Sodium ion battery

By introducing the interaction between copper elements and boron-containing compound A into the positive electrode of the sodium ion battery, a dense passivation film is formed, which solves the problem of passivation film formation of sodium ion battery at high temperatures, and significantly improves the cycle life and performance of the battery.

CN119069631APending Publication Date: 2024-12-03LIYANG HINA BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206793.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

At high temperatures, existing sodium ion batteries have difficulty forming a dense passivation film on the surface of the positive electrode current collector, resulting in a shortening of the battery cycle life and an increase in impedance, and the use of organic electrolyte salts increases cost and process complexity.

Method used

By introducing the interaction between copper element and boron-containing compound A into the positive electrode, a bidirectional dense passivation film is formed from the inside out and from the outside, and the ratio of copper element, boron-containing compound A and organic electrolyte salt is regulated to ensure bluntness The high durability, uniformity and moderate thickness of the decompression film reduce impedance.

Benefits of technology

It effectively suppresses corrosion of the positive electrode current collector, improves the battery cycle life and high temperature capacity retention rate, reduces the impedance growth rate, and improves battery performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a sodium ion battery which comprises a positive electrode containing a copper element and an electrolyte containing an organic electrolyte salt and an additive, the copper element in the positive electrode is distributed in a positive electrode active material and a current collector, and the additive comprises one or more of boron compounds A; the sodium ion battery satisfies the following conditions: 0.001 < = a * (b + 100c) / d < = 0.3, 0.1% < = a < = 5%, 0.5% < = b < = 12%, 0.01% < = c < = 0.1%, and 1% < = d < = 12%, a is the mass percentage content of the additive (boron-containing compound A) in the electrolyte, b is the mass percentage content of the copper element in the positive electrode active material, c is the mass percentage content of the copper element in the positive electrode current collector, and d is the mass percentage content of the copper element in the negative electrode current collector. And d is the mass percentage content of the organic electrolyte salt in the electrolyte. Through the interaction of the copper element and the boron-containing compound A, a passive film is constructed on the surface of the positive electrode current collector, so that the capacity retention ratio of the battery at high temperature is improved, the impedance growth rate is reduced, and the battery performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery which utilizes the interaction between a boron-containing compound A and copper elements at different distribution positions in a positive electrode to generate a good passivation film. Background Art

[0002] In recent years, lithium-ion batteries have been widely used in electric vehicles and large-scale energy storage. However, the abundance of lithium in the earth's crust is only 0.0065%, and the resource distribution is uneven. In contrast, sodium-ion batteries have the same principle and similar structure as lithium-ion batteries, and have the characteristics of wide resources, low cost, wide temperature range and high safety. They have become an important development target for the next generation of secondary batteries.

[0003] Electrolyte is an important component of secondary batteries, mainly composed of solvents, electrolyte salts and additives. Among them, sodium hexafluorophosphate (NaPF6) has high conductivity, can form a stable passivation film with aluminum foil, and has good compatibility with carbon negative electrodes, but electrolytes containing NaPF6 are easily decomposed at high temperatures to produce toxic hydrofluoric acid (HF), which poisons the positive and negative solid electrolyte interface films (SEI and CEI) and causes battery performance degradation. Therefore, organic electrolyte salts with high temperature stability, such as sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), and sodium trifluoromethanesulfonate (NaCF3SO3), have been widely studied in sodium ion batteries.

[0004] Although organic electrolyte salts can prevent the SEI and CEI layers on the positive and negative electrodes from being corroded to a certain extent, in sodium ion batteries, since the positive electrode usually uses aluminum foil as the current collector, the anions of the organic electrolyte salts are difficult to form a dense passivation film on the surface of the aluminum current collector under high voltage, resulting in a shortened battery cycle life. Although the formation of the passivation film can be promoted through interface engineering or pre-electrochemical treatment, it will significantly increase the cost and process complexity, and may cause battery component failure. In contrast, the generation of a passivation film to protect the positive electrode by the battery electrolyte can effectively reduce the cost and process complexity, and provide a stable interface for the uniform migration of ions and charge transfer, thereby improving the energy density and power density of the battery and extending the battery life. However, the passivation film formed by the current battery electrolyte often has low durability and an uneven interface, which will undoubtedly lead to uneven ion transmission paths, thereby increasing resistance and affecting battery performance. At the same time, although the formation of a passivation film can protect the positive electrode current collector from corrosion, an overly thick passivation film will also cause the protective film impedance to be too large. Therefore, how to form a highly durable, uniform and thin passivation film is crucial to improving battery performance and extending battery life. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention utilizes the interaction between the copper element and the boron-containing compound A to form a bidirectional dense passivation film from the inside to the outside and from the outside to the inside on the surface of the positive electrode current collector, thereby avoiding the corrosion problem caused by the addition of organic electrolyte salts. At the same time, by regulating the copper element, the boron-containing compound A and the organic electrolyte salt in the positive electrode, a highly durable, uniformly dense and moderately thick passivation film can be formed on the surface of the positive electrode current collector, thereby avoiding the impedance increase problem caused by the generation of the passivation film, improving the capacity retention rate of the battery at high temperature, and reducing the impedance growth rate.

[0006] A sodium ion battery proposed in the present invention comprises a positive electrode containing copper elements, and an electrolyte containing an organic electrolyte salt and an additive, wherein the copper element in the positive electrode is distributed in the positive electrode active material and the current collector, and the additive comprises one or more of the boron-containing compounds A having the structure of formula I and / or formula II:

[0007]

[0008] Wherein, X is fluorine; R is selected from one of substituted or unsubstituted alkylene with 1 to 5 carbon atoms, substituted or unsubstituted halogenated alkylene with 1 to 5 carbon atoms, substituted or unsubstituted arylene with 6 to 10 carbon atoms, and substituted or unsubstituted halogenated arylene with 6 to 10 carbon atoms, and when substituted, the substituent is selected from hydroxyl, amino, nitro, cyano, carboxyl, acyl, thio, alkenyl, and alkynyl; r is selected from an integer of 0 to 2; p represents an integer of 0 to 4, and r+p satisfies the coordination number of B in formula I; q represents 0 or 1; Z1-Z4 are independently selected from oxygen or sulfur;

[0009] The sodium ion battery of the present invention satisfies 0.001≤a*(b+100c) / d≤0.3, 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, and 1%≤d≤12%, wherein a is the mass percentage of the additive (i.e., the boron-containing compound A) in the electrolyte, b is the mass percentage of the copper element in the positive electrode active material, c is the mass percentage of the copper element in the positive electrode current collector, and d is the mass percentage of the organic electrolyte salt in the electrolyte.

[0010] As a further solution, the sodium ion battery of the present invention satisfies 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, 1%≤d≤12%, and 0.002≤a*(b+100c) / d≤0.1. The above preferred range is conducive to further improving the synergistic optimization of the passivation film in maintaining cycle stability and improving ion transmission, and further reducing the impedance growth while ensuring high temperature cycle stability.

[0011] As a further solution, the sodium-ion battery of the present invention satisfies 0.3% ≤ a ≤ 3.5%, 2% ≤ b ≤ 10%, 0.03% ≤ c ≤ 0.08%, 3% ≤ d ≤ 10%, and 0.005 ≤ a*(b + 100c) / d ≤ 0.015.

[0012] As a further solution, the positive electrode includes a positive electrode material layer and a positive electrode current collector containing a copper element.

[0013] As a further solution, the positive electrode material layer includes a positive electrode active material containing a copper element, a positive electrode binder, and a positive electrode conductive agent.

[0014] As a still further solution, the positive electrode active material containing a copper element is an O3-phase metal layered oxide containing a copper element, and the general formula of the O3-phase metal layered oxide containing a copper element is Na x Cu y TM z O2, where 0.95 < x ≤ 1.05, 0.001 ≤ y ≤ 0.4, y + z = 1, and TM represents a transition metal element with unfilled d electron orbitals, specifically including scandium (Sc), yttrium (Y), lanthanide elements (from lanthanum (La) to lutetium (Lu)), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), mercury (Hg), or one or more of them.

[0015] As a still further solution, in the positive electrode active material Na x Cu y TM z O2, 0.95 < x ≤ 1.05, 0.01 ≤ y ≤ 0.31, and y + z = 1.

[0016] As a still further solution, in the positive electrode active material Na x Cu y TM z O2, 0.95 < x ≤ 1.05, 0.02 ≤ y ≤ 0.19, y + z = 1, and TM includes Ni, Fe, and Mn.

[0017] As a still further solution, the positive electrode active material of the copper element is Na x Cu y Ni a Fe b Mn c Md O2, where 0.95 < x ≤ 1.05, 0.02 ≤ y ≤ 0.19, 0.2 ≤ a ≤ 0.34, 0.2 ≤ b ≤ 0.4, 0.2 ≤ c ≤ 0.4, 0 ≤ d ≤ 0.2, and a + b + c + d = 1, and M is one or more of scandium (Sc), yttrium (Y), lanthanide elements (from lanthanum (La) to lutetium (Lu)), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), technetium (Tc), rhenium (Re), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), mercury (Hg).

[0018] As a further solution, the positive electrode binder includes at least one of a thermoplastic resin, an acrylic resin, sodium carboxymethyl cellulose, and styrene-butadiene rubber.

[0019] As a further solution, the positive electrode conductive agent includes a crystalline carbon material and an amorphous carbon material.

[0020] As a further solution, the positive electrode current collector containing a copper element is a metal foil layer containing a copper element.

[0021] As a further solution, the metal in the metal foil layer containing a copper element may include one or several of aluminum, zinc, magnesium, titanium, and nickel.

[0022] As a further solution, in the structure of Formula I and / or Formula II of the boron-containing compound A, X is fluorine, R is selected from a substituted or unsubstituted alkylene group with 1 to 5 carbon atoms, a substituted or unsubstituted haloalkylene group with 1 to 5 carbon atoms, the substituent is selected from a hydroxyl group, an amino group, a nitro group, a cyano group, a carboxyl group, an acyl group, a sulfhydryl group, an alkenyl group, an alkynyl group, r is 0 or 2; p is an integer selected from 0 or 4, and r + p is the coordination number of B in Formula I; q is selected from 0 or 1; at least one of Z1-Z4 contains sulfur, and the rest are oxygen.

[0023] As a further solution, in the structure of Formula I and / or Formula II of the boron-containing compound A, X is fluorine, R is selected from an alkylene group or a haloalkylene group with 1 to 3 carbon atoms, r is 0 or 2; p is an integer selected from 0 or 4, and r + p is the coordination number of B in Formula I; q is 1; at least one of Z1-Z4 contains sulfur, and the rest are oxygen.

[0024] As a still further solution, the boron-containing compound A is selected from one or more of NaBF4 or a compound in which at least one of Z1-Z4 in the structural formula II contains sulfur and the rest are oxygen.

[0025] As a further embodiment, the boron-containing compound A is selected from one or more of NaBF4 compound II, compound III, and compound IV.

[0026]

[0027] As a further solution, the additive may further include a second additive, and the second additive is a sulfate compound.

[0028] As a further solution, the second additive is a cyclic sulfate compound.

[0029] As a further solution, the content of the second additive in the electrolyte is 0.1%-2%.

[0030] As a further solution, the additive may further include a third additive, and the third additive is selected from at least one of sultone compounds, cyclic carbonate compounds, or fluorine-containing inorganic salt compounds.

[0031] As a further solution, the third additive contains an O=T structure, wherein T can be any one of P, S and C.

[0032] As a further solution, the content of the third additive in the electrolyte is 0.1%-1.5%.

[0033] As a further embodiment, the electrolyte further includes an inorganic electrolyte salt, an organic electrolyte salt and a solvent.

[0034] As a further embodiment, the inorganic electrolyte salt is substituted with fluorine.

[0035] As yet a further aspect, the inorganic electrolyte salt includes NaPF6.

[0036] As a further solution, the content of NaPF6 in the electrolyte is 1%≤NaPF6≤15%.

[0037] As a further solution, the content of NaPF6 in the electrolyte is 3%≤NaPF6≤10%.

[0038] As a further embodiment, the organic electrolyte salt includes at least one of an organic sulfonyl sodium salt and an organic phosphate sodium salt.

[0039] As a further embodiment, the organic sulfonyl sodium salt includes at least one of sulfonimide sodium salt, sulfonic acid sodium salt, sulfonyl chloride sodium salt, sulfonamide sodium salt, sulfonic acid ester sodium salt, sulfonylurea sodium salt, and sulfonamide methyl ester sodium salt.

[0040] As a further embodiment, the organic sulfonyl sodium salt includes sulfonimide sodium salt and sulfonic acid sodium salt.

[0041] As a further embodiment, the organic sulfonyl sodium salt is fluorinated or substituted with fluorine.

[0042] As a further embodiment, the number of fluorine substitutions in the organic sulfonyl sodium salt molecule is preferably 3 or more.

[0043] As a further solution, the content of the organic electrolyte salt in the electrolyte is 5%-10%.

[0044] As a further solution, the solvent includes at least one of a linear carbonate solvent, a carboxylate solvent, and a phosphate solvent.

[0045] The sodium ion battery provided by the present invention also includes a negative electrode and a separator.

[0046] Compared with the prior art, the present invention has at least the following beneficial effects:

[0047] The sodium ion battery provided by the present invention introduces copper element into the positive electrode material, and uses the boron-containing compound A as an additive, utilizes the interaction between the copper element and the boron-containing compound A, forms a bidirectional dense passivation film from the inside to the outside and from the outside to the inside on the surface of the positive electrode current collector, and controls 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, 1%≤d≤12%, and 0.001≤a*(b+100c) / d≤0.3, controls the formation of a dense and uniform composite passivation film on the surface of the positive electrode current collector, effectively resists the erosion of organic electrolyte salts, reduces the occurrence of battery side reactions, reduces the overall impedance, and improves the battery cycle life.

[0048] The composite passivation film has strong chemical stability and can provide continuous and stable protection for the positive electrode current collector under high temperature conditions, maintain the contact area between the positive electrode material and the current collector, improve the capacity retention rate of the battery under high temperature conditions, reduce the impedance growth rate, and improve battery performance.

[0049] The organic electrolyte salt added in the present invention can effectively improve the battery conductivity and cation migration number, thereby increasing the battery capacity. DETAILED DESCRIPTION

[0050] For ease of understanding, the battery electrolyte of the present invention will be described in more detail below, and examples of the present invention will be given, but the scope of the present invention is not limited thereby.

[0051] A sodium ion battery proposed in the present invention comprises a positive electrode containing copper elements, and an electrolyte containing an organic electrolyte salt and an additive, wherein the copper element in the positive electrode is distributed in the positive electrode active material and the current collector, and the additive comprises one or more of the boron-containing compounds A having the structure of formula I and / or formula II:

[0052]

[0053] Wherein, X is fluorine; R is selected from one of substituted or unsubstituted alkylene with 1 to 5 carbon atoms, substituted or unsubstituted halogenated alkylene with 1 to 5 carbon atoms, substituted or unsubstituted arylene with 6 to 10 carbon atoms, and substituted or unsubstituted halogenated arylene with 6 to 10 carbon atoms, and when substituted, the substituent is selected from hydroxyl, amino, nitro, cyano, carboxyl, acyl, thio, alkenyl, and alkynyl; r is selected from an integer of 0 to 2; p represents an integer of 0 to 4, and r+p satisfies the coordination number of B in formula I; q represents 0 or 1; Z1-Z4 are independently selected from oxygen or sulfur;

[0054] The sodium ion battery of the present invention satisfies 0.001≤a*(b+100c) / d≤0.3, 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, and 1%≤d≤12%, wherein a is the mass percentage of the additive (i.e., the boron-containing compound A) in the electrolyte, b is the mass percentage of the copper element in the positive electrode active material, c is the mass percentage of the copper element in the positive electrode current collector, and d is the mass percentage of the organic electrolyte salt in the electrolyte.

[0055] By introducing copper into the positive electrode active material and the positive electrode current collector, and using the boron-containing compound A as an additive, the present invention utilizes the interaction between the copper element and the boron-containing compound A to form a bidirectional dense passivation film from the inside out and from the outside in on the surface of the positive electrode current collector, effectively inhibiting the corrosion of the aluminum positive electrode current collector by the organic electrolyte salt in the non-aqueous electrolyte. The introduction of copper into the positive electrode active material also gives the positive electrode active material a reversible capacity, allowing the positive electrode material to repeatedly insert and remove sodium ions without damaging the structure or performance of the positive electrode material. At the same time, the introduction of copper into the positive electrode current collector can effectively enhance the strength of the positive electrode current collector and improve the toughness of the positive electrode current collector. When the copper element, boron-containing compound A and organic electrolyte salt introduced into the positive electrode active material and the positive electrode current collector meet the conditions: 0.001≤a*(b+100c) / d≤0.3, and 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, 1%≤d≤12%, the corrosion of the positive electrode current collector can be effectively inhibited and the battery cycle life can be significantly improved.

[0056] In the presence of copper, the boron-containing compound A can form a dense passivation film of copper-containing borates and fluorides with a mosaic structure on the surface of the aluminum alloy positive electrode current collector. Since the radius of boron ions and fluoride ions is small, the generated passivation film is dense and has high chemical and electrochemical stability, which can inhibit the corrosion of aluminum foil, protect the positive electrode current collector, and extend the service life of the battery.

[0057] Cu, as a variable valence transition metal element, provides reversible capacity for the positive electrode active material after being introduced into the positive electrode active material. 2+ During the first charge process, the positive electrode material can migrate to the current collector surface through electrolyte migration or solid-solid contact between the positive electrode material and the current collector, assisting compound A to form a dense passivation film from the outside to the inside, thereby inhibiting the corrosion of the aluminum foil.

[0058] For the positive electrode current collector introduced with copper element, the addition of copper element can enhance the mechanical properties of the positive electrode current collector material, and the copper element on the surface of the positive electrode current collector can also form a dense passivation film containing copper element from the inside out with compound A in the electrolyte during the first charging process, further protecting the positive electrode current collector and avoiding corrosion of the positive electrode current collector.

[0059] The present invention comprehensively considers the addition and distribution of the copper element and the reaction ability of the additive to the copper element under different distribution states, comprehensively considers the single effect of the addition amount of each component on the battery performance and the influence of the interaction relationship, constructs and reveals the influence of the addition amount of each component and the stoichiometric relationship on the formation of the passivation film, thereby successfully achieving a comprehensive improvement in the high-temperature electrochemical performance of the sodium ion battery through the optimization of the component relationship.

[0060] Specifically, we first ensured that the sodium-ion battery achieved the corresponding basic performance through the addition of copper elements and the use of additives by determining the single dosage of each component (0.1% ≤ a ≤ 5%, 0.5% ≤ b ≤ 12%, 0.01% ≤ c ≤ 0.1%, 1% ≤ d ≤ 12%). Further, the reaction of boron-containing compound A with the copper element in the positive electrode active material and the positive electrode current collector was affected by the corresponding content relationship and the distribution position of the copper element through a*(b+100c) / d. At the same time, the reaction degree was also related to the concentration of the organic electrolyte salt. We found that when the value of a*(b+100c) / d was 0.001≤a*(b+100c) / d≤0.3, the sodium-ion battery was able to obtain better high-temperature electrochemical performance. a*(b+100c) / d≤0.001 or 0.3≤a*(b+100c) / d may cause the content and distribution of the copper element in the boron-containing compound A and the positive electrode material to be mismatched, and it is impossible to construct a passivation film that is sufficient to adapt to the content of the organic electrolyte salt. The clear relationship between the copper content in the boron-containing compound A, the positive electrode active material and the positive electrode current collector and the organic electrolyte salt provides a theoretical basis for judging the decline in battery activity and life, and provides a theoretical basis for constructing a composite film with moderate thickness, density and efficiency. On the above basis, the appropriate mass ratio of each component material ensures the density and efficiency of the passivation film generated in the battery system, providing the premise and guarantee for obtaining a battery with improved comprehensive performance.

[0061] As some exemplary preferred embodiments, on the basis of ensuring 0.1% ≤ a ≤ 5%, 0.5% ≤ b ≤ 12%, 0.01% ≤ c ≤ 0.1%, and 1% ≤ d ≤ 12%, we preferably select the range of 0.002 ≤ a*(b + 100c) / d ≤ 0.1. The above preferred range is beneficial to further improving the synergistic optimization of the passivation film in maintaining cyclic stability and enhancing ion transport, and further reducing the impedance growth while ensuring high-temperature cyclic stability.

[0062] As some exemplary preferred embodiments, we preferably select the single dosage of each component (0.3% ≤ a ≤ 3.5%, 2% ≤ b ≤ 10%, 0.03% ≤ c ≤ 0.08%, 3% ≤ d ≤ 10%), and simultaneously preferably select the range of 0.005 ≤ a*(b + 100c) / d ≤ 0.015.

[0063] As a further embodiment, the positive electrode includes a positive electrode material layer and a positive electrode current collector containing copper elements.

[0064] As a still further embodiment, the positive electrode material layer includes a positive electrode active material containing copper elements, a positive electrode binder, and a positive electrode conductive agent.

[0065] As a further embodiment, the positive electrode active material containing copper elements is an O3-phase metal layered oxide containing copper elements. The general formula of the O3-phase metal layered oxide containing copper elements is Na x Cu y TM z O2, where 0.95 < x ≤ 1.05, 0.001 ≤ y ≤ 0.4, y + z = 1, and TM represents a transition metal element with unfilled d electron orbitals, specifically including one or more of scandium (Sc), yttrium (Y), lanthanide elements (from lanthanum (La) to lutetium (Lu)), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), and mercury (Hg).

[0066] As a further embodiment, in the positive electrode active material Na x Cu y TM z O2, 0.95 < x ≤ 1.05, 0.01 ≤ y ≤ 0.31, and y + z = 1.

[0067] As a further embodiment, the positive electrode active material Na x Cuy TM z In O₂, 0.95 < x ≤ 1.05, 0.02 ≤ y ≤ 0.19, y + z = 1, and TM includes Ni, Fe, and Mn.

[0068] As a further solution, the positive electrode active material containing copper element is Na x Cu y Ni a Fe b Mn c M d O₂, where 0.95 < x ≤ 1.05, 0.02 ≤ y ≤ 0.19, 0.2 ≤ a ≤ 0.34, 0.2 ≤ b ≤ 0.4, 0.2 ≤ c ≤ 0.4, 0 ≤ d ≤ 0.2, and a + b + c + d = 1, and M is one or more of scandium (Sc), yttrium (Y), lanthanide elements (from lanthanum (La) to lutetium (Lu)), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), technetium (Tc), rhenium (Re), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), mercury (Hg).

[0069] As a further solution, the positive electrode active material containing copper element includes NaCu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O₂.

[0070] As a further solution, the positive electrode binder includes at least one of a thermoplastic resin, an acrylic resin, sodium carboxymethyl cellulose, and styrene-butadiene rubber.

[0071] As a still further solution, the thermoplastic resin includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride, polytetrafluoroethylene, a copolymer of vinylidene fluoride - hexafluoropropylene, a copolymer of tetrafluoroethylene - hexafluoropropylene, a copolymer of tetrafluoroethylene - perfluoroalkyl vinyl ether, a copolymer of ethylene - tetrafluoroethylene, a copolymer of vinylidene fluoride - tetrafluoroethylene, a copolymer of vinylidene fluoride - trifluoroethylene, a copolymer of vinylidene fluoride - trichloroethylene, a copolymer of vinylidene fluoride - fluoroethylene, a copolymer of vinylidene fluoride - hexafluoropropylene - tetrafluoroethylene, thermoplastic polyimide, polyethylene, and polypropylene.

[0072] As a further solution, the acrylic resin includes at least one of an acrylic vinyl ester resin, an acrylic methyl ester resin, an acrylic butyl ester resin, an acrylic styrene resin, an acrylate resin, an acrylate copolymer resin, an acrylic resin, and an acrylic emulsion resin.

[0073] As a further embodiment, the positive electrode conductor includes a crystalline carbon material and an amorphous carbon material.

[0074] As a further solution, the crystalline carbon material includes at least one of conductive graphite, carbon nanotubes, graphene, and reduced graphene oxide.

[0075] As a further solution, the amorphous carbon material includes at least one of conductive carbon black, conductive carbon balls, and conductive carbon fibers.

[0076] As a further solution, the positive electrode current collector containing copper element is a metal foil layer containing copper element.

[0077] As a further solution, the metal in the metal foil layer containing copper element may include one or more of aluminum, zinc, magnesium, titanium and nickel.

[0078] As a further embodiment, in the structure of formula I and / or formula II of the boron-containing compound A, X is fluorine, R is selected from substituted or unsubstituted alkylene groups having 1 to 5 carbon atoms, substituted or unsubstituted halogenated alkylene groups having 1 to 5 carbon atoms, the substituents are selected from hydroxyl, amino, nitro, cyano, carboxyl, acyl, thiol, alkenyl, alkynyl, r is 0 or 2; p is selected from an integer of 0 or 4, and r+p is the coordination number of B in formula I; q is selected from 0 or 1; Z1-Z4 contain at least 1 sulfur, and the rest are oxygen.

[0079] As a further scheme, in the structure of formula I and / or formula II of the boron-containing compound A, X is fluorine, R is selected from alkylene and halogenated alkylene having 1 to 3 carbon atoms, r is 0 or 2; p is selected from an integer of 0 or 4, and r+p is the coordination number of B in formula I; q is 1; Z1-Z4 contain at least 1 sulfur, and the rest are oxygen.

[0080] As a further embodiment, the boron-containing compound A is selected from one or more of NaBF4 or compounds having a structural formula II in which Z1-Z4 contain at least one sulfur and the rest are oxygen.

[0081] As a further embodiment, the boron-containing compound A is selected from one or more of NaBF4 compound II, compound III, and compound IV.

[0082]

[0083] As a further solution, the additive may further include a second additive, and the second additive is a sulfate compound.

[0084] As a further solution, the second additive is a cyclic sulfate compound.

[0085] As a further embodiment, the cyclic sulfate ester compound includes at least one of vinyl sulfate, propylene sulfate, and vinyl methyl sulfate (VMS).

[0086] As a further solution, the content of the second additive in the electrolyte is 0.1%-2%.

[0087] As a further solution, the additive may further include a third additive, and the third additive is selected from at least one of sultone compounds, cyclic carbonate compounds, or fluorine-containing inorganic salt compounds.

[0088] As a further solution, the third additive contains an O=T structure, wherein T can be any one of P, S and C.

[0089] As a further embodiment, the sultone compound includes at least one of 1,3-propane sultone, 1,4-butane sultone, 1,3-propene sultone, and 1,3-propane sultone (PS).

[0090] As a further embodiment, the cyclic carbonate compound includes at least one of vinylene carbonate (VC), vinyl ethylene carbonate, methylene carbonate, fluoroethylene carbonate (FEC), trifluoromethylethylene carbonate, and bisfluoroethylene carbonate.

[0091] As a further solution, the fluorine-containing inorganic salt compound includes any one of sodium difluorophosphate (NaPO2F2) and sodium fluorosulfonate (NaFSO3).

[0092] As a further solution, the content of the third additive in the electrolyte is 0.1%-1.5%.

[0093] As a further solution, the electrolyte also includes an inorganic electrolyte salt, an organic electrolyte salt and a solvent. The non-polar electrolyte salt is usually composed of an inorganic anion and a sodium cation. These salts usually have a higher melting point and a lower solubility in an organic solvent when in a solid state. Therefore, the sodium battery using the non-polar electrolyte salt is usually more stable at high temperature, but the non-polar electrolyte salt may react with the positive electrode material or solvent under high temperature and high voltage conditions, causing a decrease in the performance of the sodium battery. In contrast, the organic electrolyte salt composed of organic anions and sodium cations has good compatibility with organic solvents, and can provide higher conductivity and cation migration number when used as a battery electrolyte, but the organic electrolyte salt anion cannot form a dense passivation film on the surface of the positive electrode current collector, so it may cause corrosion of the current collector. The present invention combines an organic electrolyte with an inorganic electrolyte, and constructs a composite passivation film on the surface of the positive electrode current collector by using a boron-containing compound A and the copper element in the positive electrode, which ensures thermal stability while avoiding the corrosion of the organic electrolyte to the positive electrode current collector, and fully improves the performance of the sodium battery.

[0094] As a further embodiment, the inorganic electrolyte salt is substituted with fluorine.

[0095] As yet a further aspect, the inorganic electrolyte salt includes NaPF6.

[0096] As a further solution, the content of NaPF6 in the electrolyte is 1%≤NaPF6≤15%.

[0097] As a further solution, the content of NaPF6 in the electrolyte is 3%≤NaPF6≤10%. When 3%≤NaPF6≤10%, the ion conductivity in the electrolyte can be further improved, the high temperature stability of the high temperature sodium battery can be enhanced, and the battery performance can be improved.

[0098] As a further embodiment, the organic electrolyte salt includes at least one of an organic sulfonyl sodium salt and an organic phosphate sodium salt.

[0099] As a further embodiment, the organic sulfonyl sodium salt includes at least one of sulfonimide sodium salt, sulfonic acid sodium salt, sulfonyl chloride sodium salt, sulfonamide sodium salt, sulfonic acid ester sodium salt, sulfonylurea sodium salt, and sulfonamide methyl ester sodium salt.

[0100] As a further embodiment, the organic sulfonyl sodium salt includes at least one of sulfonimide sodium salt and sulfonic acid sodium salt.

[0101] As a further embodiment, the organic sulfonyl sodium salt is fluorinated or substituted with fluorine.

[0102] As a further embodiment, the number of fluorine substitutions in the organic sulfonyl sodium salt molecule is preferably 3 or more.

[0103] As a further embodiment, the sodium sulfonyl imide salt includes at least one of sodium bis(trifluoromethanesulfonyl)imide, sodium bis(pentafluoroethanesulfonyl)imide, sodium bis(perfluorobutanesulfonyl)imide, sodium bis(perfluorohexanesulfonyl)imide, sodium bis(pentafluoroethylsulfonyl)imide, and sodium bis(fluorosulfonyl)imide.

[0104] As a further embodiment, the sodium sulfonate salt includes at least one of trifluoromethanesulfonic acid sodium salt, pentafluoroethanesulfonic acid sodium salt, and perfluorooctanesulfonic acid sodium salt.

[0105] As a further embodiment, the organic sodium phosphate salt includes at least one of sodium phosphate esters, sodium phosphate diesters, sodium phosphate triesters, sodium polyphosphate, and sodium oxalate phosphate.

[0106] As a further embodiment, the sodium oxalate phosphate salt includes at least one of sodium oxalate phosphate, sodium difluorobisoxalate phosphate, and sodium tetrafluorooxalate phosphate.

[0107] As a further solution, the content of the organic electrolyte salt in the electrolyte is 5%-10%.

[0108] As a further solution, the solvent includes at least one of a linear carbonate solvent, a carboxylate solvent, and a phosphate solvent.

[0109] As a further embodiment, the linear carbonate solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate and methyl propyl carbonate.

[0110] As a further embodiment, the carboxylic acid ester solvent includes at least one of methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, methyl isobutyrate, ethyl butyrate, methyl trimethylacetate and ethyl trimethylacetate.

[0111] As a further embodiment, the phosphate solvent includes at least one of trimethyl phosphate, triethyl phosphate, tripropyl phosphate, triphenyl phosphate, tris(2,2,2-trifluoroethyl)phosphite and ethoxy(pentafluoro)cyclotriphosphazene.

[0112] The sodium ion battery provided by the present invention also includes a negative electrode and a separator.

[0113] As a further solution, the negative electrode includes a negative electrode material layer and a negative electrode current collector, and the negative electrode material layer is formed on the surface of the negative electrode current collector.

[0114] As a further solution, the negative electrode material layer includes a negative electrode active material, a negative electrode binder, a negative electrode conductor and a thickener.

[0115] As a further solution, the negative electrode active material includes at least one of a carbon-based material, a titanium-based material, an alloy material and an organic compound material.

[0116] As a further aspect, the carbon-based material includes a crystalline carbon-based material and an amorphous carbon-based material.

[0117] As a further solution, the crystalline carbon-based material includes graphite and graphene. Graphite is preferred in the present invention, and when used with a positive electrode sheet of a sodium transition metal oxide positive electrode active material, the sodium ion battery can have high conductivity and structural stability.

[0118] As a further solution, the amorphous carbon-based material includes hard carbon, soft carbon, carbon nanotubes, carbon black and carbon aerogel.

[0119] As a further solution, the type of the negative electrode binder is not limited, and technicians can choose it according to actual needs, including at least one of styrene butadiene rubber (SBR), styrene-butadiene rubber, water-based acrylic resin and carboxymethyl cellulose (CMC).

[0120] As a further solution, the type of the negative electrode conductive agent is not limited, and technicians can choose according to actual needs, including at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, conductive carbon black and carbon nanofibers.

[0121] As a further solution, the negative electrode current collector is selected from any one of a metal material capable of conducting electrons, a carbon-coated metal foil or a porous metal plate.

[0122] As a further solution, the metal material capable of conducting electrons used as the negative electrode current collector is a metal foil layer, and the metal of the foil layer includes at least one of aluminum, nickel, tin, copper and stainless steel, preferably copper or aluminum.

[0123] As a further solution, the type of thickener is not limited, and technicians can choose according to actual needs, such as using carboxymethyl cellulose as a thickener.

[0124] As a further solution, the average pore radius distribution range of the negative electrode material layer is 0.01 to 100 μm.

[0125] As a further solution, the present invention does not specifically limit the type of diaphragm, and any known porous structure diaphragm with electrochemical stability and mechanical stability can be selected according to actual needs. For example, it can be a single-layer or multi-layer film containing at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride (PVDF).

[0126] As a further solution, the thickness of the separator is 6 to 12 μm.

[0127] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0128] The chemical raw materials involved in the following examples and comparative examples are all prior art and are commercially available. The experimental devices, test devices, etc. involved in the following examples and comparative examples are all conventional devices in the art, without special requirements and limitations.

[0129] Example 1

[0130] This embodiment provides a sodium ion battery, the sodium ion battery comprising a positive electrode, a negative electrode, a separator and a non-aqueous electrolyte;

[0131] The positive electrode includes a positive electrode material layer and a positive electrode current collector containing copper elements, and the positive electrode material layer includes a positive electrode active material NaCu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2, conductive carbon black Super-P, binder polyvinylidene fluoride (PVDF). The positive electrode current collector is aluminum alloy, and the pore radius distribution range of the positive electrode sheet is 5μm;

[0132] The negative electrode includes a negative electrode material layer and a negative electrode current collector copper foil, the negative electrode material layer includes negative electrode active material graphite, conductive carbon black Super-P, binder styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC), and the average pore radius distribution range of the negative electrode sheet is 50 μm;

[0133] Preparation of the electrolyte: Ethylene carbonate and ethyl methyl carbonate are mixed in a volume ratio of 1:1, and then an electrolyte salt is added to the mixed solvent to a mass concentration as described in the table, and then compound A and the remaining additives are added to obtain the electrolyte;

[0134] Preparation of positive electrode: Mix NaCu in a mass ratio of 97:1.5:1.5 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 O2, Super-P and PVDF are then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the surface of an aluminum foil containing copper elements, and after drying, rolling and vacuum drying, an aluminum lead wire is welded with an ultrasonic welder to obtain a positive electrode sheet;

[0135] Preparation of negative electrode: Graphite, Super-P, SBR and CMC are mixed in a mass ratio of 94:1.5:3:1.5, and then dispersed in deionized water to obtain negative electrode slurry; the negative electrode slurry is coated on both sides of copper foil, and after drying, rolling and vacuum drying, a nickel lead wire is welded with an ultrasonic welder to obtain a negative electrode sheet;

[0136] Preparation of battery cells: A separator with a thickness of 8 μm is placed between the positive electrode sheet and the negative electrode sheet, and then the sandwich structure consisting of the positive electrode sheet, the negative electrode sheet and the separator is wound, and then the wound body is flattened and placed in an aluminum foil packaging bag, and vacuum baked at 75°C for 48 hours to obtain a battery cell to be injected with liquid;

[0137] In a glove box with water and oxygen contents below 20ppm and 50ppm respectively, the electrolyte was injected into the battery cell, and after vacuum packaging, it was left at 45°C for 24h; then the conventional formation of the first charge was carried out according to the following steps: 0.1C constant current charging for 180min, 0.2C constant current charging for 120min, after aging at 45°C for 48h, the battery was vacuum sealed for the second time, and then further charged to 4.0V at a constant current of 0.2C, and discharged to 2V at a constant current of 0.2C.

[0138] The type and content of the above boron-containing compound A, the type and content of the second additive, the third additive, or \ and, the Cu element content in the positive electrode material, the Cu element content in the positive electrode current collector, the type and content of the organic electrolyte salt, and the a*(b+100c) / d value are shown in Table 1.

[0139] Example 2-16

[0140] A sodium battery was prepared by changing some parameters in Example 1 and the rest of the parameters were the same as in Example 1. The parameter changes and results are listed in Table 1.

[0141] Comparative Example 1

[0142] A sodium battery was prepared by changing some parameters in Example 1 and the rest of the parameters were the same as in Example 1. The parameter changes and results are listed in Table 2.

[0143] The sodium ion batteries prepared in the embodiments and comparative examples were repeatedly charged at 1C CCCV between 2-4V and then discharged at 1CCC at a high temperature of 45°C for charge-discharge cycle performance testing. The discharge capacity retention rate and impedance growth rate of the battery at high temperature were calculated according to the following formula:

[0144] Capacity retention rate after 500 cycles at 45℃ = 500th discharge capacity at 45℃ / first cycle discharge capacity × 100%;

[0145] Impedance growth rate after 500 cycles at 45°C = (discharge DCIR after 500 cycles at 45°C - discharge DCIR after the first cycle at 45°C) / discharge DCIR after the first cycle at 45°C × 100%;

[0146] The test results obtained for Examples 1 to 27 and Comparative Examples 1 to 16 are shown in Table 2.

[0147] Table 1

[0148]

[0149]

[0150]

[0151]

[0152] Table 2

[0153]

[0154]

[0155]

[0156] From Examples 1-9 and Comparative Examples 1-8, it can be observed that when 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, and 1%≤d≤12% are satisfied in the positive electrode of the battery, the battery has a capacity retention rate of more than 86% after 500 cycles at 45°C, and an impedance growth rate of less than 60%. This indicates that satisfying 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, and 1%≤d≤12% is a prerequisite for improving the performance of sodium batteries. From Examples 10-11 and Comparative Examples 9-16, it can be seen that when 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, and 1%≤d≤12% are satisfied, it is also necessary to ensure that 0.001≤a*(b+100c) / d≤0.3. When a*(b+100c) / d>0.3, the excessive boron-containing compound A will cause the battery to react more easily in subsequent cycles to consume active sodium, and form a thicker passivation film with the copper element, which may also be excessive, to enhance impedance. Therefore, it can be observed in Comparative Examples 9-12 that the impedance growth rate exceeds 120% when a*(b+100c) / d>0.3 compared with a*(b+100c) / d<0.001. Comparative Examples 13-16 show that when a*(b+100c) / d<0.001, the copper content of the compound A in the non-aqueous electrolyte or the positive electrode active material and the current collector is insufficient to support the passivation film formed by the compound A on the surface of the positive electrode current collector from the inside out and from the outside in, or it is difficult to form a uniform passivation film, resulting in a rapid deterioration of the capacity retention rate. After 500 cycles at 45°C, the capacity retention rate is only maintained at about 70%. On the other hand, a*(b+100c) / d<0.001 may also mean that the passivation film generated by the excessively high organic electrolyte salt content in the sodium battery is difficult to resist the corrosion of the organic electrolyte salt, resulting in a deterioration in the capacity retention rate. Therefore, the calculation of a*(b+100c) / d has important practical value for the design of sodium battery performance.

[0157] According to Examples 1-9 relative to Examples 10 and 11, when 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, 1%≤d≤12% are satisfied, 0.002≤a*(b+100c) / d≤0.1 may be preferred.

[0158] According to Example 1, 0.3%≤a≤3.5%, 2%≤b≤10%, 0.03%≤c≤0.08%, and 3%≤d≤10% can be preferably selected. On the basis of satisfying the above conditions, according to Example 2, 0.005≤a*(b+100c) / d≤0.015 is further preferred, which is beneficial to further improve the capacity retention rate after 500 cycles at 45°C and reduce the impedance growth rate. By synergistically optimizing the ion transfer efficiency and the performance of the composite passivation film, the impedance growth rate is significantly reduced, the capacity retention rate is improved, and the performance of the sodium battery is enhanced.

[0159] Examples 1, 12-16 show the effects of different boron-containing compounds A on the performance of sodium batteries. First, after 500 cycles at 45°C, the capacity retention rate of Example 1 is only 89.50%, and the impedance growth rate is 41.3%, indicating that when NaDFOB is used as an additive, the performance of the sodium battery is lower than that of Examples 12-15; According to Examples 15-16, it can be observed that after 500 cycles at 45°C, the capacity retention rate of NaBF4 reaches 90.7%, and the impedance growth rate is only 33.7%, which is better than NaBOB with the same structure I. This may be because NaBF4 is more stable in the electrolyte than NaBOB, and can cooperate with copper elements to form a denser passivation film on the surface of the positive current collector during the charge and discharge process of the sodium battery. It is observed that Compound II, Compound III, and Compound IV containing at least one sulfur in Examples 1, 12-14, and Z1-Z4 have higher capacity retention (>90%) and lower impedance growth rate (<35%) after 500 cycles at 45°C. This may be because the sulfur element can not only participate in the formation of a composite passivation film, but also provide an additional ion transmission path to reduce the impedance of the battery, thereby improving the battery performance.

[0160] Examples 22-27 also compare the capacity retention rate and impedance growth rate of the sodium battery after 500 cycles at 45°C when the second and third additives are added. Compared with Example 1, Example 22 with the addition of the second additive VMS shows a lower impedance growth rate, which may be due to the presence of the cyclic structure in the cyclic sulfate compound, which makes it have higher oxidation stability, thereby improving the stability of the sodium battery; at the same time, the cyclic structure can also optimize the composite passivation film interface, further improve the stability and corrosion resistance of the composite passivation film, thereby improving the cycle stability and life of the battery. On the basis of the presence of the second additive in the electrolyte, the third additive is continued to be added, and the performance of the sodium battery after 500 cycles at 45°C is further increased. At the same time, Examples 23-27 with the second and third additives show a higher capacity retention rate (≥92%) and a lower impedance growth rate (≤27.5%) as a whole. This may be because the addition of the third additive containing the O=T structure not only enhances the synergistic effect between the boron-containing compound A and the copper element, but also cooperates with the cyclic sulfate compound to participate in the construction of the composite passivation film, thereby reducing the impedance and improving the capacity retention rate.

[0161] Examples 1, 17-19 demonstrate the effect of the type of organic electrolyte salt in the electrolyte on the performance of sodium batteries. When the types of organic electrolyte salts in the electrolyte are NaTFSI, NaBETI, and NaCF3SO3, an impedance growth rate of about 28% and a capacity retention rate of about 92% can be obtained when 0.001≤a*(b+100c) / d≤0.3, 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, and 1%≤d≤12% are met. This may be due to the presence of at least one trifluoromethyl group in NaTFSI, NaBETI, and NaCF3SO3. Compared with NaFSI, organic salts with trifluoromethyl groups generally have higher ionic conductivity, which can effectively improve the charge and discharge efficiency of the battery and reduce impedance growth.

[0162] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-described embodiments are exemplary and cannot be understood as limitations of the present invention. Those of ordinary skill in the art can change, modify, replace and deform the above-described embodiments within the scope of the present invention. In addition, those of ordinary skill in the art can combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.

[0163] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-described embodiments are exemplary and cannot be understood as limitations of the present invention. Those of ordinary skill in the art can change, modify, replace and deform the above-described embodiments within the scope of the present invention. In addition, those of ordinary skill in the art can combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.

Claims

1. A sodium ion battery, characterized in that: The invention comprises a positive electrode containing copper elements, and an electrolyte containing an organic electrolyte salt and an additive, wherein the copper elements in the positive electrode are distributed in the positive electrode active material and the current collector, and the additive comprises one or more boron-containing compounds A having a structure of formula I and / or formula II: Wherein, X is fluorine; R is selected from one of substituted or unsubstituted alkylene with 1 to 5 carbon atoms, substituted or unsubstituted halogenated alkylene with 1 to 5 carbon atoms, substituted or unsubstituted arylene with 6 to 10 carbon atoms, and substituted or unsubstituted halogenated arylene with 6 to 10 carbon atoms, and when substituted, the substituent is selected from hydroxyl, amino, nitro, cyano, carboxyl, acyl, thio, alkenyl, and alkynyl; r is selected from an integer of 0 to 2; p represents an integer of 0 to 4, and r+p satisfies the coordination number of B in formula I; q represents 0 or 1; Z1-Z4 are independently selected from oxygen or sulfur; The sodium ion battery satisfies 0.001≤a*(b+100c) / d≤0.3, 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, 1%≤d≤12%, wherein a is the mass percentage of the additive (i.e., the boron-containing compound A) in the electrolyte, b is the mass percentage of the copper element in the positive electrode active material, c is the mass percentage of the copper element in the positive electrode current collector, and d is the mass percentage of the organic electrolyte salt in the electrolyte.

2. The sodium ion battery according to claim 1, characterized in that The a, b, c, and d also satisfy 0.1%≤a≤5%, 0.5%≤b≤12%, 0.01%≤c≤0.1%, 1%≤d≤12%, and 0.002≤a*(b+100c) / d≤0.1; Further preferably, it is characterized in that the sodium ion battery satisfies 0.3%≤a≤3.5%, 2%≤b≤10%, 0.03%≤c≤0.08%, 3%≤d≤10%, and 0.005≤a*(b+100c) / d≤0.

015.

3. The sodium ion battery according to claim 1, characterized in that: The positive electrode containing copper element comprises a positive electrode material layer and a positive electrode current collector containing copper element; Further preferably, it is characterized in that the positive electrode material layer comprises a positive electrode active material containing copper element, a positive electrode binder and a positive electrode conductive agent; Further preferably, it is characterized in that the positive electrode binder includes at least one of thermoplastic resin, acrylic resin, sodium carboxymethyl cellulose and styrene butadiene rubber; Further preferably, it is characterized in that the positive electrode conductor includes crystalline carbon material and amorphous carbon material.

4. The copper-containing positive electrode active material according to claim 3, characterized in that: The positive electrode active material containing a copper element is an O3-phase metal layered oxide containing a copper element. The general formula of the O3-phase metal layered oxide containing a copper element is Na x Cu y TM z O2, where 0.95 < x ≤ 1.05, 0.001 ≤ y ≤ 0.4, y + z = 1, and TM represents a transition metal element with unfilled d electron orbitals, specifically including one or more of scandium (Sc), yttrium (Y), lanthanide elements (from lanthanum (La) to lutetium (Lu)), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), technetium (Tc), rhenium (Re), iron (Fe), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), nickel (Ni), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), mercury (Hg); Further preferably, it is characterized in that the positive electrode active material containing copper element Na x Cu y TM z O2 0.95 <x≤1.05,0.01≤y≤0.31,y+z=1; More preferably, it is characterized in that in the positive electrode active material Na x Cu y TM z O2, 0.95 < x ≤ 1.05, 0.02 ≤ y ≤ 0.19, y + z = 1, and TM includes Ni, Fe, and Mn; Further preferably, it is characterized in that the positive electrode active material of copper element is Na x Cu y Ni a Fe b Mn c M d O2, where 0.95 < x ≤ 1.05, 0.02 ≤ y ≤ 0.19, 0.2 ≤ a ≤ 0.34, 0.2 ≤ b ≤ 0.4, 0.2 ≤ c ≤ 0.4, 0 ≤ d ≤ 0.2, and a + b + c + d = 1, and M is one or more of scandium (Sc), yttrium (Y), lanthanide elements (from lanthanum (La) to lutetium (Lu)), titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), technetium (Tc), rhenium (Re), ruthenium (Ru), osmium (Os), cobalt (Co), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), mercury (Hg).

5. The copper-containing positive electrode current collector according to claim 3 is a metal foil layer containing copper elements; More preferably, it is characterized in that The metal in the copper-containing metal foil layer may include one or more of aluminum, zinc, magnesium, titanium, and nickel.

6. The sodium ion battery according to claim 1, characterized in that: The additive comprises a boron-containing compound A having a structure of formula I and / or formula II, wherein X is fluorine, R is selected from a substituted or unsubstituted alkylene group having 1 to 5 carbon atoms, a substituted or unsubstituted halogenated alkylene group having 1 to 5 carbon atoms, the substituent is selected from a hydroxyl group, an amino group, a nitro group, a cyano group, a carboxyl group, an acyl group, a thiol group, an alkenyl group, an alkynyl group, r is 0 or 2; p is selected from an integer of 0 or 4, and r+p is the coordination number of B in formula I; q is selected from 0 or 1; Z1-Z4 contains at least one sulfur, and the rest are oxygen; Further preferably, in the boron-containing compound A having the structure of formula I and / or formula II, X is fluorine, R is selected from an alkylene group or a halogenated alkylene group having 1 to 3 carbon atoms, r is 0 or 2; p is selected from an integer of 0 or 4, and r+p is the coordination number of B in formula I; q is 1; Z1-Z4 contains at least one sulfur, and the rest are oxygen; Further preferably, the boron-containing compound A is selected from one or more of NaBF4 or a compound having a structural formula II in which Z1-Z4 contains at least one sulfur and the rest is oxygen.

7. The sodium ion battery according to claim 1, characterized in that: The electrolyte may further include a second additive, a sulfate compound; Further preferably, the second additive comprises a cyclic sulfate compound; More preferably, the content of the second additive in the electrolyte is 0.1%-2%.

8. The sodium ion battery according to claim 1, characterized in that: The electrolyte may further include a third additive; More preferably, the third additive is selected from at least one of sultone compounds, cyclic carbonate compounds, or fluorine-containing inorganic salt compounds; Further preferably, the third additive is characterized in that the third additive comprises an O=T structure, wherein T can be any one of P, S and C; More preferably, the content of the third additive in the electrolyte is 0.1%-1.5%.

9. The sodium ion battery according to claim 1, characterized in that: The electrolyte solution also includes an inorganic electrolyte salt, an organic electrolyte salt and a solvent; Further preferably, the inorganic electrolyte salt is substituted with fluorine; Further preferably, the inorganic electrolyte salt comprises NaPF6; Further preferably, the content of NaPF6 in the electrolyte is 1%≤NaPF6≤15%; Further preferably, the content of NaPF6 in the electrolyte is 3%≤NaPF6≤10%; Further preferably, the organic electrolyte salt comprises at least one of an organic sulfonyl sodium salt and an organic phosphate sodium salt; More preferably, the organic sulfonyl sodium salt includes at least one of sulfonimide sodium salt, sulfonic acid sodium salt, sulfonyl chloride sodium salt, sulfonamide sodium salt, sulfonic acid ester sodium salt, sulfonylurea sodium salt, and sulfonamide methyl ester sodium salt; More preferably, the organic sulfonyl sodium salt includes sulfonimide sodium salt and sulfonic acid sodium salt; Further preferably, the organic sulfonyl sodium salt is fluorinated or substituted with fluorine; More preferably, the number of fluorine substitutions in the organic sulfonyl sodium salt molecule is 3 or more; More preferably, the content of the organic electrolyte salt in the electrolyte is 5%-10%.

10. The sodium ion battery according to claim 1, characterized in that: The solvent includes at least one of a chain carbonate solvent, a carboxylate solvent, and a phosphate solvent.