Positive plate and lithium ion battery
By covering the ceramic insulating layer on the positive electrode of the lithium-ion battery, blocking the edge effect of lithium ions and providing lithium ion supplementation during the charging and discharging process, the battery performance attenuation and safety hazards caused by excessive lithium ions embedded in the negative electrode is solved, and the battery performance attenuation and safety hazards are improved. Battery life and performance.
Patent Information
- Application Number
- CN202310636482.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the charging and discharging process of existing lithium-ion batteries, the edge effect of the positive electrode material causes excessive lithium ions to be embedded in the negative electrode, forming lithium dendrites, causing battery performance attenuation and safety hazards.
A positive electrode sheet is designed, including a positive electrode current collector, a positive electrode active material layer and a ceramic insulating layer. The ceramic insulating layer covers the edge area of the positive electrode active material layer to block the deintercalation reaction of lithium ions and provide lithium during charging and discharging. The source of supplementary ions to prevent the formation of lithium dendrites.
It effectively prevents the problem of local capacity too low due to the deintercalation of lithium ions at the edges of the positive and negative electrode sheet, prevents the formation of lithium dendrites, improves the service life and performance of the battery, and ensures the safety of the battery.
Smart Images

Figure CN119069620A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a positive electrode sheet and a lithium ion battery. Background Art
[0002] The charging and discharging process of lithium-ion batteries is achieved through the embedding and extraction of lithium ions between the positive and negative electrodes. During charging, lithium ions are extracted from the positive electrode material and embedded in the negative electrode through ion diffusion in the electrolyte; during discharging, lithium ions are extracted from the negative electrode material and embedded in the positive electrode. In order to avoid problems such as lithium dendrites caused by excessive embedding of lithium ions in the negative electrode, it is usually necessary to ensure that the negative electrode capacity of the corresponding position of the electrode sheet is greater than the positive electrode capacity, and the NP ratio is used to measure the excess ratio of the negative electrode. In production practice, there is an edge effect in the positive and negative electrode sheets. On the one hand, when the active material is coated on the current collector, the edge of the active material is affected by surface tension and will be leveled to form a gradient thin area. The active material in the thin area has a decreasing gradient compared to the internal area of the electrode body phase, and the ability to extract and extract lithium ions is reduced. In addition, the positive and negative electrode materials are relatively farther apart in space, which is not conducive to the extraction and extraction of lithium ions. On the other hand, during the charging process, lithium ions are deintercalated from the positive electrode active material, pass through the separator, and are embedded in the negative electrode active material. The migration path of lithium ions is not strictly perpendicular to the shortest path on the surface of the electrode, but a diffusion migration. As a result, in the internal area of the electrode, the lithium ions embedded in the negative electrode are evenly distributed, but at the edge of the electrode, the lithium ions from the positive electrode may diffuse to a position farther away from the edge. If this part of the lithium ions is not supported by the corresponding volume of negative electrode active material, lithium dendrites may form on the surface of the negative electrode. The lithium dendrites pierce the separator, causing the battery to short circuit and create a safety hazard. Summary of the invention
[0003] Aiming at the problem of battery performance degradation caused by excessive lithium ions migrating to the negative electrode to form lithium dendrites in the prior art, a positive electrode sheet and a lithium ion battery are provided.
[0004] The technical solution adopted by the present invention to solve the above technical problems is as follows:
[0005] The present invention provides a positive electrode sheet, comprising a positive electrode collector, a positive electrode active material layer and a ceramic insulating layer, wherein the positive electrode active material layer and the ceramic insulating layer are both coated on the surface of the positive electrode collector, the positive electrode active material layer comprises a middle area and an edge area, the edge area is located at the edge position of the middle area, and the ceramic insulating layer covers the surface of the edge area away from the positive electrode collector.
[0006] Optionally, the thickness of the bottom of the edge region gradually decreases in a direction away from the middle region, and the thickness of the ceramic insulating layer gradually increases in a direction away from the middle region.
[0007] Optionally, a surface of the ceramic insulating layer facing away from the positive electrode current collector and a surface of the middle region facing away from the positive electrode current collector are in a flush transition.
[0008] Optionally, the ceramic insulating layer is arranged around the middle area.
[0009] Optionally, the width of the edge area is 0.1-10 mm.
[0010] Optionally, a width difference between the ceramic insulating layer and the edge region is H, and H satisfies 0≤H≤1 mm.
[0011] Optionally, the thickness of the middle region is 2 μm to 200 μm, and the maximum thickness of the ceramic insulating layer is 2 μm to 200 μm.
[0012] Optionally, the ceramic insulating layer comprises the following weight components:
[0013] 60-95 parts of ceramic material and 40-5 parts of binder.
[0014] Optionally, the ceramic material includes one or more of boehmite, aluminum oxide and its modified oxides, titanium oxide and its modified oxides; the binder includes one or more of N-methylpyrrolidone, vinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer and fluorine-containing acrylate resin.
[0015] Optionally, the positive electrode active material layer includes the following components by weight:
[0016] 90-100 parts of positive electrode active material, 0-5 parts of positive electrode binder and 0-5 parts of positive electrode conductor.
[0017] Optionally, the positive electrode active material includes one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, a composite of lithium iron phosphate and carbon, lithium manganese phosphate, a composite of lithium manganese phosphate and carbon, lithium iron manganese phosphate and a composite of lithium iron manganese phosphate and carbon;
[0018] The positive electrode binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, and fluorine-containing acrylate resin;
[0019] The positive electrode conductive agent includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0020] Optionally, the positive electrode current collector is one or more of a metal foil and a composite current collector.
[0021] On the one hand, the present invention provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet is the positive electrode sheet described above, the positive electrode sheet, the separator and the negative electrode sheet are stacked, and the separator is located between the positive electrode sheet and the negative electrode sheet.
[0022] Optionally, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer, the negative electrode active material layer is coated on the surface of the negative electrode current collector, and the projection of the negative electrode active material layer on the separator overlaps with the projection of the positive electrode active material layer on the separator.
[0023] In another aspect, the present invention provides a method for preparing the positive electrode sheet, comprising the following steps:
[0024] Applying the positive electrode slurry on the positive electrode current collector and drying to form a positive electrode active material layer, wherein the positive electrode active material layer comprises a middle region and an edge region, wherein the edge region is located at an edge position of the middle region;
[0025] The ceramic insulating layer slurry is coated on the edge of the positive electrode active material layer, and the ceramic insulating layer slurry covers the surface of the edge area away from the positive electrode current collector, and is dried to obtain the ceramic insulating layer.
[0026] According to the positive electrode sheet provided by the present invention, the ceramic insulating layer is arranged at the junction of the middle area and the edge area of the positive electrode active material layer and the epitaxial position, which can block the lithium deintercalation reaction of the edge area of the positive electrode active material layer during charging and discharging, effectively preventing the local NP ratio from being too low due to the edge effect during lithium deintercalation at the edges of the positive and negative electrode sheets, and providing insulation protection after the formation of lithium dendrites at the edge of the negative electrode sheet; in addition, the active lithium ions in the positive electrode active material layer covered by the ceramic insulating layer cannot migrate during the charging and discharging process due to the obstruction of the ceramic coating, but as the battery charges and discharges and ages, the active lithium of the positive electrode is gradually consumed, and the concentration of active lithium ions in the effective electrode area of the positive electrode sheet decreases. The active lithium in the positive electrode material under the ceramic insulating layer is driven by the concentration gradient. In the subsequent charging and discharging process, it diffuses to the effective electrode area as a supplementary source of active lithium, which to a certain extent compensates for the consumption of active lithium during the aging of the battery cell and improves the service life and performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the pole piece structure provided by the present invention;
[0028] Figure 2 It is a schematic diagram of the cross-sectional structure of the pole piece provided by the present invention.
[0029] The reference numerals in the drawings of the specification are as follows:
[0030] 1. positive electrode current collector; 2. positive electrode active material layer; 21. middle area; 22. edge area;
[0031] 3. Ceramic insulating layer; 4. Positive electrode sheet; 5. Negative electrode sheet; 51. Negative electrode current collector; 52. Negative electrode active material layer; 6. Diaphragm. DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0033] In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0034] Reference Figures 1-2 The present invention provides a positive electrode sheet, comprising a positive electrode collector 1, a positive electrode active material layer 2 and a ceramic insulating layer 3, wherein the positive electrode active material layer 2 and the ceramic insulating layer 3 are both coated on the surface of the positive electrode collector 1, the positive electrode active material layer 2 comprises a middle area 21 and an edge area 22, the edge area 22 is located at the edge of the middle area 21, and the ceramic insulating layer 3 covers the surface of the edge area 22 away from the positive electrode collector 1.
[0035] Specifically, the ceramic insulating layer 3 covers the surface of the edge area 22 away from the positive electrode current collector 1. At this time, the ceramic insulating layer 3 covers and extends to the edge area 22 of the positive electrode active material layer 2. That is, the setting of the ceramic insulating layer 3 avoids the direct escape of lithium ions at the edge of the positive electrode active material layer 2, prevents excessive lithium ions from migrating to the edge of the negative electrode to form lithium dendrites, and avoids short circuits at the edge. In addition, the lithium in the positive electrode active material layer 2 covered by the ceramic insulating layer 3 is driven by the concentration gradient and continuously migrates to the effective electrode area, which is beneficial to improving the battery cycle and performance.
[0036] In some embodiments, the ceramic insulating layer 3 partially covers the surface of the edge region 22 away from the positive electrode current collector 1, and the ceramic insulating layer 3 partially covers the surface of the positive electrode current collector 1. In other embodiments, the ceramic insulating layer 3 completely covers the surface of the edge region 22 away from the positive electrode current collector 1.
[0037] In some embodiments, the thickness of the edge region 22 gradually decreases in a direction away from the middle region 21 , and the thickness of the ceramic insulating layer 3 gradually increases in a direction away from the middle region 21 .
[0038] Specifically, the thickness of the edge area 22 gradually decreases in the direction away from the middle area 21, and the thickness of the ceramic insulating layer 3 gradually increases in the direction away from the middle area 21, which is conducive to forming an insulating belt flush with the positive electrode current collector 1, thereby playing an insulating protection role; in addition, the active lithium under the covering area of the ceramic insulating layer 3 close to the middle area 21 can be used as a source of active lithium in subsequent charging and discharging to provide supplements, which to a certain extent compensates for the consumption of active lithium during the aging process of the battery cell and improves the life performance of the battery.
[0039] In some embodiments, the surface of the ceramic insulating layer 3 facing away from the positive electrode current collector 1 is in a flush transition with the surface of the middle region 21 facing away from the positive electrode current collector 1 .
[0040] The surface of the ceramic insulating layer 3 facing away from the positive electrode current collector 1 is in a flush transition with the surface of the intermediate region 21 facing away from the positive electrode current collector 1 , which is beneficial to ensure that the surface of the positive electrode current collector 1 is flat and that the battery energy density does not decrease in the absence of lithium deposition.
[0041] In some embodiments, the ceramic insulating layer 3 is disposed around the middle region 21 .
[0042] The ceramic insulating layer 3 is disposed around the middle area 21 , so that the lithium ions at the position of the middle area 21 covered by the ceramic insulating layer 3 can provide compensation in the subsequent battery consumption.
[0043] In some embodiments, the width of the edge region 22 is 0.1-10 mm.
[0044] In some embodiments, the width difference between the ceramic insulating layer 3 and the edge region 22 is H, and H satisfies 0≤H≤1mm. Within this range, the amount of the ceramic insulating layer 3 can be reduced while ensuring full coverage, thereby ensuring the energy density of the positive electrode sheet.
[0045] In some embodiments, the thickness of the middle region 21 is 2 μm to 200 μm, and the maximum thickness of the ceramic insulating layer 3 is 2 μm to 200 μm.
[0046] The maximum thickness of the ceramic insulating layer 3 is controlled to be between 2 μm and 200 μm. If the maximum thickness of the ceramic insulating layer 3 is less than 2 μm, it cannot be bonded and coated with the middle area 21, and cannot provide effective lithium compensation in the later stage of battery use; if the maximum thickness of the ceramic insulating layer 3 is greater than 200 μm, the battery energy density will be reduced.
[0047] In some embodiments, the ceramic insulating layer 3 includes the following weight components:
[0048] 60-95 parts of ceramic material and 40-5 parts of binder.
[0049] In some embodiments, the ceramic material includes one or more of boehmite, aluminum oxide and its modified oxides, titanium oxide and its modified oxides; the binder includes one or more of N-methylpyrrolidone, vinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer and fluorine-containing acrylate resin.
[0050] In some embodiments, the positive electrode active material layer 2 includes the following weight components:
[0051] 90-100 parts of positive electrode active material, 0-5 parts of positive electrode binder and 0-5 parts of positive electrode conductor.
[0052] In some embodiments, the positive electrode active material layer 2 includes the following weight components:
[0053] 90-99 parts of positive electrode active material, 1-5 parts of positive electrode binder and 0-5 parts of positive electrode conductor.
[0054] In some embodiments, the positive electrode active material includes one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, a composite of lithium iron phosphate and carbon, lithium manganese phosphate, a composite of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite of lithium iron manganese phosphate and carbon;
[0055] The positive electrode binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, and fluorine-containing acrylate resin;
[0056] The positive electrode conductive agent includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0057] In some embodiments, the positive electrode current collector 1 is one or more of a metal foil and a composite current collector.
[0058] Specifically, the metal sheet may be an aluminum foil, and the composite current collector may be a conductive sheet material formed by a composite of metal and polymer material.
[0059] An embodiment of the present invention further provides a lithium-ion battery, comprising a positive electrode sheet 4, a negative electrode sheet 5 and a separator 6, wherein the positive electrode sheet 4 is the positive electrode sheet according to any one of claims 1 to 11, and the positive electrode sheet 4, the separator 6 and the negative electrode sheet 5 are stacked, and the separator 6 is located between the positive electrode sheet 4 and the negative electrode sheet 5.
[0060] The separator 6 is located between the positive electrode sheet 4 and the negative electrode sheet 5 and is prepared into a lithium-ion battery by a winding or lamination process. The separator 6 blocks the positive electrode sheet 4, the negative electrode sheet 5 and the electron transmission and conducts the ion transmission in the lithium-ion battery.
[0061] In some embodiments, the negative electrode sheet 5 includes a negative electrode current collector 51 and a negative electrode active material layer 52, the negative electrode active material layer 52 is coated on the surface of the negative electrode current collector 51, and the projection of the negative electrode active material layer 52 on the separator 6 overlaps with the projection of the positive electrode active material layer 2 on the separator 6.
[0062] Specifically, the positive electrode sheet 4 and the negative electrode sheet 5 are overlapped and the coating areas of the positive electrode active material layer 2 and the negative electrode active material layer 52 are the same. This design is beneficial to increase the coating area of the positive electrode active material layer 2 and increase the overall energy density of the battery.
[0063] In some embodiments, the negative electrode current collector 51 is one or more of a metal foil and a composite current collector.
[0064] Specifically, the metal sheet may be a copper foil, and the composite current collector may be a conductive sheet material formed by a composite of metal and polymer material.
[0065] In some embodiments, the negative electrode active material layer 52 includes a negative electrode active material, a negative electrode binder, and a thickener.
[0066] The negative electrode active material includes one or more of artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate; the negative electrode binder includes one or more of styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid and carboxymethyl chitosan; the thickener includes one or more of sodium carboxymethyl cellulose and lithium carboxymethyl cellulose.
[0067] In some embodiments, the positive electrode sheet 4 and the negative electrode sheet 5 are subjected to edge passivation treatment.
[0068] Specifically, by passivating the edge positions of the positive electrode sheet 4 and the negative electrode sheet 5 to weaken the edge effect, the effective electrode sheet area is maximized, thereby making the best use of the space structure in the battery.
[0069] In some embodiments, the lithium-ion battery is prepared by a lamination process and / or a winding process.
[0070] Specifically, for the lamination process, the ceramic insulating layer 3 is usually coated simultaneously with the positive electrode slurry on the upper layer of the positive electrode slurry and the edge of the positive electrode active material. After the positive electrode sheet 4 is cut, the newly exposed electrode sheet end needs to be coated with a secondary ceramic insulating layer 3 to ensure that all edges of the positive electrode sheet 4 are protected by the ceramic insulating layer 3; in the specific preparation, the ceramic insulating layer 3 can also be coated at any process stage before the positive electrode sheet 4, the negative electrode sheet 5 and the separator 6 are assembled. When a lithium-ion battery is prepared by a winding process, the ceramic insulating layer 3 is usually coated simultaneously with the positive electrode slurry. The ceramic insulating layer 3 may not be coated on the upper layer of the positive electrode slurry and the edge of the positive electrode active material, and at the start and end of the cut ends of the positive electrode sheet 4 of the wound electrode core, but may be wrapped with insulating tape to simplify the process.
[0071] In some examples, the lithium-ion battery further includes a housing and positive and negative electrode lead terminals.
[0072] The shell includes one or more of a plastic shell, an aluminum shell, a steel shell, a composite aluminum-plastic film, and a soft shell made of a polypropylene flexible material.
[0073] Another embodiment of the present invention provides a method for preparing a positive electrode sheet, comprising the following steps:
[0074] The positive electrode slurry is coated on the positive electrode current collector 1, and dried to form a positive electrode active material layer 2, wherein the positive electrode active material layer 2 includes a middle region 21 and an edge region 22, and the edge region 22 is located at the edge of the middle region 21;
[0075] The ceramic insulating layer slurry is coated on the edge of the positive electrode active material layer 2 , and the ceramic insulating layer slurry covers the surface of the edge area 22 away from the positive electrode current collector 1 , and dried to obtain the ceramic insulating layer 3 .
[0076] The present invention is further described below by way of examples.
[0077] Example 1
[0078] This embodiment is used to illustrate a positive electrode sheet and a lithium-ion battery disclosed in the present invention, and includes the following operating steps:
[0079] Nickel-cobalt-manganese ternary material, carbon black, polyvinylidene fluoride, and N-methylpyrrolidone are mixed evenly in a weight ratio of 100:1:1.5:40 to obtain a positive electrode slurry; boehmite, polyvinylidene fluoride, and N-methylpyrrolidone are mixed evenly in a mass ratio of 5:1:25 to obtain a ceramic insulating layer slurry; the positive electrode slurry and the ceramic insulating layer slurry are uniformly coated on the positive electrode current collector at the same time, and the ceramic insulating layer slurry covers the positive electrode slurry and exceeds the positive electrode slurry by 1mm, so that the edge of the positive electrode active material layer is completely isolated under the ceramic insulating layer slurry; after drying, cold pressing, and cutting, a positive electrode sheet of the target size is obtained, and then the ceramic insulating layer slurry is coated again on the edge position of the positive electrode active material layer of the cut positive electrode sheet, and after drying and cold pressing, a spare positive electrode sheet is obtained. In the positive electrode sheet, the thickness of the middle area is 200μm; the maximum thickness of the ceramic insulating layer is 199μm; the width of the edge area is 9.0mm; and the width of the ceramic insulating layer is 10mm.
[0080] The spare positive electrode sheet, the negative electrode sheet with the same size of active material layer and the separator are stacked to form a battery core, the electrolyte is injected, and the shell assembly is assembled to obtain the lithium-ion battery of the present application.
[0081] Embodiments 2 to 5
[0082] Examples 2 to 5 are used to illustrate a positive electrode sheet and a lithium-ion battery disclosed in the present invention, and include most of the operating steps in Example 1, except that:
[0083] Examples 2 to 5 used the positive electrode active material layer size (mm), negative electrode active material layer size (mm), and the difference in width between the ceramic insulating layer and the edge region (mm) shown in Table 1 for Examples 2 to 5.
[0084] Comparative Examples 1 to 4
[0085] Comparative Examples 1 to 4 are used to compare and illustrate a positive electrode sheet and a lithium ion battery disclosed in the present invention, including most of the operating steps in Example 1, except that:
[0086] Comparative Examples 1 to 4 used the positive electrode active material layer size (mm) and the negative electrode active material layer size (mm) shown in Table 1 for Comparative Examples 1 to 4, and no ceramic insulating layer was provided in Comparative Examples 1 to 4.
[0087] Comparative Examples 5 to 8
[0088] Comparative Examples 5 to 8 are used to compare and illustrate a positive electrode sheet and a lithium ion battery disclosed in the present invention, including most of the operating steps in Example 1, except that:
[0089] Comparative Examples 5 to 8 adopted the positive electrode active material layer size (mm) and negative electrode active material layer size (mm) shown in Comparative Examples 5 to 8 in Table 1, and in Comparative Examples 5 to 8, a ceramic insulating layer was provided at the edge of the positive electrode active material layer, but the ceramic insulating layer did not cover the positive electrode active material layer.
[0090] Performance Testing
[0091] The performance of the lithium-ion batteries prepared in Examples 1 to 4 and Comparative Examples 1 to 8 was tested:
[0092] GB / T 31484 was used to perform capacity tests on the embodiments and comparative examples.
[0093] GB / T 31484 was used to perform cycle life tests on the embodiments and comparative examples.
[0094] The test results obtained are entered in Table 1.
[0095] Table 1
[0096]
[0097]
[0098] It can be seen from the test results in Table 1 that after Examples 1 to 4 are coated with a ceramic insulating layer, their battery capacity and cycle performance are better, while Comparative Examples 1 to 4 are not coated with a ceramic insulating layer, and their cycle performance is relatively poor and lithium deposition problems occur.
[0099] By comparing the test results of Examples 1 to 4 and Comparative Examples 1 to 4, it can be seen that the electrode of the present scheme can achieve a larger effective electrode area, improve the battery capacity, and perform better in cycle performance; by comparing Examples 1 to 2 and Comparative Example 2, it can be seen that the ceramic coating can effectively block the deintercalation of lithium ions at the edge of the electrode and inhibit the formation of lithium dendrites; similarly, by comparing Examples 3 to 4 and Comparative Examples 3 and 4, the same conclusion can be drawn.
[0100] Comparative Examples 5 to 8 are provided with a ceramic insulating layer but do not cover the positive electrode active material layer. From the test results, it can be seen that the lithium plating phenomenon of the lithium ion batteries of Comparative Examples 5 to 8 is alleviated, but the cycle performance is deteriorated. In summary, the present invention uses a ceramic insulating layer to partially coat the positive electrode active material layer, which effectively improves the lithium plating and battery cycle performance and increases its service life.
[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A positive electrode sheet, characterized in that: It includes a positive electrode collector, a positive electrode active material layer and a ceramic insulating layer, wherein the positive electrode active material layer and the ceramic insulating layer are both coated on the surface of the positive electrode collector, the positive electrode active material layer includes a middle area and an edge area, the edge area is located at the edge of the middle area, and the ceramic insulating layer covers the surface of the edge area away from the positive electrode collector.
2. A positive electrode sheet according to claim 1, characterized in that: The thickness of the bottom of the edge region gradually decreases in a direction away from the middle region, and the thickness of the ceramic insulating layer gradually increases in a direction away from the middle region.
3. A positive electrode sheet according to claim 2, characterized in that: The surface of the ceramic insulating layer facing away from the positive electrode current collector is in flush transition with the surface of the middle region facing away from the positive electrode current collector.
4. The positive electrode sheet according to claim 1, characterized in that: The ceramic insulating layer is disposed around the middle region.
5. The positive electrode sheet according to claim 1, characterized in that: The width of the edge area is 0.1-10 mm.
6. A positive electrode sheet according to claim 1 or 5, characterized in that: A width difference between the ceramic insulating layer and the edge region is H, and H satisfies 0≤H≤1 mm.
7. The positive electrode sheet according to claim 1, characterized in that: The thickness of the middle region is 2 μm to 200 μm, and the maximum thickness of the ceramic insulating layer is 2 μm to 200 μm.
8. The positive electrode sheet according to claim 1, characterized in that: The ceramic insulating layer comprises the following components by weight: 60-95 parts of ceramic material and 40-5 parts of binder.
9. A positive electrode sheet according to claim 8, characterized in that: The ceramic material includes one or more of boehmite, aluminum oxide and its modified oxides, titanium oxide and its modified oxides; the binder includes one or more of N-methylpyrrolidone, vinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer and fluorine-containing acrylate resin.
10. The positive electrode sheet according to claim 1, characterized in that: The positive electrode active material layer includes the following components by weight: 90-100 parts of positive electrode active material, 0-5 parts of positive electrode binder and 0-5 parts of positive electrode conductor.
11. A positive electrode sheet according to claim 10, characterized in that: The positive electrode active material includes one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, a composite of lithium iron phosphate and carbon, lithium manganese phosphate, a composite of lithium manganese phosphate and carbon, lithium iron manganese phosphate and a composite of lithium iron manganese phosphate and carbon; The positive electrode binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, and fluorine-containing acrylate resin; The positive electrode conductive agent includes one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
12. The positive electrode sheet according to claim 1, characterized in that: The positive electrode current collector is one or more of a metal foil and a composite current collector.
13. A lithium ion battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the positive electrode sheet is the positive electrode sheet according to any one of claims 1 to 12, the positive electrode sheet, the separator and the negative electrode sheet are stacked, and the separator is located between the positive electrode sheet and the negative electrode sheet.
14. The lithium ion battery according to claim 13, characterized in that: The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is coated on the surface of the negative electrode current collector. The projection of the negative electrode active material layer on the separator overlaps with the projection of the positive electrode active material layer on the separator.
15. The method for preparing a positive electrode sheet according to any one of claims 1 to 12, characterized in that: The following steps are involved: Applying the positive electrode slurry on the positive electrode current collector and drying to form a positive electrode active material layer, wherein the positive electrode active material layer comprises a middle region and an edge region, wherein the edge region is located at an edge position of the middle region; The ceramic insulating layer slurry is coated on the edge of the positive electrode active material layer, and the ceramic insulating layer slurry covers the surface of the edge area away from the positive electrode current collector, and is dried to obtain the ceramic insulating layer.
Citation Information
Patent Citations
Negative pole piece as well as preparation method thereof, and lithium ion battery
CN108258193A
Positive plate and lithium ion battery
CN216250793U
Negative plate and lithium ion battery
CN217691221U
Electrode assemblies, battery cells, batteries and electrical devices
CN218867146U
Cited By
Solid-state battery, electrode layer, battery cell, single battery and electric equipment
CN121097354A