Secondary battery and electric device

By designing a multi-layer structure in the positive electrode sheet of the secondary battery, optimizing the distribution of conductive carbon and sulfide electrolytes, the problem of insufficient rate performance and thermal stability of existing secondary batteries is solved, and higher battery performance and Security.

CN119069628AActive Publication Date: 2024-12-03SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410963482.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-12-03
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The current secondary batteries have insufficient rate performance and thermal stability, especially in areas such as power tools and electric drones that have not met the demand.

Method used

A positive electrode sheet structure of a secondary battery is designed, including a first positive electrode layer and a second positive electrode layer arranged in sequence on the surface of the positive electrode current collector, the first positive electrode layer contains a first conductive carbon and a first sulfide electrolyte, and the second The positive electrode layer contains the second conductive carbon and the second sulfide electrolyte. By controlling the thickness and component ratio of each layer, the first positive electrode layer provides more electronic paths, the second positive electrode layer provides more ion paths, and the intermediate layer is added. To improve thermal stability.

Benefits of technology

It significantly improves the rate performance and thermal stability of the positive electrode plate, reduces the risk of thermal runaway caused by a sharp rise in battery temperature, and enhances the safety and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069628A_ABST
    Figure CN119069628A_ABST
Patent Text Reader

Abstract

The invention discloses a secondary battery and a power utilization device, and belongs to the technical field of batteries, the secondary battery comprises a positive pole piece, the positive pole piece comprises a positive pole current collector, and a first positive pole layer and a second positive pole layer which are sequentially arranged on at least one surface of the positive pole current collector; the first positive electrode layer comprises a first positive electrode active material, first conductive carbon and a first sulfide electrolyte; the second positive electrode layer comprises a second positive electrode active material, second conductive carbon and a second sulfide electrolyte; the mass percentage content of the first conductive carbon in the first positive electrode layer is M1, and the mass percentage content of the first sulfide electrolyte in the first positive electrode layer is N1; the mass percentage content of the second conductive carbon in the second positive electrode layer is M2, and the mass percentage content of the second sulfide electrolyte in the second positive electrode layer is N2; the following formula is satisfied: M1gt; m2, N2gt; the material has excellent rate capability and thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a secondary battery and an electrical device. Background Art

[0002] Secondary batteries, also known as rechargeable batteries or storage batteries, refer to batteries that can continue to be used by activating the active substances by charging after the battery is discharged. Since its development, secondary batteries have been widely used in 3C digital products, electric vehicles and energy storage power stations.

[0003] The rate performance of a secondary battery refers to the ratio of the current value output by the battery to its rated capacity within a specified time, and is usually used to indicate the speed of battery charging and discharging. As the secondary battery market continues to expand, the requirements for its various performances are also increasing, especially in areas such as power tools and electric drones that have high requirements for rate performance, while the rate performance of existing secondary batteries still needs to be improved.

[0004] In view of this, this application is filed. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a secondary battery and an electrical device having excellent rate performance and thermal stability.

[0006] To achieve the above object, in a first aspect of the present application, the present application provides a secondary battery, the secondary battery comprising a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a first positive electrode layer and a second positive electrode layer sequentially arranged on at least one surface of the positive electrode current collector;

[0007] The first positive electrode layer includes a first positive electrode active material, a first conductive carbon and a first sulfide electrolyte;

[0008] The second positive electrode layer includes a second positive electrode active material, a second conductive carbon and a second sulfide electrolyte;

[0009] The mass percentage of the first conductive carbon in the first positive electrode layer is M1, and the mass percentage of the first sulfide electrolyte in the first positive electrode layer is N1;

[0010] The mass percentage of the second conductive carbon in the second positive electrode layer is M2, and the mass percentage of the second sulfide electrolyte in the second positive electrode layer is N2;

[0011] Satisfies: M1>M2, N2>N1.

[0012] As an implementation scheme of the present application, at least one of the following (a) to (d) is satisfied:

[0013] (a) 2% ≤ M1 ≤ 5%;

[0014] (b) 4.5% ≤ N1 ≤ 6%;

[0015] (c) 1% ≤ M2 ≤ 2%;

[0016] (d)12%≤N2≤13%.

[0017] As an embodiment of the present application, the first positive electrode layer further includes a first halide electrolyte, and the mass ratio of the first sulfide electrolyte to the first halide electrolyte is 5:(4-6); and / or

[0018] The mass ratio of the second sulfide electrolyte to the second conductive carbon is (6-13):1.

[0019] As an embodiment of the present application, the mass percentage of the first halide electrolyte in the first positive electrode layer is 4.5% to 6%.

[0020] As an embodiment of the present application, the mass percentage of the first positive electrode active material in the first positive electrode layer is 80% to 90%; and / or

[0021] The mass percentage of the second positive electrode active material in the second positive electrode layer is 80% to 90%.

[0022] As an embodiment of the present application, the positive electrode sheet further includes an intermediate layer, and the intermediate layer is located between the first positive electrode layer and the second positive electrode layer;

[0023] The intermediate layer includes a third positive electrode active material, a third conductive carbon, an oxide electrolyte, and a second halide electrolyte.

[0024] As an implementation scheme of the present application, at least one of the following (I) to (V) is satisfied:

[0025] (I) the mass ratio of the oxide electrolyte to the second halide electrolyte is 1:(2-12);

[0026] (II) the mass percentage of the third conductive carbon in the intermediate layer is 0.5% to 2%;

[0027] (III) The mass percentage of the oxide electrolyte in the intermediate layer is 1% to 5%;

[0028] (IV) the mass percentage of the second halide electrolyte in the intermediate layer is 8% to 12%;

[0029] (V) The mass percentage of the third active material in the intermediate layer is 80% to 90%.

[0030] As an embodiment of the present application, the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material each independently include LiCoO2, Li x1 Ni y1 Co z1 Mn 1-y1-z1 At least one of O2, wherein 0.96≤x1≤1.1, 0.6≤y1≤1, 0≤z1≤0.2; and / or

[0031] The first conductive carbon, the second conductive carbon, and the third conductive carbon each independently include at least one of carbon black, acetylene black, carbon nanotubes, vapor-grown carbon fibers, and graphene.

[0032] As an implementation scheme of the present application, at least one of the following (1) to (3) is satisfied:

[0033] (1) The first sulfide electrolyte and the second sulfide electrolyte each independently include Li x2 A y2 B z2 , wherein A includes at least one of Ge, Sn, and P, B includes S, 3≤x2≤10, 1≤y2≤3, 0≤z2≤12;

[0034] (2) The first halide electrolyte and the second halide electrolyte each independently include Li x3 DCl6, wherein D comprises at least one of In, Sc, and Zr, and 2≤x3≤3;

[0035] (3) The oxide electrolyte includes Li X4 E y3 G z3 , wherein E includes at least one of La, Al, Zr, Ti, and Ge, G includes one of PO and O, 0.3<X4≤7, 0.3≤y3≤3, 3≤z3≤12.

[0036] As an embodiment of the present application, the thickness of the first positive electrode layer is greater than the thickness of the intermediate layer; and / or

[0037] The thickness of the second positive electrode layer is greater than the thickness of the intermediate layer.

[0038] As an embodiment of the present application, the thickness of the first positive electrode layer is 60 μm to 80 μm; and / or

[0039] The thickness of the second positive electrode layer is 60 μm to 80 μm.

[0040] As an embodiment of the present application, the thickness of the intermediate layer is 10 μm to 20 μm.

[0041] In a second aspect of the present application, the present application provides an electrical device, comprising the secondary battery described above.

[0042] The beneficial effects of the present invention are as follows: the present application sequentially arranges a first positive electrode layer and a second positive electrode layer on at least one surface of a positive electrode current collector, adds a first conductive carbon and a first sulfide electrolyte to the first positive electrode layer, and respectively adds a second conductive carbon and a second sulfide electrolyte to the second positive electrode layer, and by controlling M1>M2, N2>N1, the content of conductive carbon in the first positive electrode layer is greater than that in the second positive electrode layer, and the content of sulfide electrolyte in the first positive electrode layer is less than that in the second positive electrode layer, so that the first positive electrode layer close to the positive electrode current collector can provide more electron paths, and the second positive electrode layer far away from the positive electrode current collector provides more ion paths, thereby effectively improving the rate performance and thermal stability of the positive electrode sheet. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 Schematic diagram of the positive electrode structure of an embodiment of the present invention.

[0044] Figure 2 Schematic diagram of the positive electrode structure of another embodiment of the present invention. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0046] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0047] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0048] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0049] See also Figure 1 , the embodiment of the present application provides a secondary battery, the secondary battery comprises a positive electrode sheet, the positive electrode sheet comprises a positive electrode collector 1 and a first positive electrode layer 2 and a second positive electrode layer 3 sequentially arranged on at least one surface of the positive electrode collector;

[0050] The first positive electrode layer includes a first positive electrode active material, a first conductive carbon and a first sulfide electrolyte;

[0051] The second positive electrode layer includes a second positive electrode active material, a second conductive carbon and a second sulfide electrolyte;

[0052] The mass percentage of the first conductive carbon in the first positive electrode layer is M1, and the mass percentage of the first sulfide electrolyte in the first positive electrode layer is N1;

[0053] The mass percentage of the second conductive carbon in the second positive electrode layer is M2, and the mass percentage of the second sulfide electrolyte in the second positive electrode layer is N2;

[0054] Satisfies: M1>M2, N2>N1.

[0055] The present application creatively arranges a first positive electrode layer and a second positive electrode layer in sequence on at least one surface of a positive electrode current collector, adds a first conductive carbon and a first sulfide electrolyte to the first positive electrode layer, and respectively adds a second conductive carbon and a second sulfide electrolyte to the second positive electrode layer, and by controlling M1>M2, N2>N1, the content of conductive carbon in the first positive electrode layer is greater than that in the second positive electrode layer, and the content of sulfide electrolyte in the first positive electrode layer is less than that in the second positive electrode layer. With such an arrangement, the first positive electrode layer close to the positive electrode current collector can provide more electron pathways, while the second positive electrode layer far from the positive electrode current collector provides more ion pathways, which is beneficial to the transmission of electrons and ions, and effectively improves the rate performance and thermal stability of the positive electrode sheet.

[0056] In one embodiment, it satisfies: 2%≤M1≤5%, for example, it can be 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or a range consisting of any two of these values. In particular, when the mass percentage of the first conductive carbon in the first positive electrode layer is within this range, it can provide more electron pathways, which is beneficial to the transmission of electrons and further improves the rate performance of the positive electrode sheet.

[0057] In one embodiment, it satisfies: 4.5%≤N1≤6%, for example, it can be 4.5%, 4.6%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6% or a range consisting of any two of these values, especially when the mass percentage of the first sulfide electrolyte in the first positive electrode layer is within this range, its content is significantly lower than the mass percentage of the second sulfide electrolyte in the second positive electrode layer, providing more ion pathways, which is beneficial to the transmission of ions and improving the rate performance of the positive electrode sheet.

[0058] In one embodiment, it satisfies: 1%≤M2≤2%, for example, it can be 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% or a range consisting of any two of these values, especially when the mass percentage of the second conductive carbon in the second positive electrode layer is within this range, its content is lower than the mass percentage of the first conductive carbon in the first positive electrode layer, which can provide more electron pathways, facilitate the transmission of electrons, and at the same time can improve the thermal stability of the positive electrode plate to a certain extent, and further improve the rate performance of the positive electrode plate.

[0059] In one embodiment, the following is satisfied: 12%≤N2≤13%, for example, it may be 12%, 12.1%, 12.2%, 12.3%, 12.4%, 12.5%, 12.6%, 12.7%, 12.8%, 12.9%, 13% or a range consisting of any two of these values.

[0060] In one embodiment, the first positive electrode layer also includes a first halide electrolyte, and the mass ratio of the first sulfide electrolyte to the first halide electrolyte is 5:(4-6), for example, it can be 5:4, 5:4.2, 5:4.5, 5:4.8, 5:5, 5:5.2, 5:5.5, 5:5.8, 5:6 or a range consisting of any two of the values. By adding the first halide electrolyte to the first positive electrode layer, the thermal stability of the positive electrode plate can be improved, especially by controlling the mass ratio of the first sulfide electrolyte to the first halide electrolyte within this range, the thermal stability and rate performance can be balanced.

[0061] In one embodiment, the mass ratio of the second sulfide electrolyte to the second conductive carbon is (6-13):1, for example, it can be 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 10:1, 11:1, 12:1, 13:1 or a range consisting of any two of the values. In particular, the mass ratio of the second sulfide electrolyte to the second conductive carbon is controlled within this range, which can effectively balance thermal stability and rate performance.

[0062] In one embodiment, the mass percentage of the first halide electrolyte in the first positive electrode layer is 4.5% to 6%, for example, it can be 4.5%, 4.6%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6% or a range consisting of any two of these values.

[0063] In one embodiment, the mass percentage of the first positive electrode active material in the first positive electrode layer is 80% to 90%, for example, it can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90% or a range consisting of any two of these values.

[0064] In one embodiment, the mass percentage of the second positive electrode active material in the second positive electrode layer is 80% to 90%, for example, it can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90% or a range consisting of any two of these values.

[0065] See also Figure 2 In one embodiment, the positive electrode sheet further includes an intermediate layer 4, and the intermediate layer is located between the first positive electrode layer and the second positive electrode layer;

[0066] The intermediate layer includes a third positive electrode active material, a third conductive carbon, an oxide electrolyte, and a second halide electrolyte.

[0067] The present application sets an intermediate layer between the first positive electrode layer and the second positive electrode layer, and adds a third conductive carbon, an oxide electrolyte and a second halide electrolyte to the intermediate layer, which effectively improves the thermal stability of the positive electrode plate, thereby reducing the risk of thermal runaway of the battery caused by a sharp increase in the temperature of the secondary battery, and improving the thermal safety of the secondary battery. At the same time, the setting of the intermediate layer can further improve the rate performance.

[0068] In one embodiment, the mass ratio of the oxide electrolyte to the second halide electrolyte is 1:(2-12); for example, it can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12 or a range consisting of any two of the values.

[0069] In one embodiment, the mass percentage of the third conductive carbon in the middle layer is 0.5% to 2%; for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2% or a range consisting of any two of these values.

[0070] In one embodiment, the mass percentage of the oxide electrolyte in the intermediate layer is 1% to 5%; for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or a range consisting of any two of these values.

[0071] In one embodiment, the mass percentage of the second halide electrolyte in the intermediate layer is 8% to 12%; for example, it can be 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12% or a range consisting of any two of these values.

[0072] In one embodiment, the mass percentage of the third active material in the intermediate layer is 80% to 90%; for example, it can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90% or a range consisting of any two of these values.

[0073] In one embodiment, the first positive electrode active material, the second positive electrode active material, and the third positive electrode active material each independently include LiCoO2, Li x1 Ni y1 Co z1 Mn 1-y1-z1 At least one of O2, wherein 0.96≤x1≤1.1, 0.6≤y1≤1, and 0≤z1≤0.2.

[0074] In one embodiment, the first conductive carbon, the second conductive carbon, and the third conductive carbon each independently include at least one of carbon black, acetylene black, carbon nanotubes, vapor-grown carbon fibers, and graphene.

[0075] In one embodiment, the first sulfide electrolyte and the second sulfide electrolyte each independently include Li x2 A y2 B z2 , wherein A includes at least one of Ge, Sn, and P, B includes S, 3≤x2≤10, 1≤y2≤3, 0≤z2≤12.

[0076] In one embodiment, the first sulfide electrolyte and the second sulfide electrolyte each independently include Li 10 GeP2S 12 、Li7P3S 11 、Li6PS5Cl、Li 5.5 PS 4.5 Cl 1.5 , Li3PS4 or at least one of the following.

[0077] In one embodiment, the first halide electrolyte and the second halide electrolyte each independently include Li x3 DCl6, wherein D includes at least one of In, Sc, and Zr, and 2≤x3≤3.

[0078] In one embodiment, the first halide electrolyte and the second halide electrolyte each independently include at least one of Li3InCl6, Li3ScCl6, and Li2ZrCl6.

[0079] In one embodiment, the oxide electrolyte comprises Li X4 E y3 G z3 , wherein E includes at least one of La, Al, Zr, Ti, and Ge, G includes one of PO and O, 0.3<x4≤7, 0.3≤y3≤3, 3≤z3≤12.

[0080] In one embodiment, the oxide electrolyte comprises Li7La3Zr2O 12 , Li 1.3 Al 0.3 Ti 1.7 (PO4)3, Li1 .3 Al 0.3 Ge 1.7 (PO4)3, Li 0.33 La 0.55 One or more of TiO3.

[0081] In one embodiment, the thickness of the first positive electrode layer is greater than the thickness of the intermediate layer.

[0082] In one embodiment, the thickness of the second positive electrode layer is greater than the thickness of the intermediate layer.

[0083] By controlling the thickness relationship between the first positive electrode layer, the second positive electrode layer and the intermediate layer, the present application can provide suitable ion and electron transmission lines, the diffusion distance of ions and electrons is appropriate, the diffusion path is relatively appropriate, the polarization phenomenon is effectively reduced, and the rate performance is improved.

[0084] In one embodiment, the thickness of the first positive electrode layer is 60 μm to 80 μm, for example, it can be 60 μm, 62 μm, 65 μm, 68 μm, 70 μm, 72 μm, 75 μm, 78 μm, 80 μm or a range consisting of any two of these values.

[0085] The thickness of the second positive electrode layer is 60 μm to 80 μm, for example, 60 μm, 62 μm, 65 μm, 68 μm, 70 μm, 72 μm, 75 μm, 78 μm, 80 μm or a range consisting of any two of these values.

[0086] As an embodiment of the present application, the thickness of the intermediate layer is 10μm to 20μm, for example, it can be 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm or a range consisting of any two of these values.

[0087] In one embodiment, the first positive electrode layer further includes a first binder, and the mass percentage of the first binder in the first positive electrode layer is 0.5% to 2%; for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2% or a range consisting of any two of these values.

[0088] In one embodiment, the second positive electrode layer further includes a second binder, and the mass percentage of the second binder in the second positive electrode layer is 0.5% to 2%; for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2% or a range consisting of any two of these values.

[0089] In one embodiment, the intermediate layer also includes a third binder, and the mass percentage of the third binder in the intermediate layer is 0.5% to 2%; for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2% or a range consisting of any two of these values.

[0090] In one embodiment, the first binder, the second binder, and the third binder each independently include at least one of polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene·ethylene copolymer\polyethylene, propylene·α-olefin copolymer, polyvinylidene fluoride, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, styrene-butadiene rubber, nitrile rubber, fluororubber, isoprene rubber, polybutadiene rubber, ethylene-propylene rubber, styrene·butadiene·styrene block copolymer or its hydrogenated product, ethylene·propylene·diene terpolymer, styrene·ethylene·butadiene·ethylene copolymer, styrene·isoprene·styrene block copolymer, isotactic-1,2-polybutadiene, polyvinyl acetate, and ethylene·vinyl acetate copolymer.

[0091] In one embodiment, the type of the positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. In one embodiment, the positive electrode current collector includes metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and carbon materials such as carbon cloth and carbon paper. In one embodiment, the positive electrode current collector is a metal material. In one embodiment, the positive electrode current collector is aluminum.

[0092] There is no particular restriction on the form of the positive electrode current collector. When the positive electrode current collector is a metal material, the positive electrode current collector may be in the form of metal foil, metal cylinder, metal strip roll, metal plate, metal foil, metal plate mesh, stamped metal, foamed metal, etc. When the positive electrode current collector is a carbon material, the positive electrode current collector may include but is not limited to a carbon plate, a carbon film, a carbon cylinder, etc.

[0093] It should be noted that the present application can detect the thickness of the first positive electrode layer, the second positive electrode layer and the intermediate layer and the content of each component therein by the following two methods:

[0094] 1. In the case where the positive electrode sheet can be separated from the battery, first analyze the positive electrode cross section by SEM and EDS-mapping, and determine the thickness, element type and element ratio of each layer in a semi-quantitative manner by EDS-mapping. Then scrape the powder on both sides of the positive electrode sheet (corresponding to the first positive electrode layer and the second positive electrode layer, respectively) and perform ICP-OES analysis to quantify the content of all elements involved and calculate the ratio of each component in the first positive electrode layer and the second positive electrode layer. Then take the entire positive electrode sheet for ICP-OES analysis to quantify the content of all elements involved, and then deduct the element content in the first positive electrode layer and the second positive electrode layer to calculate the ratio of each component in the middle layer.

[0095] 2. In the case where the positive electrode sheet is difficult to separate from the battery, the positive electrode cross section is first analyzed by SEM and EDS-mapping, and the thickness, element type and element ratio of each layer are determined semi-quantitatively by EDS-mapping. Then, advanced ion beam thinning technology (CP or FIB) is used to obtain the surfaces of the first positive electrode layer, the middle layer, and the second positive electrode layer, and then TOF-SIMS is used to quantitatively detect and analyze the three surfaces to infer the components corresponding to each layer.

[0096] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape.

[0097] In one embodiment, the secondary battery further includes a negative electrode sheet and a solid electrolyte disposed between the positive electrode sheet and the negative electrode sheet.

[0098] In one embodiment, the negative electrode plate includes one or more of a lithium plate, an indium plate, and a LiIn alloy plate.

[0099] An embodiment of the present application provides an electric device, comprising the secondary battery described above, wherein the secondary battery serves as a power supply for the electric device.

[0100] Exemplarily, the above-mentioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0101] The present application is further described below with specific embodiments:

[0102] Example 1

[0103] A method for preparing a secondary battery comprises the following steps:

[0104] (1) Cathode preparation

[0105] LiNi 0.8 Co 0.1 Mn 0.1 O2 (hereinafter referred to as NCM811), Li6PS5Cl, Li3InCl6, vapor grown carbon fiber (hereinafter referred to as VGCF), and PTFE were weighed in a weight ratio of 87:5:5:2:1, ball-milled at 200 rpm for 1 hour using a planetary ball mill, and roller-pressed to obtain the first positive electrode layer.

[0106] NCM811, Li6PS5Cl, VGCF, and PTFE were weighed in a weight ratio of 85:13:1:1, ball-milled at 200 rpm for 1 hour using a planetary ball mill, and roller-pressed to obtain a second positive electrode layer.

[0107] (2) All-solid-state battery assembly: Add electrolyte powder Li6PS5Cl to the mold battery, and then apply 30MPa pressure for pre-pressing. Then add the second positive electrode layer and the first positive electrode layer on the electrolyte side in sequence. Add indium sheets and lithium sheets on the other side. Then apply 400MPa pressure to complete the assembly of the all-solid-state battery. Finally, the assembled all-solid-state battery is subjected to constant current charge and discharge test.

[0108] The thickness, component content and ratio of Example 1 are shown in Table 1.

[0109] P in Table 1 represents the mass ratio of the sulfide electrolyte to the first halide electrolyte in the first positive electrode layer; Q represents the mass ratio of the sulfide electrolyte to the second conductive carbon in the second positive electrode layer.

[0110] Examples 2 to 18, Comparative Examples 4 to 7

[0111] The difference between Examples 2 to 18 and Comparative Examples 4 to 7 and Example 1 is that Examples 2 to 18 and Comparative Examples 4 to 7 change the composition ratio or thickness of the first positive electrode layer and the second positive electrode layer, and the other aspects are the same.

[0112] Embodiment 19

[0113] A method for preparing a secondary battery comprises the following steps:

[0114] (1) Cathode preparation

[0115] LiNi 0.8 Co 0.1 Mn 0.1 O2 (hereinafter referred to as NCM811), Li6PS5Cl, Li3InCl6, vapor grown carbon fiber (hereinafter referred to as VGCF), and PTFE were weighed in a weight ratio of 87:5:5:2:1, ball-milled at 200 rpm for 1 hour using a planetary ball mill, and roller-pressed to obtain the first positive electrode layer.

[0116] NCM811, Li7La3Zr2O 12 , Li3InCl6, VGCF, and PTFE were weighed in a weight ratio of 85:2:11:1:1, ball-milled at 200 rpm for 1 hour using a planetary ball mill, and roller-pressed to obtain an intermediate layer;

[0117] NCM811, Li6PS5Cl, VGCF, and PTFE were weighed in a weight ratio of 85:13:1:1, ball-milled at 200 rpm for 1 hour using a planetary ball mill, and roller-pressed to obtain a second positive electrode layer.

[0118] (2) All-solid-state battery assembly: Add electrolyte powder Li6PS5Cl to the mold battery, and then apply 30MPa pressure for pre-pressing. Then add the second positive electrode layer, the middle layer, and the first positive electrode layer on the electrolyte side in sequence. Add indium sheets and lithium sheets on the other side. Then apply 400MPa pressure to complete the assembly of the all-solid-state battery. Finally, the assembled all-solid-state battery is subjected to constant current charge and discharge tests.

[0119] Among them, the thickness, component content and ratio of Example 19 are shown in Table 2.

[0120] R in Table 2 represents the mass ratio of the oxide electrolyte to the halide electrolyte in the intermediate layer.

[0121] Embodiments 20 to 35

[0122] The difference between Examples 20 to 35 and Example 19 is that Examples 20 to 35 change the composition ratio or thickness of the intermediate layer, and are otherwise the same.

[0123] Comparative Example 1

[0124] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not contain the first intermediate layer, and the other aspects are the same.

[0125] Comparative Example 2

[0126] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not contain a second intermediate layer, and the other aspects are the same.

[0127] Comparative Example 3

[0128] The difference between Comparative Example 3 and Example 1 is that the first intermediate layer of the same thickness is used to replace the second intermediate layer in Comparative Example 3, and the other aspects are the same.

[0129] Table 1

[0130]

[0131]

[0132]

[0133] Table 2

[0134]

[0135]

[0136] Performance Testing

[0137] DSC onset exothermic temperature: tested using Hitachi NEXTADSC series differential scanning calorimeter (DSC).

[0138] 1C capacity / 0.1C capacity: cut-off voltage 1.9-3.7V, first cycle 3 times at 0.1C, then cycle 100 times at 0.5C.

[0139] Table 3

[0140]

[0141]

[0142]

[0143] It can be seen from Table 3 that the positive electrode plate of the present invention has excellent rate performance and thermal stability.

[0144] By comparing Example 1 with Comparative Examples 1 to 3, it can be seen that the first positive electrode layer and the second positive electrode layer sequentially arranged on at least one surface of the positive electrode current collector in the present application significantly improve the rate performance and thermal stability.

[0145] By comparing Example 1 with Comparative Examples 4 to 7, it can be seen that the present application significantly improves the rate performance and thermal stability by controlling M1>M2 and N2>N1.

[0146] By comparing Examples 1 to 4 with Examples 5 to 6, it can be seen that the rate performance is further improved by controlling the content of conductive carbon in the first positive electrode layer to 2% to 5% and the content of conductive carbon in the second positive electrode layer to 1% to 3%.

[0147] By comparing Examples 1, 8, and 9 with Examples 7 and 10, it can be seen that in the present application, the rate performance is further improved by controlling the content of the sulfide electrolyte in the first positive electrode layer to 4.5% to 6% and the content of the sulfide electrolyte in the second positive electrode layer to 12% to 14%.

[0148] By comparing Examples 1, 12, and 13 with Examples 11 and 14, it can be seen that with the increase of the halide electrolyte in the first positive electrode layer, the battery rate performance is slightly improved, while the DSC onset exothermic temperature gradually increases, indicating that the halide electrolyte is beneficial to improving the safety of the positive electrode.

[0149] By comparing Examples 1, 16, and 17 with Examples 15 and 18, it can be seen that by controlling the thickness of the first positive electrode layer and the second positive electrode layer to be 60 μm to 80 μm, the rate performance is further improved.

[0150] By comparing Example 1 with Examples 19 to 35, it can be seen that the present application further improves the rate performance and thermal stability of the positive electrode plate by introducing an intermediate layer.

[0151] It can be seen from the comparison of Examples 19 to 23 that as the content of the halide electrolyte increases, the rate performance of the positive electrode is slightly improved, but the DSC onset exothermic temperature decreases significantly, wherein the content range of the preferred halide electrolyte is 8% to 12%.

[0152] By comparing Examples 21 and 24 to 27, it can be seen that the optimal content of conductive carbon in the middle layer is 0.5% to 2%. Within this content range, a positive electrode sheet with better rate performance and better thermal stability can be obtained.

[0153] By comparing Examples 21 and 28 to 31, it can be seen that the optimal addition amount of the oxide electrolyte in the intermediate layer is 1% to 5%. Within this content range, a positive electrode sheet with better rate performance and better thermal stability can be obtained.

[0154] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.

Claims

1. A secondary battery comprising a positive electrode plate, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a first positive electrode layer and a second positive electrode layer sequentially arranged on at least one surface of the positive electrode current collector; The first positive electrode layer includes a first positive electrode active material, a first conductive carbon and a first sulfide electrolyte; The second positive electrode layer includes a second positive electrode active material, a second conductive carbon and a second sulfide electrolyte; The mass percentage of the first conductive carbon in the first positive electrode layer is M1, and the mass percentage of the first sulfide electrolyte in the first positive electrode layer is N1; The mass percentage of the second conductive carbon in the second positive electrode layer is M2, and the mass percentage of the second sulfide electrolyte in the second positive electrode layer is N2; Satisfies: M1>M2, N2>N1.

2. The secondary battery according to claim 1, characterized in that: Satisfy at least one of the following (a) to (d): (a) 2% ≤ M1 ≤ 5%; (b) 4.5% ≤ N1 ≤ 6%; (c) 1% ≤ M2 ≤ 2%; (d)12%≤N2≤13%.

3. The secondary battery according to claim 1, characterized in that: The first positive electrode layer further includes a first halide electrolyte, and the mass ratio of the first sulfide electrolyte to the first halide electrolyte is 5:(4-6); and / or The mass ratio of the second sulfide electrolyte to the second conductive carbon is (6-13):

1.

4. The secondary battery according to claim 3, characterized in that: The mass percentage of the first halide electrolyte in the first positive electrode layer is 4.5% to 6%.

5. The secondary battery according to claim 1, characterized in that: The mass percentage of the first positive electrode active material in the first positive electrode layer is 80% to 90%; and / or The mass percentage of the second positive electrode active material in the second positive electrode layer is 80% to 90%.

6. The secondary battery according to claim 1, characterized in that: The positive electrode sheet further includes an intermediate layer, and the intermediate layer is located between the first positive electrode layer and the second positive electrode layer; The intermediate layer includes a third positive electrode active material, a third conductive carbon, an oxide electrolyte, and a second halide electrolyte.

7. The secondary battery according to claim 6, characterized in that: Satisfy at least one of the following (I) to (V): (I) the mass ratio of the oxide electrolyte to the second halide electrolyte is 1:(2-12); (II) the mass percentage of the third conductive carbon in the intermediate layer is 0.5% to 2%; (III) The mass percentage of the oxide electrolyte in the intermediate layer is 1% to 5%; (IV) the mass percentage of the second halide electrolyte in the intermediate layer is 8% to 12%; (V) The mass percentage of the third active material in the intermediate layer is 80% to 90%.

8. The secondary battery according to claim 6, characterized in that: The first positive electrode active material, the second positive electrode active material, and the third positive electrode active material independently include LiCoO2, Li x1 Ni y1 Co z1 Mn 1-y1-z1 At least one of O2, wherein 0.96≤x1≤1.1, 0.6≤y1≤1, 0≤z1≤0.2; and / or The first conductive carbon, the second conductive carbon, and the third conductive carbon each independently include at least one of carbon black, acetylene black, carbon nanotubes, vapor-grown carbon fibers, and graphene.

9. The secondary battery according to claim 6, characterized in that: Satisfy at least one of the following (1) to (3): (1) The first sulfide electrolyte and the second sulfide electrolyte each independently include Li x2 A y2 B z2 , wherein A includes at least one of Ge, Sn, and P, B includes S, 3≤x2≤10, 1≤y2≤3, 0≤z2≤12; (2) The first halide electrolyte and the second halide electrolyte each independently include Li x3 DCl6, wherein D comprises at least one of In, Sc, and Zr, and 2≤x3≤3; (3) The oxide electrolyte includes Li X4 E y3 G z3 , wherein E includes at least one of La, Al, Zr, Ti, and Ge, G includes one of PO and O, 0.3<x4≤7, 0.3≤y3≤3, 3≤z3≤12.

10. The secondary battery according to claim 6, characterized in that: The thickness of the first positive electrode layer>the thickness of the intermediate layer; and / or The thickness of the second positive electrode layer is greater than the thickness of the intermediate layer.

11. The secondary battery according to claim 10, characterized in that: The thickness of the first positive electrode layer is 60 μm to 80 μm; and / or The thickness of the second positive electrode layer is 60 μm to 80 μm.

12. The secondary battery according to claim 9, characterized in that: The thickness of the intermediate layer is 10 μm to 20 μm.

13. An electrical device, characterized in that: A secondary battery comprising any one of claims 1 to 12.

Citation Information

Patent Citations

  • Double-layer coated positive electrode, preparation method thereof and all-solid-state battery

    CN116779766A

  • Nonaqueous secondary battery

    JP2003151550A

  • All-solid-state secondary battery

    US20190067695A1

  • Lithium sulfur battery positive electrode, lithium sulfur battery, and charging / discharging method for same

    WO2023210232A1

  • Secondary battery and electric device

    WO2024119474A1

Cited By

  • Secondary battery and electric device

    CN119852493A

  • Secondary battery and electric device

    WO2026144545A1