Multilayer ceramic capacitor, method for manufacturing the same,

By introducing pores in the shell into the ceramic layer of the laminated ceramic capacitor, the movement of oxygen defects is hindered, and the problem of accumulation of oxygen defects in the dielectric layer is solved, and insulation reliability and moisture resistance are improved.

CN119069258APending Publication Date: 2024-12-03TAIYO YUDEN KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410677507.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2024-05-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the laminated ceramic capacitor, oxygen defects are easily generated when the content of rare earth elements in the dielectric layer increases, causing oxygen defects to move from the dielectric layer to the internal electrode layer, reducing insulation reliability.

Method used

By introducing pores in the shell into the grains of the ceramic layer, the movement of oxygen defects is hindered, thereby suppressing the accumulation of oxygen defects in the boundary between the dielectric layer and the internal electrode layer, and improving insulation reliability.

Benefits of technology

It effectively improves the insulation reliability of the stacked ceramic capacitors and shows excellent performance in moisture resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069258A_ABST
    Figure CN119069258A_ABST
Patent Text Reader

Abstract

The invention provides a multilayer ceramic capacitor capable of improving insulation reliability of the multilayer ceramic capacitor, a method for manufacturing the same, a circuit module, and an electronic apparatus. A main body of a multilayer ceramic capacitor according to one embodiment includes a first internal electrode layer, a second internal electrode layer, and a ceramic layer. The ceramic layer is disposed between the first internal electrode layer and the second internal electrode layer, and includes crystal grains of a ceramic material. The crystal grain has a core portion and a shell portion covering the core portion. The shell portion includes one or more in-shell apertures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates mainly to a laminated ceramic capacitor and a method for manufacturing the laminated ceramic capacitor. The present invention also relates to a circuit assembly including the laminated ceramic capacitor and an electronic device including the circuit assembly. Background Art

[0002] A multilayer ceramic capacitor is mounted in various electronic devices. The multilayer ceramic capacitor has a capacitance generating portion, which includes a dielectric layer and an internal electrode layer sandwiching the dielectric layer. It is known that by making the dielectric layer containing barium titanate as the main component contain rare earth elements, various properties of the multilayer ceramic capacitor can be improved. For example, Japanese Patent Publication No. 2014-090119 discloses that by making the dielectric layer containing barium titanate as the main component contain rare earth elements, the electrostatic capacitance and high temperature load life of the multilayer ceramic capacitor can be improved.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2014-090119 Summary of the invention

[0006] Technical problem to be solved by the invention

[0007] When the content of rare earth elements in the dielectric layer increases, oxygen defects are easily generated in the dielectric layer. When a voltage is applied between the internal electrodes when using a stacked ceramic capacitor, the oxygen defects generated in the dielectric layer will move from the inside of the dielectric layer to the internal electrode layer (negative electrode) and accumulate at the interface between the dielectric layer and the internal electrode layer. The oxygen defects accumulated at the interface between the dielectric layer and the internal electrode layer will increase the leakage current, thus becoming the cause of reducing the insulation reliability of the capacitor.

[0008] The purpose of the invention described in this specification is to solve or alleviate at least part of the above-mentioned problems. One of the more specific purposes of the invention described in this specification is to improve the insulation reliability of a laminated ceramic capacitor. One of the more specific purposes of the invention described in this specification is to suppress the accumulation of oxygen defects at the interface between the dielectric layer and the internal electrode layer by suppressing the movement of oxygen defects generated in the dielectric layer, thereby improving the insulation reliability of the laminated ceramic capacitor.

[0009] The purposes of the present invention other than those mentioned above will become clear through the description of the entire specification. The invention described in this specification can also solve technical problems that can be grasped from the contents other than those described in the "technical problems to be solved by the invention". When the effects of the embodiments are described in this specification, the technical problems of the invention corresponding to the embodiments can be grasped from the effects.

[0010] Means for solving technical problems

[0011] The various inventions described in this specification are sometimes collectively referred to as "the present invention". The main body of a laminated ceramic capacitor of one embodiment of the present invention has a first internal electrode layer, a second internal electrode layer and a ceramic layer. The ceramic layer is arranged between the first internal electrode layer and the second internal electrode layer and includes crystal grains of a ceramic material. The crystal grains have a core and a shell covering the core. The shell includes one or more pores in the shell.

[0012] Effects of the Invention

[0013] According to one embodiment of the invention described in this specification, the insulation reliability of a multilayer ceramic capacitor can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 FIG. 1 is a perspective view schematically showing a multilayer ceramic capacitor according to an embodiment of the present invention.

[0015] Figure 2 It is a schematic representation of Figure 1 A cross-sectional view of a cross section of a capacitor cut along line II.

[0016] Figure 3 Yes Figure 2 An enlarged cross-sectional view showing an enlarged portion (region A) of the cross section.

[0017] Figure 4 It is schematically indicated Figure 1 A cross-sectional view of a cross section of a crystal grain contained in a dielectric layer of a capacitor.

[0018] Figure 5 This is a flowchart showing the flow of a method for manufacturing a multilayer ceramic capacitor according to one embodiment of the present invention.

[0019] Figure 6 It means that it is made in Figure 5 FIG. 1 is a flow chart showing the flow of steps of producing composite ceramic particles used in the method for producing the composite ceramic particles.

[0020] Figure 7a It is a schematic diagram explaining the production process of composite ceramic particles.

[0021] Figure 7b It is a schematic diagram explaining the production process of composite ceramic particles.

[0022] Figure 7c It is a schematic diagram explaining the production process of composite ceramic particles.

[0023] Figure 7dIt is a schematic diagram explaining the production process of composite ceramic particles.

[0024] Description of Reference Numerals

[0025] 1 stacked ceramic capacitor, 10 body, 11 ceramic layer, 21 first internal electrode layer, 22 second internal electrode layer, 31 first external electrode, 32 second external electrode, 40 crystal grains, 41 core, 42 shell, 43 pores in shell, 51 first ceramic particles, 52 second ceramic particles, 52a pores, 60 composite ceramic particles. DETAILED DESCRIPTION

[0026] Below, various embodiments of the present invention are described with appropriate reference to the drawings. For the same components in multiple drawings, the same or similar reference figure numbers are marked in the multiple drawings. It should be noted that, for the convenience of explanation, the drawings are not necessarily recorded in an accurate scale. The embodiments described below do not limit the technical solutions described in the claims. The elements described in the following embodiments are not necessarily necessary for the solution of the present invention.

[0027] In the drawings, for convenience of explanation, mutually orthogonal L, W, and T axes are sometimes described. In this specification, the size, arrangement, shape, and other features of each component of the multilayer ceramic capacitor 1 are sometimes described with reference to the L, W, and T axes.

[0028] 1Multilayer Ceramic Capacitor 1

[0029] 1-1 Basic Structure of Multilayer Ceramic Capacitors 1

[0030] Reference Figure 1 and Figure 2 , a basic structure of a multilayer ceramic capacitor 1 according to a first embodiment will be described. The multilayer ceramic capacitor 1 is an example of a capacitor described in the claims. Figure 1 It is a perspective view of the multilayer ceramic capacitor 1 according to the first embodiment. Figure 2 It is a cross-sectional view schematically showing a cross section of the multilayer ceramic capacitor 1 cut along line II.

[0031] The multilayer ceramic capacitor 1 includes a main body 10, and a first external electrode 31 and a second external electrode 32 provided on the main body 10. The first external electrode 31 and the second external electrode 32 are arranged with a gap therebetween. Figure 2 In the illustrated example, the first external electrode 31 is disposed at a distance from the second external electrode 32 in the L-axis direction.

[0032] The body 10 includes a plurality of ceramic layers 11, a plurality of first internal electrode layers 21, and a plurality of second internal electrode layers 22. The ceramic layer 11 is disposed between the first internal electrode layer 21 and the second internal electrode layer 22 adjacent to the first internal electrode layer 21. In this specification, when it is not necessary to distinguish the first internal electrode layer 21 and the second internal electrode layer 22 from each other, the first internal electrode layer 21 and the second internal electrode layer 22 are sometimes collectively referred to as "internal electrode layers".

[0033] The body 10 has an upper surface 10a, a lower surface 10b, a first end surface 10c, a second end surface 10d, a first side surface 10e, and a second side surface 10f. The outer surface of the body 10 is defined by the upper surface 10a, the lower surface 10b, the first end surface 10c, the second end surface 10d, the first side surface 10e, and the second side surface 10f.

[0034] The upper surface 10a and the lower surface 10b are respectively the surfaces at the two ends of the height direction (T-axis direction) of the main body 10. In other words, the upper surface 10a and the lower surface 10b are opposite in the T-axis direction. The first end surface 10c and the second end surface 10d are respectively the surfaces at the two ends of the length direction (L-axis direction) of the main body 10. In other words, the first end surface 10c and the second end surface 10d are opposite in the L-axis direction. The first side surface 10e and the second side surface 10f are respectively the surfaces at the two ends of the width direction (W-axis direction) of the main body 10. In other words, the first side surface 10e and the second side surface 10f are opposite in the W-axis direction. The upper surface 10a and the lower surface 10b are spaced apart by the height dimension of the main body 10, the first end surface 10c and the second end surface 10d are spaced apart by the length dimension of the main body 10, and the first side surface 10e and the second side surface 10f are spaced apart by the width dimension of the main body 10.

[0035] In one embodiment, the main body 10 may be configured to have a rectangular parallelepiped shape. In this specification, when referred to as a "rectangular parallelepiped" or a "rectangular parallelepiped shape", it does not only refer to a "rectangular parallelepiped" in a strict mathematical sense. As described later, the corners and / or sides of the main body 10 may also be curved. The size and shape of the main body 10 are not limited to those explicitly described in this specification.

[0036] The main body 10 is formed by stacking the ceramic layer 11, the first internal electrode layer 21, and the second internal electrode layer 22 along the stacking direction. In the illustrated embodiment, the ceramic layer 11, the first internal electrode layer 21, and the second internal electrode layer 22 are stacked along the T-axis direction. The stacking direction may be along the T-axis as shown in the figure, or along the L-axis or W-axis. The ceramic layers 11 disposed at both ends of the stacking direction are sometimes referred to as cover layers.

[0037] One end of the first internal electrode layer 21 is led out to the outside of the main body 10. The first internal electrode layer 21 is connected to the first external electrode 31 provided on the surface of the main body 10. One end of the second internal electrode layer 22 is led out to the outside of the main body 10. The second internal electrode layer 22 is connected to the second external electrode 32 provided on the surface of the main body 10. In the illustrated embodiment, the first internal electrode layer 21 is led out to the outside of the main body 10 from one end in the L-axis direction, and is connected to the first external electrode 31 at one end in the L-axis direction of the main body 10. The second internal electrode layer 22 is led out to the outside of the main body 10 from the other end in the L-axis direction, and is connected to the second external electrode 32 at the other end in the L-axis direction of the main body 10. Figure 2 In the example shown, the first internal electrode layer 21 and the second internal electrode layer 22 are led out at the first end face 10c and the second end face 10d facing each other, respectively. However, the first internal electrode layer 21 and the second internal electrode layer 22 may be led out from various surfaces of the main body 10 in accordance with the arrangement and shape of the first external electrode 31 and the second external electrode 32. For example, in the case where the first external electrode 31 and the second external electrode 32 are both arranged on the lower surface 10b, the first internal electrode layer 21 and the second internal electrode layer 22 are both led out from the lower surface. The first external electrode 31 and the second external electrode 32 may be provided on any surface of the main body 10 as long as they are spaced apart from each other.

[0038] When a voltage is applied between the first external electrode 31 and the second external electrode 32 , capacitance is generated between the first internal electrode layer 21 and the second internal electrode layer 22 .

[0039] exist Figure 2 In order to simplify the illustration, the first internal electrode layer 21 and the second internal electrode layer 22 are each shown as 5 layers, but the laminated ceramic capacitor 1 can be set to any number of layers. The laminated ceramic capacitor 1 can include, for example, 300 to 1000 layers of the first internal electrode layer 21 and the second internal electrode layer 22. In other words, the number of layers in the laminated ceramic capacitor 1 can be 300 to 1000 layers.

[0040] The laminated ceramic capacitor 1 can be mounted on an electronic circuit board. An electronic circuit board equipped with the laminated ceramic capacitor 1 is sometimes referred to as a circuit assembly. Various electronic components other than the laminated ceramic capacitor 1 can also be installed in the circuit assembly. The circuit assembly can be mounted in various electronic devices. Electronic devices that can be equipped with the circuit assembly include smartphones, tablet computers, game consoles, electrical components of automobiles, servers, and various electronic devices other than these.

[0041] In one embodiment, the dimension (length dimension) of the multilayer ceramic capacitor 1 in the L-axis direction is in the range of 0.2 mm to 4.5 mm, the dimension (width dimension) in the W-axis direction is in the range of 0.1 mm to 3.2 mm, and the dimension (height dimension) in the T-axis direction is in the range of 0.1 mm to 3.2 mm. In one embodiment, the length dimension of the multilayer ceramic capacitor 1 can be larger than the width dimension. In one embodiment, the height dimension of the multilayer ceramic capacitor 1 can be larger than the width dimension. In one embodiment, the width dimension of the multilayer ceramic capacitor 1 can be larger than the length dimension.

[0042] 1-2 Ceramic layer 11

[0043] 1-2-1 Composition of Ceramic Layer 11

[0044] The ceramic layer 11 contains an oxide of a ceramic material represented by the chemical formula ABO3 as a main component. The oxide may have a perovskite structure. Based on the total mass of the ceramic layer 11, a component containing 50 wt% or more in the ceramic layer 11 may be referred to as the main component of the ceramic layer 11. In the case where the oxide represented by the chemical formula ABO3 contains 50 wt% or more in the ceramic layer 11, it can be said that the ceramic layer 11 contains the oxide represented by the chemical formula ABO3 as a main component. The ceramic layer 11 preferably contains 60 wt% or more, 70 wt% or more, 80 wt% or more or 90 wt% or more of the oxide represented by the chemical formula ABO3. Oxygen defects may exist in the main component oxide of the ceramic layer 11. The oxygen defects may be generated at the A position of the main component oxide of the ceramic layer 11. When oxygen defects are generated at the A position of the main component oxide of the ceramic layer 11, the composition formula of the main component oxide of the ceramic layer 11 may be expressed as A α BO 3-β When the main component oxide of the ceramic layer 11 is expressed as a composition formula A α BO 3-β In the case of, for example, the range of values ​​that α can take is 0.98≤α≤1.01, and the range of values ​​that β can take is 0≤β≤0.05.

[0045] In the chemical formula ABO3, "A" is at least one element selected from Ba (barium), Sr (strontium), Ca (calcium) and Mg (magnesium). In the chemical formula ABO3, "B" is at least one element selected from Ti (titanium), Zr (zirconium) and Hf (hafnium). In the case where the oxide represented by the chemical formula ABO3 has a perovskite structure, the elements "A" and "B" are located at the A position and the B position of the perovskite structure, respectively. Examples of oxides contained as main components in the ceramic layer 11 include BaTiO3 (barium titanate), CaZrO3 (calcium zirconate), CaTiO3 (calcium titanate), SrTiO3 (strontium titanate) and MgTiO3 (magnesium titanate).

[0046] The oxide contained as a main component in the ceramic layer 11 may also be a compound having a chemical formula of Ba 1-x-y Ca x Sr y Ti 1-z Zr z An oxide represented by O3 (0≤x≤1, 0≤y≤1, 0≤z≤1). Examples of such oxides include barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, and barium calcium titanate zirconate.

[0047] The ceramic layer 11 may contain additive elements in addition to the oxide of the main component. In one embodiment, the additive element contained in the ceramic layer 11 is at least one element selected from Fe (iron), Ni (nickel), Mo (molybdenum), Nb (niobium), Ta (tantalum), W (tungsten), Mg (magnesium), Mn (manganese), V (vanadium) and Cr (chromium). The ceramic layer 11 may contain two or more of the above additive elements.

[0048] The ceramic layer 11 may contain an oxide of a rare earth element in addition to the oxide of the main component. The oxide of the rare earth element contained in the ceramic layer 11 may be an oxide of at least one rare earth element selected from the group consisting of Y (yttrium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium) and Yb (ytterbium). The ceramic layer 11 may contain oxides of two or more rare earth elements.

[0049] The ceramic layer 11 may also contain other types of oxides. For example, the ceramic layer 11 may contain an oxide of at least one element selected from Co (cobalt), Ni (nickel), Li (lithium), B (boron), Na (sodium), K (potassium) and Si (silicon). The ceramic layer 11 may also contain oxides of two or more of these elements.

[0050] The ceramic layer 11 may contain glass containing at least one element selected from the group consisting of Co, Ni, Li, B, Na, K, and Si.

[0051] In one embodiment, the film thickness (dimension in the T-axis direction) of the ceramic layer 11 is 0.2 to 10 μm.

[0052] 1-2-2 Grain

[0053] The ceramic layer 11 comprises a plurality of ceramic material grains. At least a portion of the plurality of grains has a core-shell structure. Figure 3 and Figure 4 , the crystal grains included in the ceramic layer 11 are described. Figure 3 Yes Figure 2 An enlarged cross-sectional view showing an area A of a cross section of the body 10 is shown enlarged, Figure 4 The cross section of one crystal grain is schematically shown. The region A extends from the first internal electrode layer 21 to the second internal electrode layer 22 through the ceramic layer 11 .

[0054] like Figure 3 As shown, the ceramic layer 11 includes a plurality of crystal grains 40. Adjacent crystal grains 40 are separated from each other by grain boundaries 45. That is, the ceramic layer 11 is a polycrystalline body including a plurality of crystal grains 40, and has a plurality of crystal grains 40 in which atoms are regularly arranged and grain boundaries 45 between adjacent crystal grains in the plurality of crystal grains 40.

[0055] like Figure 3 and Figure 4 As shown, the crystal grain 40 has a core-shell structure. Specifically, the crystal grain 40 having the core-shell structure includes a core portion 41 and a shell portion 42 covering the core portion 41. The crystal grain 40 is, for example, a crystal of barium titanate. The element added to the ceramic layer 11 is more solid-dissolved in the shell portion 42 than in the core portion 41. For example, when rare earth elements are added to the ceramic layer 11, the concentration of the rare earth elements in the shell portion 42 is higher than the concentration of the rare earth elements in the core portion 41. By making the shell portion 42 contain rare earth elements, the electrostatic capacitance and high-temperature load life of the stacked ceramic capacitor 1 can be improved.

[0056] It is possible to confirm that the grain 40 has a core 41 and a shell 42 in the following manner. First, a thin-sliced ​​analysis sample with a thickness of about 30 to 80 nm is taken out from the multilayer ceramic capacitor 1 using a focused ion beam device (FIB). The analysis sample is placed in a scanning transmission electron microscope (STEM) equipped with an energy dispersive X-ray spectrometer (EDS: Energy Dispersive X-ray Spectroscopy) or a wavelength dispersive X-ray spectrometer (WDS: Wavelength-Dispersive X-ray Spectroscopy) to obtain a high-angle annular dark-field scanning transmission electron microscopy image (HAADF-STEM image: high-angle annular dark-field scanning transmission electron microscopy image). In the HAADF-STEM image, the dark-looking area can be determined as the core 41, and the area surrounding the core 41 and appearing brighter than the core 41 can be determined as the shell 42. In this way, the core portion 41 and the shell portion 42 can be identified using the HAADF-STEM method.

[0057] The core 41 and the shell 42 can also be identified by methods other than the HAADF-STEM method. For example, a concentration map of elements contained in an analysis sample taken out from the multilayer ceramic capacitor 1 can be obtained, and the core 41 and the shell 42 can be identified based on the concentration map. As a specific example, a thin-film sample taken out from the multilayer ceramic capacitor 1 using FIB is set in a STEM equipped with EDS, and observed at a magnification of 10,000 to 150,000 times to obtain a concentration map of quantitative elements in the observation area. At this time, the added elements added to the ceramic layer 11 can be used as quantitative elements. For example, rare earth elements added to the ceramic layer 11 can be used as quantitative elements. Because the concentration of the added elements (such as rare earth elements) in the ceramic layer 11 is higher in the shell 42 than in the core 41, in the concentration map obtained using EDS, the area with a high concentration of the added elements can be determined as the shell 42.

[0058] As described above, the main component oxide of the ceramic layer 11 may have oxygen defects. When a voltage is applied between the first internal electrode layer 21 and the second internal electrode layer 22, the oxygen defects generated in the ceramic layer 11 move from the inside of the ceramic layer 11 to the first internal electrode layer 21 or the second internal electrode layer 22, which becomes the negative electrode, and accumulate at the interface between the ceramic layer 11 and the first internal electrode layer 21 or the second internal electrode layer 22. The oxygen defects accumulated at the interface between the ceramic layer 11 and the first internal electrode layer 21 or the second internal electrode layer 22 increase the leakage current, thereby causing a decrease in the insulation reliability of the multilayer ceramic capacitor 1. Therefore, even if oxygen defects are generated in the ceramic layer 11, if the movement of the oxygen defects to the first internal electrode layer 21 or the second internal electrode layer 22 is prevented, the insulation reliability of the multilayer ceramic capacitor 1 can be improved.

[0059] As described above, the concentration of the additive element in the crystal grain 40 is higher in the shell portion 42 than in the core portion 41. Therefore, by suppressing the movement of oxygen defects in the shell portion 42, the insulation reliability of the multilayer ceramic capacitor 1 can be effectively improved.

[0060] In one embodiment, the shell portion 42 of each crystal grain 40 has one or more intra-shell pores 43. The intra-shell pores 43 are voids contained in the shell portion 42. The oxygen defects generated in the ceramic layer 11 cannot move in the voids, and therefore, the movement of the oxygen defects can be hindered by the intra-shell pores 43. The intra-shell pores 43 are contained in the shell portion 42, and therefore, the movement of the oxygen defects can be hindered in the shell portion 42. When the content of the added element (such as a rare earth element) in the ceramic layer 11 increases, oxygen defects are easily generated in the shell portion 42. By providing the intra-shell pores 43 in the shell portion 42, the movement of the oxygen defects generated in the shell portion 42 can be hindered.

[0061] Conventionally, there is no technology for selectively introducing voids inside a crystal grain, especially in the shell portion 42. In the invention disclosed in this application, by introducing the intra-shell voids 43 inside the crystal grain 40, more specifically inside the shell portion 42, the movement of oxygen defects in the shell portion 42 can be effectively hindered.

[0062] The average value of the diameter of the pores 43 in the shell is a sufficient size to hinder the movement of oxygen defects, specifically, it is greater than 1 nm. It can be considered that when the diameter of the pores 43 in the shell is larger than the lattice constant of the ceramic particles of the ceramic layer 11, the pores 43 in the shell can be used to hinder the movement of oxygen defects. The lattice constant of the ceramic particles contained in the ceramic layer 11 is less than 1 nm, so the lower limit of the diameter of the pores 43 in the shell can be set to 1 nm. For example, the lattice constant of barium titanate is 0.399 nm in a-axis length and 0.404 nm in c-axis length. Therefore, by setting the lower limit of the diameter of the pores 43 in the shell to 1 nm, the pores 43 in the shell can be used to hinder the movement of oxygen defects generated in the ceramic layer 11.

[0063] When the diameter of the pores 43 in the shell is too large, moisture easily enters the pores 43 in the shell during the manufacture and use of the multilayer ceramic capacitor 1, which may become a major factor that deteriorates the moisture resistance of the multilayer ceramic capacitor 1. Therefore, in order to ensure the moisture resistance of the multilayer ceramic capacitor 1, it is preferable to set an upper limit on the average value of the diameter of the pores 43 in the shell. In one embodiment, the average value of the diameter of the pores 43 in the shell is 25 nm or less.

[0064] In one embodiment, the average diameter of the one or more pores 43 in the shell may be 1 nm to 25 nm.

[0065] In addition to the average value of the diameter of the pores 43 in the shell, the area ratio of the pores 43 in the shell 42 also affects the moisture resistance of the multilayer ceramic capacitor 1. When the area ratio of the pores 43 in the shell 42 is too large, moisture easily enters the pores 43 in the shell during the manufacture and use of the multilayer ceramic capacitor 1. Therefore, in order to ensure the moisture resistance of the multilayer ceramic capacitor 1, it is preferred to set an upper limit on the area ratio of the pores 43 in the shell 42. In one embodiment, the area ratio of the pores 43 in the shell 42 is 22% or less. In order to ensure the moisture resistance of the multilayer ceramic capacitor 1, it is more preferred that the area ratio of the pores 43 in the shell is 19% or less.

[0066] The presence of the shell pores 43 in the shell portion 42 can be confirmed as follows. First, a thin-film analysis sample with a thickness of less than 50 nm is taken out from the multilayer ceramic capacitor 1 using a focused ion beam device (FIB). The thickness of the analysis sample can be, for example, 10 nm to 50 nm. Next, the analysis sample is placed in a transmission electron microscope (TEM) and a TEM image of the observation surface of the thin-film sample is obtained. The shell pores 43 appear bright in the TEM image, so the shell pores 43 can be determined by binarizing the TEM image. In addition, the length of the diameter of the shell pores 43 can be measured in the binarized TEM image. In the case where the cross-section of the shell pores 43 is not circular, the diameter of a circle with the same area as the cross-section is taken as the diameter of the pore (Heywood diameter). When obtaining the TEM image, the acceleration voltage can be set to 200 kV.

[0067] The area ratio of the intra-shell pores 43 in the shell portion 42 can be expressed by obtaining a TEM image of the observation surface of a thin-film analysis sample with a thickness of less than 50 nm taken out from the multilayer ceramic capacitor 1, and the ratio of the total area of ​​the intra-shell pores 43 contained in the observation area to the total area of ​​the shell portion 42.

[0068] 1-3 First Internal Electrode Layer 21 and Second Internal Electrode Layer 22

[0069] In one embodiment, the first internal electrode layer 21 contains a base metal such as Ni (nickel), Cu (copper), Sn (tin) as a main component. Based on the total mass of the first internal electrode layer 21, a component contained in the first internal electrode layer 21 by 50 wt% or more can be referred to as a main component of the first internal electrode layer 21. The first internal electrode layer 21 preferably contains a base metal as a main component by 60 wt% or more, 70 wt% or more, 80 wt% or more, or 90 wt% or more.

[0070] The first internal electrode layer 21 may contain a secondary element in addition to a main component metal element. The secondary element that may be contained in the first internal electrode layer 21 is, for example, one element or two or more elements selected from the group consisting of As (arsenic), Au (gold), Co, Cr, Cu, Fe, In (indium), Ir (iridium), Mg, Os (osmium), Pd (palladium), Pt (platinum), Re (rhenium), Rh (rhodium), Ru (ruthenium), Se (selenium), Sn, Ge (germanium), Te (tellurium), W, Y (yttrium), Zn (zinc), Ag (silver), and Mo. The main component metal element and the secondary element are different elements. For example, when the main component metal element is Ni, Sn can be used as a secondary element, but when the main component metal element is Sn, Sn cannot be selected as a secondary element.

[0071] In one embodiment, the internal electrode layer may contain 0.01 at % to 5 at % of the accessory element. When the internal electrode layer contains two or more elements as accessory elements, the total concentration of the two or more accessory elements is 0.01 at % to 5 at %.

[0072] The description about the composition of the first internal electrode layer 21 also applies to the composition of the second internal electrode layer 22 .

[0073] In one embodiment, the thickness of the first internal electrode layer 21 (dimension in the T-axis direction) is 0.1 μm or more and 2 μm or less. In one embodiment, the thickness of the first internal electrode layer 21 is preferably 0.4 μm or less. The description of the thickness of the first internal electrode layer 21 also applies to the second internal electrode layer 22.

[0074] 1-4 First external electrode 31 and second external electrode 32

[0075] In one embodiment, the first external electrode 31 and the second external electrode 32 can be formed by applying a conductive paste to the main body 10 and heating the conductive paste. The conductive paste can contain at least one substance selected from Ag, Pd, Au, Pt, Ni, Sn, Cu, W, Ti, and alloys thereof.

[0076] 2. Method for manufacturing multilayer ceramic capacitor 1

[0077] 2-1 Overview of Method for Manufacturing Multilayer Ceramic Capacitor 1

[0078] Next, refer to Figure 5 and Figure 6 Flowchart and Figure 7a to Figure 7d , an example of a method for manufacturing the multilayer ceramic capacitor 1 will be described. Figure 5 1 is a flowchart showing the flow of a method for manufacturing the multilayer ceramic capacitor 1 according to one embodiment of the present invention. Figure 6 It is used for Figure 5 The flowchart shows the step of preparing the composite ceramic particles in the production method in more detail.

[0079] Reference Figure 5 The method for manufacturing the laminated ceramic capacitor 1 is briefly described. First, in step S1, composite ceramic particles are prepared in which second ceramic particles with a small diameter are bonded to the surface of first ceramic particles with a large diameter. The method for manufacturing the composite ceramic particles will be described in detail later.

[0080] Next, in step S2, the composite ceramic particles are used to form a sheet laminate as a precursor of the body 10. The sheet laminate includes: a ceramic green sheet as a precursor of the ceramic layer 11; and an internal conductor pattern as a precursor of each of the first internal electrode layer 21 and the second internal electrode layer 22. The sheet laminate can also be formed by alternately laminating a ceramic green sheet having an internal conductor pattern as a precursor of the first internal electrode layer 21 provided on the surface, and a ceramic green sheet having an internal conductor pattern as a precursor of the second internal electrode layer 22 provided on the surface.

[0081] Ceramic green sheets can be produced by adding a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer to the composite ceramic particles 60 and wet mixing them to form a slurry, applying the slurry on a substrate film by, for example, a die coating method or a doctor blade method, and drying the slurry applied on the substrate film to produce ceramic green sheets.

[0082] Next, internal electrode patterns are formed on the plurality of ceramic green sheets formed as described above. The internal electrode pattern can be formed, for example, by printing an internal electrode paste on the ceramic green sheets using a known printing method such as screen printing. In the case of forming the internal electrode pattern by screen printing, the internal electrode paste can be manufactured by kneading metal powder, binder resin and solvent using a three-roll mill. That is, the internal electrode paste is obtained by dispersing metal powder in a binder resin. The metal powder contained in the internal electrode paste includes powders of main component metal elements such as Ni, Cu, Sn, etc., which are the main components of the first internal electrode layer 21 and the second internal electrode layer 22. As an organic binder for the internal electrode paste, a cellulose resin such as ethyl cellulose and an acrylic resin such as butyl methacrylate can be used. The internal electrode pattern formed on a part of the ceramic green sheets is a precursor of the first internal electrode layer 21, and the internal electrode pattern formed on the other ceramic green sheets is a precursor of the second internal electrode layer 22. The internal electrode pattern can also be formed on the ceramic green sheets by sputtering.

[0083] As described above, a stacking unit having a ceramic green sheet and an internal electrode pattern formed on the surface of the ceramic green sheet is obtained. A sheet stack can be obtained by stacking a predetermined number of the stacking units and performing thermocompression bonding. Green sheets without internal electrode patterns can be stacked on the top and bottom layers of the sheet stack.

[0084] Next, by singulating the sheet laminate formed as described above, a sheet-shaped laminate that becomes a precursor of the main body 10 can be obtained. The sheet-shaped laminate can be degreased. The degreasing process can be performed in a nitrogen atmosphere. In addition, the metal paste that becomes the base electrode layer of the first external electrode 31 and the second external electrode 32 can be applied to the degreased laminate by dip coating.

[0085] Next, in step S3, the unit cell laminate produced in step S2 is placed in a firing furnace, and the laminate is fired in the firing furnace, so that the unit cell laminate is fired to obtain a laminated ceramic capacitor 1. In this firing process, the ceramic green sheets in the unit cell laminate are fired to form ceramic layers 11, and the internal electrode patterns are fired to form internal electrode layers (first internal electrode layer 21 and second internal electrode layer 22).

[0086] In order to manufacture the multilayer ceramic capacitor 1, it is also possible to perform Figure 5 For example, the laminated body subjected to the firing treatment in step S3 may be subjected to a reoxidation treatment at 600°C to 1000°C in a nitrogen atmosphere. In addition, a plating layer of Cu, Ni, Sn, etc. may be provided on the surface of the first external electrode 31 and the second external electrode 32. The plating layer may be formed by an electrolytic plating method or an electroless plating method.

[0087] 2-2 Production process of composite ceramic particles

[0088] Next, refer to Figure 6 and Figure 7a to Figure 7d , the step S1 of making composite ceramic particles is described in more detail. The composite ceramic particles are composite particles containing first ceramic particles and second ceramic particles. In the following description, it is assumed that the first ceramic particles and the second ceramic particles are both barium titanate (BaTiO3) particles.

[0089] exist Figure 6 In the process of preparing the mixed ceramic powder shown in FIG. 1 , first, in step S11, a first ceramic particle 51 having a large diameter is prepared. An example of the first ceramic particle 51 is as follows: Figure 7a As shown. The first ceramic particles 51 can be formed by any known synthesis method such as a solid phase synthesis method, a sol-gel synthesis method, a hydrothermal synthesis method, etc. In the case of using a solid phase synthesis method, the first ceramic particles 51 can be formed by mixing a titanium raw material such as titanium dioxide and a barium raw material such as barium carbonate, and subjecting the titanium raw material and the barium raw material to a solid phase reaction. The average particle size of the first ceramic particles 51 is, for example, not less than 50 nm and not more than 150 nm. As described later, the core 41 of the crystal grain 40 is mainly formed by the first ceramic particles 51. In order to suppress the degradation of the dielectric properties, the first ceramic particles 51 preferably do not contain pores. The first ceramic particles 51 are preferably made by a solid phase synthesis method rather than a hydrothermal synthesis method that is prone to produce pores. The first ceramic particles 51 may contain additive elements contained in the ceramic layer 11 (for example, one or more of the above-mentioned metal elements such as Fe, rare earth elements, and additive elements other than these).

[0090] Next, in step S12, second ceramic particles 52 having a diameter smaller than that of the first ceramic particles 51 are produced. The second ceramic particles 52 can be produced by a hydrothermal synthesis method. The second ceramic particles 52 can be formed, for example, by hydrothermally treating titanium hydroxide and barium hydroxide. Figure 7b As shown, the second ceramic particle 52 has a pore 52a. The second ceramic particle 52 may have one pore 52a or a plurality of pores 52a. By synthesizing the raw material to form the second ceramic particle 52 using a hydrothermal synthesis method, it is easy to generate pores 52a in the second ceramic particle 52. The method for synthesizing the second ceramic particle 52 is not limited to the hydrothermal synthesis method. The average particle size of the second ceramic particle 52 is, for example, not less than 5nm and not more than 50nm. The pore 52a becomes the shell pore 43 contained in the main body 10 in the laminated ceramic capacitor 1 as a finished product. In the firing step S3, there is a situation where the diameter of the shell pore 43 becomes smaller than the diameter of the pore 52a due to the crystal growth of barium titanate. Therefore, by controlling the firing conditions in the firing step S3, the diameter of the shell pore 43 can be controlled. Specifically, by increasing the firing temperature or extending the firing time to promote the growth of barium titanate crystals, the diameter of the shell pore 43 can be reduced. In one embodiment, the diameter of the pore 52 a is 1 to 30 nm. The diameter of the pore 52 a may be 20 to 80% of the diameter of the second ceramic particle 52 .

[0091] The second ceramic particles 52 may contain the additive elements contained in the ceramic layer 11 (for example, the above-mentioned metal elements such as Fe, rare earth elements, and one or more additive elements other than these).

[0092] Next, in step S13, the powder of the first ceramic particles 51, the powder of the second ceramic particles 52, and the additive powder 53 are dispersed in the dispersion solution to prepare a colloidal solution. Figure 7c and Figure 7d In the figure, the additive powder 53 is represented by a figure other than a circle to make it easy to distinguish from the second ceramic particles 52, but it can also be spherical particles. As a dispersion solution, for example, water or ethanol solvent can be used. The additive powder 53 is a powder containing additive elements added to the ceramic layer 11. As described above, the ceramic layer 11 can contain metal elements such as Fe, rare earth elements such as Ho, and additive elements other than these. The additive powder 53 is a powder of the additive elements contained in the ceramic layer 11. A pH adjuster can be added to the colloidal solution as needed.

[0093] One or both of the first ceramic particles 51 and the second ceramic particles 52 may be surface-modified so that the zeta potential of the first ceramic particles 51 and the zeta potential of the second ceramic particles 52 have opposite polarities in the dispersed solution. The pH of the dispersed solution is adjusted to a specified range. The first ceramic particles 51 and / or the second ceramic particles 52 may be surface-modified so that in a dispersed solution having a pH in a specified range, the zeta potential of the first ceramic particles 51 and the zeta potential of the second ceramic particles 52 have opposite polarities. In the dispersed solution, the first ceramic particles 51 having zeta potentials of the same polarity electrostatically repel each other, and the second ceramic particles 52 having zeta potentials of the same polarity also electrostatically repel each other. Therefore, the coagulation of the first ceramic particles 51 and the coagulation of the second ceramic particles 52 in the dispersed solution can be suppressed. The surface modification of the first ceramic particles 51 may be performed, for example, by adsorbing an organic substance such as a surfactant on the surface of the first ceramic particles 51. Similarly, the surface modification of the second ceramic particles 52 can be performed by, for example, allowing an organic substance such as a surfactant to be adsorbed on the surface of the second ceramic particles 52 .

[0094] Next, in step S14, the colloidal solution obtained in step S13 is stirred in a mixing container to heterogeneously aggregate the first ceramic particles 51, the second ceramic particles 52, and the additive powder 53 to form composite ceramic particles 60. Figure 7d As shown, the composite ceramic particle 60 has a first ceramic particle 51, a second ceramic particle 52 adsorbed on the surface of the first ceramic particle 51, and an additive powder 53 similarly adsorbed on the surface of the first ceramic particle 51. The first ceramic particle 51 and the second ceramic particle 52 have zeta potentials of different polarities and are therefore electrostatically attracted to each other. In addition, van der Waals force (intermolecular force) also acts between the first ceramic particle 51 and the second ceramic particle 52. By utilizing the electrostatic attraction and van der Waals force acting between the first ceramic particle 51 and the second ceramic particle 52, the second ceramic particle 52 can be adsorbed on the surface of the first ceramic particle 51. Van der Waals force also acts between the first ceramic particle 51 and the additive powder 53, and therefore, the additive powder 53 is also adsorbed on the surface of the first ceramic particle 51. Figure 7d In the figure, the additive powder 53 is represented by a figure other than a circle so as to distinguish the additive powder 53 from the second ceramic particles 52, but the additive powder 53 may also be a spherical particle. Figure 7d In order to illustrate the addition of the additive powder 53, the additive powder 53 is prominently shown. Figure 7d Compared with the case shown, the ratio of the second ceramic particles 52 is greater than the ratio of the additive powder 53 .

[0095] The colloid solution containing the composite ceramic particles 60 obtained as described above is filtered to separate the composite ceramic particles 60 from the dispersion solution. Then, the separated composite ceramic particles 60 are washed with water and dried to prepare a powder of the composite ceramic particles 60.

[0096] By using the composite ceramic particles 60 prepared as described above, Figure 5 The multilayer ceramic capacitor 1 is manufactured by the process of S3, and in the firing process of step S3, the barium titanate contained in the first ceramic particles 51 and the second ceramic particles 52 is densified to form the core 41. In addition, in this firing process, the additional elements contained in the additive powder 53 are dissolved in the densified barium titanate to form the shell 42 containing a large amount of the additional elements. The additional elements contained in the shell 42 can also be derived from the additional elements contained in the first ceramic particles 51 and / or the second ceramic particles 52.

[0097] Furthermore, during the firing process, the pores 52a included in the second ceramic particles 52 become the shell pores 43 in the shell portion 42. The diameter of the shell pores 43 becomes smaller than the diameter of the pores 52a due to the densification of the barium titanate included in the second ceramic particles 52. However, when the barium titanate is densified, in the case where two or more pores 52a included in the second ceramic particles 52 are connected to form one shell pore 43, the diameter of the shell pore 43 formed by connecting the two or more pores 52a may become larger than the diameter of each of the two or more connected pores 52a.

[0098] As described above, the laminated ceramic capacitor 1 can be manufactured in such a manner that the shell portion 42 of the crystal grain 40 included in the ceramic layer 11 includes the intra-shell pores 43 .

[0099] 3. Embodiment

[0100] The present invention will be further described in detail below based on examples. The present invention is not limited to the following examples.

[0101] according to Figure 5 and Figure 6 Samples of the multilayer ceramic capacitor 1 were manufactured according to the manufacturing method described in , and the manufactured samples were subjected to a test for examining insulation reliability and moisture resistance.

[0102] 3-1 Preparation of samples

[0103] 3-1-1 Preparation of Sample 1

[0104] First, composite ceramic particles 60 are prepared according to step S1. Specifically, according to step S11, barium titanate particles (first ceramic particles 51) having an average particle size of 100 nm are prepared by synthesizing titanium dioxide and barium carbonate using a solid phase synthesis method. Next, according to step S12, barium titanate particles (second ceramic particles 52) having an average particle size of 5 nm are prepared by hydrothermally treating titanium hydroxide and barium hydroxide. Next, the first ceramic particles 51 are weighed so that the second ceramic particles 52 are 2 wt % and the additive powder 53 containing Ho is 2 % when the first ceramic particles 51 are 100 wt %, and the weighed powders of the first ceramic particles 51, the second ceramic particles 52 and the additive powder 53 are added to a mixed solution to prepare a colloidal solution. As the mixed solution, a solution obtained by adding 150 ml of water is used. The colloidal solution is stirred for a sufficient time to allow the first ceramic particles 51, the second ceramic particles 52 and the additive powder to undergo heterogeneous agglomeration. Next, the colloidal solution is filtered to separate the composite ceramic particles 60 from the dispersed solution, and the separated composite ceramic particles 60 are washed with water. The washed composite ceramic particles 60 are dried to prepare a powder of the composite ceramic particles 60 .

[0105] Next, a stack is formed according to step S2. Specifically, polyvinyl butyral (PVB) resin, toluene and a plasticizer are added to the above-mentioned composite ceramic particles 60 and wet-mixed to form a slurry, which is applied to a substrate film using a doctor blade method, and the slurry applied to the substrate film is dried to produce a ceramic green sheet. Next, an internal electrode slurry is printed on a portion of the surface of the ceramic green sheet formed as described above to form an internal electrode pattern on each ceramic green sheet. The stacking unit has a ceramic green sheet and an internal electrode pattern formed on the surface of the ceramic green sheet. Next, 250 stacking units are stacked to form a sheet stack, and the stack is monolithicized to obtain a unit sheet stack. The unit sheet stack is in the shape of 0603 (length dimension: 0.6 mm, width dimension: 0.3 mm, height dimension: 0.3 mm). Next, the unit sheet stack is degreased in an N2 atmosphere. Next, a metal paste is applied to the degreased laminated body by a dip coating method, thereby forming a base layer of an external electrode on each die laminated body.

[0106] Next, the die stack obtained as described above is placed in a firing furnace and fired under predetermined firing conditions according to a predetermined temperature profile. Specifically, the die stack is fired at an oxygen partial pressure of 7.8×10 -8Atm low oxygen atmosphere, the unit chip stack is fired according to a temperature distribution diagram in which the temperature in the firing furnace is increased from room temperature to 600°C at a heating rate of 300°C / h, from 600°C to 1300°C at a heating rate of 30000°C / h, and cooling begins immediately after reaching 1300°C.

[0107] The firing process yielded a laminated ceramic capacitor of sample 1 shown in Table 1 below. In this laminated ceramic capacitor, the ceramic green sheet was fired to form a dielectric layer, and the internal electrode pattern was fired to form an internal electrode layer. In addition, the base layer formed on the laminated body became an external electrode.

[0108] 3-1-2 Preparation of Samples 2 to 4

[0109] According to step S11, barium titanate particles having an average particle size of 100 nm, which are the same as those used in the preparation of sample 1, are prepared as first ceramic particles 51. Furthermore, according to step S12, barium titanate particles, which are the same as those used in the preparation of sample 1, are prepared as second ceramic particles 52. The first ceramic particles 51 and the second ceramic particles 52 are weighed in the proportions described in the rows of samples 2 to 4 in Table 1, respectively, and three types of composite ceramic particles 60 are prepared using the weighed first ceramic particles 51 and second ceramic particles 52. Using these three types of composite ceramic particles 60, a laminate is formed by the same process as sample 1, and the laminate is fired to prepare samples 2 to 4.

[0110] 3-1-3 Preparation of Samples 5 to 6

[0111] According to step S11, barium titanate particles having an average particle size of 100 nm, which are the same as the barium titanate particles used in the preparation of sample 1, are prepared as first ceramic particles 51. Furthermore, according to step S12, barium titanate particles having an average particle size of 20 nm are prepared as second ceramic particles 52 by hydrothermally treating titanium hydroxide and barium hydroxide. The first ceramic particles 51 and the second ceramic particles 52 are weighed in the proportions described in the rows of samples 5 to 6 in Table 1, respectively, and two types of composite ceramic particles 60 are prepared using the weighed first ceramic particles 51 and second ceramic particles 52. Using these two types of composite ceramic particles 60, a laminate is formed by the same process as sample 1, and the laminate is fired to prepare samples 5 to 6.

[0112] 3-1-4 Preparation of Samples 7 to 9

[0113] According to step S11, barium titanate particles having an average particle size of 100 nm, which are the same as the barium titanate particles used in the preparation of sample 1, are prepared as first ceramic particles 51. Furthermore, according to step S12, barium titanate particles having an average particle size of 50 nm are prepared as second ceramic particles 52 by hydrothermally treating titanium hydroxide and barium hydroxide. The first ceramic particles 51 and the second ceramic particles 52 are weighed in the proportions described in the rows of samples 7 to 9 in Table 1, respectively, and three types of composite ceramic particles 60 are prepared using the weighed first ceramic particles 51 and second ceramic particles 52. Using these three types of composite ceramic particles 60, a laminate is formed by the same process as sample 1, and the laminate is fired to prepare samples 7 to 9.

[0114] 3-1-5 Preparation of Sample 10 (Comparative Example)

[0115] According to step S11, barium titanate particles having an average particle size of 100 nm were prepared, which were the same as those used in the preparation of sample 1. The barium titanate particles were used to form a laminated body by the same process as sample 1, and the laminated body was fired to prepare sample 10. That is, sample 10 was prepared without using the second ceramic particles 52 prepared by the hydrothermal synthesis method.

[0116] 3-2 Thickness of ceramic layer and internal electrode layer

[0117] The thickness of the dielectric layer and the internal electrode layer included in the sample 1 prepared as described above was confirmed as follows. First, the sample 1 was embedded in a resin, and each sample embedded in the resin was measured along a plane parallel to the stacking direction (e.g. Figure 2The LT surface in the sample is polished to expose the cross section parallel to the stacking direction. Next, a field emission scanning secondary electron microscope (FE-SEM) is used to determine an observation area at a magnification of 5000 to 20000 times in the exposed cross section of each sample, and the cross section of each sample is observed in the observation area. In the observation area, the dimensions of the 10 layers of the ceramic layer 11 and the internal electrode layers 21 and 22 in the T-axis direction are focused on, and the average value of the dimensions of the 10 layers of the ceramic layer 11 in the T-axis direction can be used as the thickness of the ceramic layer 11. Similarly, the dimensions of the internal electrode layers 21 and 22 in the T-axis direction of the total of 10 layers are measured, and the average value of the dimensions of the 10 layers of the first internal electrode layer 21 and the second internal electrode layer 22 in the T-axis direction can be used as the thickness of the first internal electrode layer 21 and the second internal electrode layer 22, respectively. The average values ​​of the thicknesses of the ceramic layer 11, the first internal electrode layer 21, and the second internal electrode layer 22 obtained in this way are all approximately 0.5 μm. For Samples 2 to 10, the thicknesses of the ceramic layer 11 and the internal electrode layers 21 and 22 were determined in the same manner as for Sample 1. As a result, in Samples 2 to 10, the average thicknesses of the ceramic layer 11, the first internal electrode layer 21, and the second internal electrode layer 22 were all approximately 0.5 μm.

[0118] 3-3 Confirmation of pores in the shell and measurement of pore diameter

[0119] From the laminated ceramic capacitor of sample 1, a thin-sliced ​​analysis sample with a thickness of less than 50 nm was taken out by FIB in such a way that the LT surface became the observation surface. Then, the thin-sliced ​​sample was set in a TEM (TEM JEM-ARM200F manufactured by JEOL Ltd.), and the core 41 and the shell 42 were identified by the HAADF-STEM method. Then, the shell 42 in the observation surface of the analysis sample in the TEM was observed at a magnification of 500,000 times to obtain a TEM image of the observation area. The accelerating voltage of the TEM during observation was 200 kV. The TEM image was binarized to obtain a binarized TEM image. In the binarized TEM image, the white-looking part in the shell 42 was determined to be the pore 43 in the shell. In addition, the diameter of each pore 43 in the shell was measured in the binarized TEM image, and the average value of the measured diameter was taken as the average pore diameter of the pore 43 in the shell in sample 1, and recorded in the "average pore diameter" column of Table 1.

[0120] For samples 2 to 9, the average value of the diameter of the pores 43 in the shell was also calculated using the same method, and the average pore diameters of each sample calculated are recorded in Table 1. For sample 10, the presence of pores in the shell could not be confirmed. In samples 1 to 9, the pores 43 in the shell 42 are derived from the pores contained in the second ceramic particles 52 mixed during the manufacturing process of each sample. When sample 10 was manufactured, the second ceramic particles 52 were not mixed, and therefore, in sample 10, there were no pores in the shell.

[0121] 3-4 Calculation of pore area ratio

[0122] For each of Samples 1 to 9, in the binarized TEM image used to find the average pore diameter, the total area of ​​the shell portion 42 and the total area of ​​the pores 43 in the shell included in the observation area were found, and the ratio of the total area of ​​the pores 43 in the shell to the total area of ​​the shell portion 42 was calculated, and the calculated area ratio was recorded in the column of "pore area ratio" in Table 1. In Sample 10, there were no pores in the shell, so the pore area ratio was not calculated for Sample 10.

[0123] 3-5 Accelerated life test

[0124] Next, 10 samples were selected for each of Samples 1 to 10, and an accelerated life test (HALT) was performed on each of the selected samples. In the accelerated life test, the life of each of the selected 10 samples was calculated when a voltage of 15V / μm was applied at 120°C, and the average failure time was calculated by averaging the lifespans obtained for the 10 samples. The average failure time of each sample calculated in this way is recorded in the "Lifetime" column of Table 1.

[0125] 3-6 Moisture resistance load test

[0126] A moisture resistance load test was performed on each sample 1 to sample 10. Specifically, 1000 samples were selected for each sample 1 to sample 10, and after the moisture resistance load test was performed under the conditions of test temperature = 85°C, relative humidity = 85% RH, applied voltage = 10Vdc (direct current), and time = 1000h, the samples were immediately taken out from the moisture resistance tank, and the resistance value of each sample was measured when it returned to room temperature. Samples with a resistance value less than 25MΩ were judged to be poor in moisture resistance, and their defective rate was investigated. The defective rate of the moisture resistance load test obtained in this way is recorded in the "Moisture Resistance Test" column of Table 1. The result of the moisture resistance load test is that in samples 1 to sample 9, the defective rate is less than 0.50%, which is good. In samples 1 to sample 3 and samples 5 to sample 7, the defective rate is 0%, which has particularly excellent moisture resistance.

[0127] [Table 1]

[0128] Sample No. Average particle size of particles 52 Ratio of particles 52 Average pore diameter Pore ​​area ratio life Humidity resistance test 1 5nm 2% 3nm 5% 121min 0 / 1000 2 5nm 10% 4nm 9% 135min 0 / 1000 3 5nm 15% 5nm 15% 119min 0 / 1000 4 5nm 20% 3nm 22% 95min 5 / 1000 5 20nm 15% 12nm 13% 140min 0 / 1000 6 20nm 20% 15nm 19% 110min 0 / 1000 7 50nm 8% 20nm 8% 108min 0 / 1000 8 50nm 10% 23nm 10% 98min 4 / 1000 9 50nm 15% 25nm 16% 89min 7 / 1000 10(*) none none N / A N / A 45min 1 / 1000

[0129] In Table 1, an asterisk (*) is added to the sample number for samples not included in the present invention (ie, comparative examples). Specifically, sample 10 is a comparative example not included in the present invention.

[0130] Analysis of 3-7 Embodiments

[0131] According to the above results, samples 1 to 9 in which the shell portion 42 of the crystal grain 40 included in the ceramic layer 11 has the pores 43 in the shell have a life of about twice or more than that of sample 10 (comparative example) without the pores in the shell. Therefore, samples 1 to 9 have excellent insulation reliability. It is believed that the reason why samples 1 to 9 have excellent insulation reliability is that the pores 43 in the shell hinder the movement of oxygen defects generated in the shell portion 42, thereby suppressing the accumulation of oxygen defects at the interface between the dielectric layer and the internal electrode layer.

[0132] According to the results of the moisture resistance load test, when the average pore diameter is greater than 23nm, the defect rate begins to increase, and the defect rate (0.7%) of sample 9 with an average pore diameter of 25nm is worse than the defect rate (0.5%) of sample 8 with an average pore diameter of 23nm. The defect rate in the moisture resistance load test deteriorates when the average pore diameter becomes larger. It can be considered that the reason is that when the average pore diameter becomes larger, moisture easily enters the inside of the main body 10 from the outside of the main body 10 through the large-diameter shell pores 43. Therefore, in order to maintain the moisture resistance of the multilayer ceramic capacitor, it is preferred to set an upper limit for the average particle size of the shell pores 43. The upper limit of the shell pores 43 is preferably 25nm. The upper limit of the shell pores 43 is further preferably 23nm.

[0133] In samples 1 to 4 where the average particle size of the pores 43 in the shell is less than 5nm, when the pore area ratio increases, the defective rate in the moisture load test becomes worse. Specifically, the defective rates of samples 1 to 4 where the average particle size of the pores 43 in the shell is 5nm are compared. In samples 1 to 3 where the pore area ratio is distributed in the range of 5% to 15%, the defective rate is 0%, while in sample 4 where the pore area ratio is 22%, the defective rate is 5%. According to the results, even when the average particle size of the pores 43 in the shell is as small as 5nm or less, when the pore area ratio increases, moisture can easily enter the interior of the main body 10, thereby reducing the moisture resistance of the laminated ceramic capacitor. Therefore, it is preferred to set an upper limit for the pore area ratio. When the average pore diameter is less than 5nm, the upper limit of the pore area ratio is preferably 22%. As a result, the defective rate of the moisture load test can be made less than 5%. In addition, when the average pore diameter is less than 5nm, it is further preferred to set the upper limit of the pore area ratio to 15%.

[0134] 4 Comments

[0135] The dimensions, materials, and configurations of the components described in the foregoing embodiments are not limited to the dimensions, materials, and configurations explicitly described in the embodiments, and the components may be modified in such a manner as to have any dimensions, materials, and configurations that are within the scope of the present invention.

[0136] Constituent elements that are not explicitly described in this specification may be added to the above-described embodiments, and some of the constituent elements described in the embodiments may be omitted.

[0137] The expressions "first", "second", "third" and the like in this specification are used to identify constituent elements and do not necessarily limit the number, order or content thereof. In addition, the numbers used to identify constituent elements are used in each context, and the numbers used in one context do not necessarily represent the same structure in another context. In addition, a constituent element identified by one number does not prevent a constituent element identified by another number from having the same function.

[0138] In the present specification, when one component is “comprising”, other components are not excluded and other components may be included as long as it does not conflict with the content of the present invention.

[0139] 5. Notes

[0140] The embodiments described in this specification also include the following matters.

[0141] [Note 1]

[0142] A stacked ceramic capacitor comprises: a main body having a first internal electrode layer, a second internal electrode layer, and a ceramic layer of crystal grains containing ceramic material arranged between the first internal electrode layer and the second internal electrode layer; a first external electrode arranged on the main body in a manner electrically connected to the first internal electrode layer; and a second external electrode arranged on the main body in a manner electrically connected to the second internal electrode layer, the crystal grains having a core portion and a shell portion covering the core portion, the shell portion including one or more pores within the shell.

[0143] [Note 2]

[0144] The multilayer ceramic capacitor according to Supplementary Note 1, wherein an average value of the diameters of the one or more pores in the shell is 1 nm or more.

[0145] [Note 3]

[0146] The multilayer ceramic capacitor according to Supplementary Note 1 or Supplementary Note 2, wherein an average value of the diameter of the one or more pores in the shell is 25 nm or less.

[0147] [Note 4]

[0148] A multilayer ceramic capacitor as described in any one of Appendixes 1 to 3, wherein the average diameter of the one or more pores in the shell is 5 nm or less, and in the cross section of the body, the area ratio of the one or more pores in the shell in the shell portion is 22% or less.

[0149] [Note 5]

[0150] The multilayer ceramic capacitor according to any one of Appendixes 1 to 4, wherein the ceramic material is barium titanate.

[0151] [Note 6]

[0152] The multilayer ceramic capacitor according to any one of Appendixes 1 to 5, wherein the shell portion contains a rare earth element.

[0153] [Note 7]

[0154] A circuit component comprising the multilayer ceramic capacitor according to any one of Supplementary Notes 1 to 6.

[0155] [Note 8]

[0156] An electronic device comprising the circuit assembly described in Note 7.

[0157] [Note 9]

[0158] A method for manufacturing a stacked ceramic capacitor, comprising: a powder production step for producing composite ceramic particles, the composite ceramic particles comprising a first ceramic particle and a plurality of second ceramic particles attached to the surface of the first ceramic particle, the second ceramic particle having a diameter smaller than that of the first ceramic particle and having one or more intra-particle pores; a step for forming a stacked body, the stacked body comprising a ceramic green sheet and an internal electrode pattern, the ceramic green sheet containing the composite ceramic particle, the internal electrode pattern being arranged on the first and second surfaces of the ceramic green sheet; and a step for firing the stacked body.

[0159] [Note 10]

[0160] The method for producing a multilayer ceramic capacitor according to Supplementary Note 9, wherein the powder production step includes a step of producing the second ceramic particles by a hydrothermal synthesis method.

[0161] [Note 11]

[0162] The method for producing a multilayer ceramic capacitor according to Supplementary Note 9 or Supplementary Note 10, wherein the powder production step includes a step of producing the first ceramic particles by a solid phase synthesis method.

Claims

1. A laminated ceramic capacitor, characterized in that: include: a main body having a first internal electrode layer, a second internal electrode layer, and a ceramic layer including crystal grains of a ceramic material disposed between the first internal electrode layer and the second internal electrode layer; a first external electrode provided on the main body so as to be electrically connected to the first internal electrode layer; and a second external electrode provided on the main body so as to be electrically connected to the second internal electrode layer, The crystal grain has a core portion and a shell portion covering the core portion, The shell portion includes one or more intra-shell pores.

2. The multilayer ceramic capacitor according to claim 1, wherein: The average value of the diameter of the one or more pores in the shell is greater than 1 nm.

3. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The average value of the diameter of the one or more pores in the shell is 25 nm or less.

4. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The average diameter of the one or more pores in the shell is less than 5 nm, In a cross section of the body, an area ratio of the one or more intra-shell pores in the shell portion is 22% or less.

5. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The ceramic material is barium titanate.

6. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The shell portion contains a rare earth element.

7. A circuit assembly, characterized in that: A multilayer ceramic capacitor according to claim 1 is included.

8. An electronic device, characterized in that: A circuit assembly comprising the circuit assembly of claim 7.

9. A method for manufacturing a laminated ceramic capacitor, characterized in that: include: A powder production process for producing composite ceramic particles, the composite ceramic particles comprising a first ceramic particle and a plurality of second ceramic particles attached to the surface of the first ceramic particle, the second ceramic particle having a smaller diameter than the first ceramic particle and having one or more intra-particle pores; a step of forming a laminated body including a ceramic green sheet containing the composite ceramic particles and an internal electrode pattern provided on a first surface and a second surface of the ceramic green sheet; and A step of firing the laminated body.

10. The method for manufacturing a laminated ceramic capacitor according to claim 9, wherein: The powder production step includes a step of producing the second ceramic particles by a hydrothermal synthesis method.

11. The method for manufacturing a laminated ceramic capacitor according to claim 9 or 10, wherein: The powder production step includes a step of producing the first ceramic particles by a solid phase synthesis method.