f cu,k +c2; Among them, the fineness modulus of machine-made sand is M x The value range of coefficient a2 is not less than 3.80 and not more than 4.20; concrete strength grade f cu,k The value range of the coefficient b2 is not less than 0.019 and not more than 0.021; the value range of the constant term c2 is not less than 3.80 and not more than 4.
20.
3. The design method according to claim 2, characterized in that: In step S1, the calculation formula of the mineral admixture influence coefficient γ is as follows: γ=-a3·β f -b3·b k +c3; Among them, the value range of fly ash content coefficient a3 is not less than 0.898 and not more than 0.993, which is applicable to secondary ash; the value range of slag powder content coefficient b3 is not less than 0.100 and not more than 0.111, which is applicable to S95 slag powder; the value range of constant term c3 is not less than 0.950 and not more than 1.050; β f is the amount of fly ash added; β k is the dosage of mineral powder; The water-binder ratio The calculation formula is as follows: Among them, the value range of coefficient a4 is not less than 0.447 and not more than 0.494, the value range of constant term b4 is not less than 0.008 and not more than 0.010, f cu,o is the mix strength of concrete, f ce It is the actual measured strength of cement and is applicable to the calculation of mix proportion of concrete C55 and below prepared with cement of strength grade 42.
5.
4. The design method according to claim 3, characterized in that: The step S3 comprises: Step S31, according to the amount of the adhesive material m bo , the actual slump requirement value H of concrete and the stone powder content N of sand are used to calculate the water consumption m' per cubic meter of concrete without admixture wo , the calculation formula is as follows: m' wo =a5·m bo +b5·H+c5·N+d5; Among them, the value range of coefficient a5 is not less than 0.2 and not more than 0.3, the value range of coefficient b5 is not less than 160 and not more than 200, the value range of coefficient c5 is not less than 0.80 and not more than 1.00, and the value range of constant term d5 is not less than 115 and not more than 120; Step S32, obtaining the water reduction rate β corresponding to the water reducing agent, according to the water consumption m wo , the amount of the adhesive material m bo The amount of admixture m is calculated by the water reduction rate β ao , and according to the water-binder ratio The amount of water to be added after adding the admixture m wo Calculate the fly ash dosage m fo , Slag powder dosage m ko And cement consumption m co .
5. The design method according to claim 4, characterized in that: In the step S32, the amount of the additive m ao The calculation formula is as follows: Wherein, Z is the equivalent value of water reducer, which is used to indicate the amount of water equivalently replaced by 1 kg of water reducer.
6. The design method according to claim 5, characterized in that: The calculation formula of the water reducing agent equivalent value Z is as follows: Z = a6·β+b6; Wherein, β is the water reduction rate corresponding to the water reducing agent, the value range of the coefficient a6 is not less than 35 and not more than 45, and the value range of the constant term b6 is not less than 0.950 and not more than 1.
050.
7. The design method according to claim 6, characterized in that: In the step S4, the sand ratio β s The calculation formula is as follows: β s =a7·M x -b7·m bo -c7·N+d7; Among them, M x is the fineness modulus of sand, m bo is the amount of glue; N is the stone powder content of sand; the value range of coefficient a7 is not less than 9.5 and not more than 10.5, the value range of coefficient b7 is not less than 0.033 and not more than 0.037, the value range of coefficient c7 is not less than 15 and not more than 25, and the value range of constant term d7 is not less than 29.5 and not more than 32.
5.
8. The design method according to claim 7, characterized in that: In step S5, the amount of coarse aggregate m go And the amount of fine aggregate m so The calculation formula is as follows: m co +m fo +m ko +m so +m go +m wo +m ao =m cp ; The amount of coarse aggregate m is calculated by the above-mentioned simultaneous equations. go And the amount of fine aggregate m so ; Among them, the assumed mass of concrete mixture per cubic meter is m cp Not less than 2350kg / m 3 And not more than 2450kg / m 3 The value assumed within.
Citation Information
Cited By
Method for designing mix proportion of magnesium grouting reinforcement slurry
CN119724412A