Composite pole piece, preparation method thereof and solid-state battery

By using composite electrode sheets in solid-state batteries, the continuous structure of halide solid electrolyte and hot pressing treatment technology are used to solve the problem of poor contact performance between electrodes and solid electrolytes in solid-state batteries, and the battery's magnification and cycling performance are significantly improved. And enhanced security.

CN119069633AActive Publication Date: 2024-12-03SUZHOU QINGTAO NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411270181.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-03
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The poor interface contact between the solid electrolyte and the electrode in a solid-state battery leads to an increase in internal resistance, affecting the rate performance and cycling performance of the battery.

Method used

Using composite electrode sheets, including current collector layer and active layer, halide solid electrolyte is added to the active layer to convert it from solid state to liquid state and then to solid state, forming a continuous structure, improving the lithium ion transmission path, and optimizing through hot pressing treatment Extreme sheet structure.

Benefits of technology

Significantly reduce the internal resistance of the battery, improve rate performance and cycling performance, improve the interface contact between the electrode and the solid electrolyte layer, and enhance the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069633A_ABST
    Figure CN119069633A_ABST
Patent Text Reader

Abstract

The invention provides a composite pole piece, a preparation method thereof and a solid-state battery, and relates to the technical field of energy storage. The composite pole piece comprises a current collector layer and an active layer formed on the current collector layer, the active layer comprises an active material and halide solid-state electrolyte, the halide solid-state electrolyte comprises Li3MCl6-xBrx, the second halide solid-state electrolyte is converted from a solid state to a liquid state and then converted from the liquid state to the solid state, the surface roughness of the composite pole piece is 1.5-30 [mu] m, and the surface roughness of the composite pole piece is 1.5-30 [mu] m. On one hand, a continuous conduction channel of lithium ions can be formed, the transmission capability of the lithium ions is improved, and the electrochemical performance of the solid-state battery is improved, and on the other hand, the interface contact between the composite pole piece and the solid-state electrolyte layer can be effectively improved, and the internal resistance of the battery is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to a composite pole piece and a preparation method thereof, and a solid-state battery. Background Art

[0002] Solid-state batteries are energy storage elements that can store electrical energy and release it when needed. Compared with traditional liquid batteries, solid-state batteries use solid electrolytes instead of liquid or gel electrolytes for ion transmission, and have higher safety, higher energy density, faster charging speed and longer cycle life.

[0003] In solid-state batteries, the solid electrolyte is located between the positive electrode and the negative electrode, and lithium ions are deintercalated from the positive electrode and transferred through the electrolyte to the negative electrode.

[0004] However, solid-state batteries still face some difficulties in their full commercial use. On the one hand, solid electrolytes replace electrolytes as the transmission medium for lithium ions in batteries. Compared with the liquid-solid contact between electrolytes and electrodes to form a good interface contact, solid electrolytes are often granular and have "point-to-point" solid-solid contact with electrodes, which increases the internal resistance of the battery and is not conducive to the use of battery capacity. On the other hand, traditional positive and negative electrodes are often porous electrodes, and the electrolyte has fluidity. The electrolyte establishes a lithium ion transmission path inside the positive and / or negative electrodes by wetting the electrodes. However, the solid electrolyte is solid and cannot wetting the electrodes. Even if solid electrolyte particles are added to the electrodes in the prior art, the battery performance is affected due to the limitations of the ionic conductivity of the solid electrolyte and the solid-solid contact between the active material particles and the solid electrolyte particles. Summary of the invention

[0005] Based on this, it is necessary to provide a composite electrode sheet and its preparation method, and a solid-state battery, which can effectively improve the interface contact performance between the electrode and the solid electrolyte layer, reduce the internal resistance of the battery, and enhance the lithium ion transmission capacity inside the electrode sheet and inside the battery, thereby improving the battery's rate performance and cycle performance.

[0006] In a first aspect, the present application provides a composite pole piece, the composite pole piece comprising a current collector layer and an active layer formed on the current collector layer, the active layer comprising an active material and a halide solid electrolyte, wherein the second halide solid electrolyte is transformed from a solid state to a liquid state, and then transformed from a liquid state to a solid state;

[0007] The surface roughness of the composite pole piece is 1.5 μm to 30 μm.

[0008] In some embodiments, the halide solid electrolyte includes Li3MCl 6-x Br x, at least part of Li3MCl 6-x Br x A continuous structure is formed in the active layer, wherein M is a trivalent metal element and x satisfies 0<x<6.

[0009] In some embodiments, the melting point of the halide solid electrolyte is 80°C to 200°C.

[0010] In some embodiments, M is selected from Ga 3+ 、In 3+ 、Al 3+ , Fe 3+ , Y 3+ Sc 3+ 、Bi 3+ , one or more trivalent lanthanide metals, and the value range of x is 2≤x≤5.

[0011] In some of the embodiments, the porosity of the composite pole piece is 0.1% to 10%.

[0012] In some embodiments, the Li3MCl 6-x Br x The ionic conductivity λ satisfies λ ≥ 1 mS / cm.

[0013] In some embodiments, the content of the halide solid electrolyte in the active layer increases in sequence along a direction away from the current collector layer.

[0014] In some embodiments, the composite pole piece includes a first pole layer and multiple second pole layers, the first pole layer includes an active material, and the second pole layer includes an active material and the halide solid electrolyte; wherein the first pole layer is formed on the composite pole piece, and the second pole layer is formed on the first pole layer.

[0015] In some embodiments, the composite electrode is a composite positive electrode, and the mass proportion of the halide solid electrolyte in the active layer is 5% to 40%; or,

[0016] The composite electrode is a composite negative electrode, and in the active layer, the mass proportion of the halide solid electrolyte is 8% to 50%.

[0017] In a second aspect, the present application further provides a method for preparing a composite electrode, the method comprising:

[0018] Prepare a pole piece precursor; the pole piece precursor comprises a current collector layer and an active layer, and the active layer comprises an active material and a halide solid electrolyte;

[0019] The electrode precursor is subjected to hot pressing treatment to obtain a composite electrode; wherein the temperature of the hot pressing treatment is greater than or equal to the melting point temperature of the halide solid electrolyte.

[0020] In some embodiments, the temperature of the hot pressing treatment is 80° C. to 200° C.; and / or, the time of the hot pressing treatment is 0.5 min to 30 min; and / or, the pressure of the hot pressing treatment is 10 MPa to 500 MPa.

[0021] In a third aspect, the present application also provides a solid-state battery, which includes the composite pole piece.

[0022] Beneficial technical effects

[0023] The composite electrode provided by the present application includes active electrode materials and halide solid electrolytes. On the one hand, the halide solid electrolyte changes from liquid to solid in the active layer, and the liquid halide solid electrolyte can penetrate into the active layer. At the same time, thanks to the high ionic conductivity of the halide solid electrolyte, a continuous and high-speed lithium ion transmission path can be formed inside the positive electrode or the negative electrode, thereby significantly improving the battery rate performance. On the other hand, the halide solid electrolyte can be transformed from liquid to solid to make its density significantly high, so that when forming a composite electrode with the positive or negative active material, the surface density of the composite electrode is significantly improved, and the roughness is significantly reduced, which can effectively improve the interface contact between the composite electrode and the solid electrolyte layer, and effectively reduce the internal resistance of the battery; when the composite electrode is a composite negative electrode, the improvement of the surface roughness is conducive to reducing the uneven deposition of lithium ions on the negative electrode side, effectively preventing the generation and growth of lithium dendrites, and improving the safety performance of the battery.

[0024] The present application forms a mass ratio gradient of the halide solid electrolyte on the electrode side, so as to maintain the energy density of the battery while making full use of the compactness of the halide solid electrolyte to improve the interface performance between the composite electrode and the solid electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] FIG. 1 is a schematic diagram of a method for preparing a composite electrode according to an embodiment. DETAILED DESCRIPTION

[0026] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0027] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0028] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0029] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0030] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0031] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0032] If there is no special explanation, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps S12 and S14, which means that the method may include steps S12 and S14 performed sequentially, or may include steps S14 and S12 performed sequentially. For example, it is mentioned that the method may also include step S16, which means that step S16 may be added to the method in any order, for example, the method may include steps S12, S14 and S16, or may include steps S12, S16 and S14, or may include steps S16, S12 and S14, etc.

[0033] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0034] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0035] All-solid-state batteries have higher safety and higher energy density than liquid batteries. However, since all-solid-state batteries use a membrane made of solid electrolyte powder as a medium for lithium ion transmission, the solid-state characteristics affect the contact between the solid electrolyte and the electrode and the conduction of lithium ions, resulting in a high internal resistance of the prepared battery and poor rate performance and cycle performance. Due to the poor fluidity of the solid electrolyte powder in the all-solid-state battery, there are gaps between the particles, and the lithium ion transmission path is discontinuous, which reduces the lithium ion transmission efficiency, thereby causing the performance of the all-solid-state battery to decline.

[0036] The present application provides a composite pole piece, which includes a current collector layer and an active layer formed on the current collector layer, wherein the active layer includes an active material and a halide solid electrolyte, wherein the second halide solid electrolyte changes from a solid state to a liquid state, and then changes from a liquid state to a solid state.

[0037] In the present application, by adding a halide solid electrolyte into the active layer, the halide solid electrolyte changes from liquid to solid in the active layer, which can effectively improve the surface roughness of the composite electrode and reduce the internal resistance of the battery. At the same time, the rate performance of the battery is also significantly improved.

[0038] One possible guess is that the existing electrode and the solid electrolyte layer usually show point-to-point contact between particles, while in the present application, the halide solid electrolyte changes from liquid to solid in the active layer, and the liquid halide solid electrolyte can penetrate into various places in the active layer, adhere to the surface of the active material particles, and / or fill in the pores between the active material particles to form a continuous structure. At the same time, thanks to the high ionic conductivity of the halide solid electrolyte, a continuous and high-speed lithium ion transmission path can be formed inside the positive electrode or the negative electrode, thereby significantly improving the battery rate performance. On the other hand, the transformation of the halide solid electrolyte from liquid to solid can make its density significantly high, so that when forming a composite electrode with the positive or negative active material, the surface density of the composite electrode is significantly improved, and the roughness is significantly reduced. After the surface roughness is improved, the surface of the composite electrode is smoother, and there are more contact points between the composite electrode and the solid electrolyte layer, which can effectively improve the interface contact between the composite electrode and the solid electrolyte layer, and effectively reduce the internal resistance of the battery. The above is only a possible speculation on the mechanism of the technical solution of the present application and does not constitute a limitation on the protection scope of the present application.

[0039] The surface roughness of the composite pole piece is 1.5 μm to 30 μm. The surface roughness of the composite pole piece may be, but is not limited to, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 5 μm, 8 μm, 10 μm, 15 μm, 18 μm, 20 μm, 25 μm or 30 μm. Within the above range, the composite pole piece can be well combined with the solid electrolyte layer, optimizing the interface between the pole piece and the solid electrolyte layer. Further, the surface roughness of the composite pole piece may be 5 μm to 20 μm.

[0040] In some embodiments, the halide solid electrolyte comprises Li3MCl 6-x Br x , at least part of Li3MCl 6-x Br x A continuous structure is formed in the active layer, wherein M is a trivalent metal element and x satisfies 0<x<6.

[0041] In some preferred embodiments, M is selected from Ga 3+ 、In 3+ 、Al 3+ , Fe 3+ , Y 3+ Sc 3+ 、Bi 3+ , one or more of trivalent lanthanide metals, and the value range of x is 2≤x≤5. For example, Li3MCl 6-x Br x It can be but not limited to Li3Y 0.5 Dy 0.5 Cl3Br3、Li3In 0.5 Fe 0.5 Cl3Br3, Li3YCl3Br3.

[0042] In some embodiments, the melting point of the halide solid electrolyte is 80°C-200°C.

[0043] In some embodiments, the porosity of the composite pole piece is 0.1% to 10%. The porosity of the composite pole piece can be, but is not limited to, 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5% or 10%. The reason for the low porosity of the composite pole piece may be that at least part of the Li3MCl 6-x Br xThe composite electrode has a lower porosity and more ion transmission pathways, which is conducive to ion diffusion and can improve the overall volume energy density of the battery. A lithium ion transmission path is established inside the electrode. Li3MCl 6-x Br x The ionic conductivity is high, forming an effect similar to "electrolyte infiltration" inside the composite electrode, which is beneficial to reducing the internal resistance of the battery and improving the battery's rate performance and cycle performance.

[0044] In some embodiments, Li3MCl 6-x Br x The ionic conductivity λ satisfies λ≥1 mS / cm; preferably, λ≥1.5 mS / cm, more preferably, λ≥2 mS / cm.

[0045] In some embodiments, the content of the halide solid electrolyte in the active layer increases in sequence along the direction away from the current collector layer. In this way, the content is higher on the side close to the solid electrolyte layer, ensuring the conduction of lithium ions, and the content is lower on the side away from the solid electrolyte layer, so that the proportion of active material content is increased, the active material content is guaranteed, and it is beneficial to improve the energy density of the battery prepared by the composite pole piece.

[0046] In some embodiments, the composite pole piece includes a first pole layer and multiple second pole layers, the first pole layer includes an active material, and the second pole layer includes an active material and a halide solid electrolyte; wherein the first pole layer is formed on the composite pole piece, and the second pole layer is formed on the first pole layer.

[0047] In some embodiments, there are multiple second polar layers, and the multiple second polar layers are located between the first polar layer and the solid electrolyte layer; wherein, along the direction close to the solid electrolyte layer, the Li3MCl 6-x Br x The quality ratio increases.

[0048] In some embodiments, the composite electrode is a composite positive electrode, and the mass proportion of the halide solid electrolyte in the active layer is 5% to 40%; or, the composite electrode is a composite negative electrode, and the mass proportion of the halide solid electrolyte in the active layer is 8% to 50%. It is understandable that due to the different selection of positive electrode active materials and negative electrode active materials in the composite positive electrode and the composite negative electrode, the initial porosity of the positive electrode and the negative electrode is not the same. The density of the positive electrode material is greater than that of the negative electrode material, and the volume is smaller at the same mass ratio. The volume of the halide electrolyte material used is smaller, and its mass proportion will be smaller. Conversely, the mass of the halide electrolyte material used in the negative electrode material is relatively large, so the mass proportion of the halide solid electrolyte in the composite positive electrode and the composite negative electrode is different.

[0049] When the composite electrode is a composite positive electrode, the mass proportion of the halide solid electrolyte in the composite positive electrode can be, but is not limited to, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc. Within the above range, the proportion of the positive electrode active material is guaranteed, and the halide solid electrolyte can play a good lithium ion conduction role. Furthermore, the mass proportion of the halide solid electrolyte in the composite positive electrode can be 15% to 35%.

[0050] When the composite electrode is a composite negative electrode, the mass proportion of the halide solid electrolyte in the composite negative electrode can be, but is not limited to, 8%, 10%, 15%, 20%, 25%, 30%, 35% or 40%, etc. Within the above range, the proportion of the negative electrode active material is guaranteed, and the halide solid electrolyte can play a good lithium ion conduction role. Furthermore, the mass proportion of the halide solid electrolyte in the composite negative electrode can be 15% to 35%.

[0051] In some embodiments, the active material is a positive electrode active material. Exemplarily, the positive electrode active material includes a ternary positive electrode material, a lithium-rich manganese-based positive electrode material, lithium cobalt oxide, lithium nickel manganese oxide, lithium iron phosphate, and lithium manganese iron phosphate.

[0052] In some embodiments, the composite electrode sheet is a composite positive electrode, and the composite positive electrode further includes a positive electrode conductor and a positive electrode binder.

[0053] In some embodiments, the positive electrode conductor includes graphite, such as natural graphite or artificial graphite; carbon materials, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; conductive fibers, such as carbon fibers and metal fibers; conductive tubes, such as carbon nanotubes; metal powders, such as fluorocarbon powders, aluminum powders and nickel powders; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; and polyphenylene derivatives, and from the aspect of improving conductivity, the positive electrode conductor may preferably be superconducting carbon black.

[0054] In some embodiments, the specific surface area of ​​the conductive agent may be 80 m 2 / g~200 m 2 / g, preferably 100 m 2 / g~150 m 2 / g.

[0055] In some embodiments, the positive electrode binder includes at least one of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, styrene-butadiene rubber and fluororubber, preferably polytetrafluoroethylene. It should be noted that the selection of the positive electrode binder in this application is related to the melting point of the halide solid electrolyte, and should satisfy the following requirements: the melting point temperature of the positive electrode binder is greater than the melting point temperature of the halide solid electrolyte.

[0056] In a preferred embodiment, the binder comprises a fiberized binder. It is understood that the fiberized binder can be transformed from a granular state to a fibrous state under the action of a high shear force.

[0057] Exemplarily, the fiberized binder includes one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyethylene (PE), and polypropylene (PP).

[0058] In some embodiments, in the composite positive electrode, the thickness of the positive electrode active layer may be 30 μm to 400 μm, for example, 30 μm, 40 μm, 50 μm, 80 μm, 110 μm, 200 μm, 300 μm, 400 μm, preferably 50 μm to 110 μm.

[0059] In some embodiments, the active material is a negative electrode active material. In the embodiments of the present application, there is no particular limitation on the negative electrode active material, as long as it is a material that can electrochemically absorb and release lithium ions, sodium ions, potassium ions, magnesium ions and other S-zone metal ions, such as carbonaceous materials, metal compound materials, or their oxides, carbides, nitrides, silicides, sulfides, phosphides, etc. These materials can be used alone, or two or more can be used in combination.

[0060] In some embodiments, a carbon material can be selected as the negative electrode active material, and specifically one or more of the following can be selected: graphite, needle coke, amorphous carbon, a carbon-containing mesophase, carbon fiber, and a carbon material with a low degree of graphitization. Among them, graphite can include natural graphite, artificial graphite, and the like. In addition, materials obtained by coating them with carbon materials, such as amorphous carbon and graphitized materials, can also be used. Amorphous carbon includes, but is not limited to, particles obtained by firing the entire mesophase, and particles obtained by infusible treatment and firing of a carbon precursor. As carbonaceous particles with a low degree of graphitization, particles obtained by firing organic matter at a temperature generally below 2500°C can be cited.

[0061] In some embodiments, non-metallic materials that can be used as negative electrode active materials also include silicon and its compounds, such as Si, SiOx (0≤x<2). Since silicon-containing materials are prone to expansion, easy to fall off from the negative electrode current collector, and have poor conductivity, they are often mixed with carbon materials, such as a core-shell structure containing a carbon coating layer.

[0062] In some embodiments, metal compounds can also be selected as negative electrode active materials, such as compounds containing metals or metalloids such as Li, Ag, Al, Bi, Cu, Ga, Ge, In, Ni, Pb, Sb, Si, Sn, Sr, and Zn.

[0063] In one embodiment, when the negative electrode active material is a non-metallic material such as a carbon material, the negative electrode binder may be an aqueous binder such as one or more of sodium hydroxymethyl cellulose, styrene-butadiene latex, polyacrylic acid, acrylic copolymer, cyclodextrin, and the like.

[0064] Referring to FIG. 1 , the present application also provides a method for preparing a composite electrode, the method comprising the following steps:

[0065] S1. Prepare a pole piece precursor; the pole piece precursor includes a current collector layer and an active layer, the active layer includes an active material and a halide solid electrolyte, wherein M is a trivalent metal element, and x satisfies 0<x<6.

[0066] S2. Perform hot pressing treatment on the electrode precursor, and cool it to obtain a composite electrode; wherein the temperature of the hot pressing treatment is greater than or equal to the melting point of the halide solid electrolyte.

[0067] The halide solid electrolyte has a certain fluidity under the condition of temperature higher than the melting point. By adding the halide solid electrolyte to the composite electrode, during the heat treatment, the halide solid electrolyte changes from a granular state to a fluid state, and flows in the pores between the active material particles. At least part of the halide solid electrolyte forms a continuous structure in the active layer, which can be partially filled in the gap of the composite electrode, reducing the gap between the active material and / or the halide solid electrolyte. The solid electrolyte conducts lithium ions by relying on solid-phase contact conduction, and the lithium ion conduction efficiency of the granular solid electrolyte is limited. By continuously filling the halide solid electrolyte in the composite positive electrode, the lithium ion conduction channel can be made continuous, improving the lithium ion conduction capacity, and thus improving the electrochemical performance of the all-solid-state battery.

[0068] In some embodiments, the melting point temperature of the halide solid electrolyte is 80°C to 200°C.

[0069] In some embodiments, the temperature of the hot pressing treatment is 80°C to 200°C. The temperature of the hot pressing treatment may be, but is not limited to, 80°C, 100°C, 120°C, 140°C, 150°C, 160°C, 180°C, 200°C, or 220°C. In this way, the hot pressing treatment can ensure that the halide solid electrolyte has a certain fluidity and does not excessively melt the binder in the pole piece. Further, the temperature of the hot pressing treatment may be 80 to 200°C.

[0070] In some embodiments, the time of hot pressing treatment is 3min~20min, including but not limited to 3min, 4min, 5min, 6min, 8min, 10min, 12min, 14min, 15min, 16min, 18min or 20min. In this way, the halide solid electrolyte can flow within a certain time and has a suitable flow range. When it can flow to the interface between the pole piece and the solid electrolyte layer, it will not cause excessive loss of the solid electrolyte, ensuring the conductivity of lithium ions. Further, the time of hot pressing treatment can be 5min-15min.

[0071] In some embodiments, the pressure of the hot pressing treatment is 10MPa~500MPa, including but not limited to 10MPa, 20MPa, 50MPa, 80MPa, 100MPa, 150MPa, 200MPa, 250MPa, 300MPa, 350MPa, 400MPa, 450MPa or 500MPa, etc. In this way, the hot pressing pressure can promote the flow of the halide solid electrolyte within a suitable range without damaging the pole piece and the solid electrolyte layer structure. Further, the pressure of the hot pressing treatment can be 50MPa~250MPa.

[0072] In some preferred embodiments, step S1 further includes step S11: uniformly mixing the active material with the conductive agent, the binder, and the halide solid electrolyte, placing the mixture in a high shear force device, and performing a binder fiberization treatment to prepare an active layer; or uniformly mixing the active material with the conductive agent and the halide solid electrolyte to form a mixture, uniformly mixing the mixture with the binder, placing the mixture in a high shear force device, and performing a binder fiberization treatment to prepare an active layer.

[0073] The present application also provides a solid-state battery, which includes the above-mentioned composite electrode sheet. The solid-state battery may be an all-solid-state battery.

[0074] In some embodiments, a solid-state battery includes a solid-state electrolyte layer disposed between a positive electrode or a composite positive electrode and a composite negative electrode or a negative electrode.

[0075] In some embodiments, at least one of the positive electrode and the negative electrode of the solid-state battery is the above-mentioned composite electrode sheet, preferably the positive electrode is a composite positive electrode and the negative electrode is a composite negative electrode.

[0076] In some embodiments, the solid electrolyte layer includes a solid electrolyte. The types of solid electrolytes are not limited in this application and are not specifically defined here. Conventional solid electrolyte materials in the art can be used. Solid electrolyte materials include, but are not limited to, one or more of oxide solid electrolytes, sulfide solid electrolytes, halide solid electrolytes, hydride solid electrolytes, boride solid electrolytes, and nitride solid electrolytes.

[0077] In some embodiments, the oxide solid electrolyte can be selected from crystalline oxide solid electrolytes or glassy oxide solid electrolytes. Crystalline oxide solid electrolytes include, but are not limited to, perovskite-type oxide solid electrolytes, NASICON-type oxide solid electrolytes, LISICON-type oxide solid electrolytes, and garnet-type oxide solid electrolytes, etc.; glassy oxide solid electrolytes include, but are not limited to, LiPON-type oxide solid electrolytes, etc.

[0078] In some embodiments, the perovskite-type oxide solid electrolyte includes, but is not limited to, Li 3.3 La 0.53 TiO3, LiSr1 .65 Zr 1.3 Ta 1.7 O9, Li 2x-y Sr 1-x Ta y Zr 1-y O3 (where x = 0.75y and 0.60 < y < 0.75), Li 3 / 8 Sr 7 / 16 Nb 3 / 4Zr 1 / 4 O3, Li 3x La (2 / 3-x) TiO3 (where 0 < x < 0.25), or one or more thereof.

[0079] In some embodiments, the NASICON-type oxide solid electrolyte can be defined by LiMM′(PO4)3, where M and M′ are independently selected from Al, Ge, Ti, Sn, Hf, Zr, and La. For example, in certain variants, the NASICON-type oxide solid electrolyte includes, but is not limited to, Li 1+x Al x Ge 2-x (PO4)3 (LAGP) (where 0 ≤ x ≤ 2), Li 1+x Al x Ti 2-x(PO4)3(LATP) (where 0 ≤ x ≤ 2), Li 1+x Y x Zr 2-x (PO4)3(LYZP) (where 0 ≤ x ≤ 2), Li 1.3 Al 0.3 Ti 1.7 One or more of (PO4)3, LiTi2(PO4)3, LiGeTi(PO4)3, LiGe2(PO4)3, LiHf2(PO4)3.

[0080] In some embodiments, the LISICON-type oxide solid electrolyte includes, but is not limited to, Li 14 Zn(GeO4)4, Li 3+x (P 1-x Si x )O4 (where 0 < x < 1), Li 3+x Ge x V 1-x O4 (where 0 < x < 1).

[0081] In some embodiments, the garnet-type oxide solid electrolyte includes, but is not limited to, Li 6.5 La3Zr 1.75 Te 0.25 O 12 , Li7La3Zr2O 12 , Li 6.2 Ga 0.3 La 2.95 Rb 0.05 Zr2O 12 , Li 6.85 La 2.9 Ca 0.1 Zr 1.75 Nb 0.25 O 12 , Li 6.25 Al 0.25 La3Zr2O 12 , Li 6.75 La3Zr 1.75 Nb 0.25 O 12 One or more of them.

[0082] In some embodiments, the sulfide solid electrolyte includes, but is not limited to, Li2S-P2S5, Li2S-P2S5-MS x (where M is Si, Ge, and Sn and 0 ≤ x ≤ 2), Li 3.4 Si 0.4 P 0.6 S4, Li 10GeP2S 11.7 O 0.3 、Li 9.6 P3S 12 、Li7P3S 11 、Li9P3S9O3、Li 10.35 Si 1.35 P 1.65 S 12 、Li 9.81 Sn 0.81 P 2.19 S 12 、Li 10 (Si 0.5 Ge 0.5 )P2S 12 、Li(Ge 0.5 Sn 0.5 )P2S 12 、Li(Si 0.5 Sn 0.5 )PsS 12 、Li 10 GeP2S 12 (LGPS)、Li6PS5X (where X is Cl, Br or I), Li7P2S8I, Li 10.35 Ge 1.35 P 1.65 S 12 、Li 3.25 Ge 0.25 P 0.75 S4、Li 10 SnP2S 12 、Li 10 SiP2S 12 、Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 、 one or more sulfide-based materials such as xLi2S-(1-x)P2S5 (where 0.5 ≤ x ≤ 0.7).

[0083] In some embodiments, the halide solid electrolyte includes, but is not limited to, one or more halide-based materials such as Li2CdCl4, Li2MgCl4, Li2CdI4, Li2ZnI4, Li3OCl, Li2ZrCl6, Li2HfCl6, Li3InCl6, Li3InCl6, Li3YCl6, L3ScCl6, Li5ZnI4, Li3OCl 1-x Br x (where 0 < x < 1).

[0084] In some embodiments, the hydride solid electrolyte includes, but is not limited to, one or more hydride-based materials of Li3AlH6, LiBH4, LiBH4-LiX (wherein X is one of Cl, Br, and I), LiNH2, Li2NH, LiBH4-LiNH2.

[0085] In some embodiments, the boride solid electrolyte includes, but is not limited to, one or more borate-based materials of Li2B4O7, Li2O-(B2O3)-(P2O5).

[0086] In some embodiments, the nitride solid electrolyte includes, but is not limited to, one or more nitride-based materials of Li3N, Li7PN4, LiSi2N3, and LiPON.

[0087] It can be understood that the terms including the above-mentioned oxide solid electrolyte, sulfide solid electrolyte, halide solid electrolyte, hydride solid electrolyte, boride solid electrolyte, nitride solid electrolyte and other materials are all known in the art. The refinement of the above-mentioned materials is only for illustrative purposes and not for limitation of the scope of protection. Without violating the inventive concept of the present application, any known solid electrolyte material can be used in the present application.

[0088] In some preferred embodiments, the solid electrolyte layer includes a halide solid electrolyte.

[0089] The following are specific embodiments.

[0090] Example 1

[0091] This embodiment provides a composite positive electrode, the composite positive electrode includes a current collector aluminum foil and an active layer formed on the surface of the aluminum foil, the active layer includes active materials NCM811 and Li3YCl3Br3, and the surface roughness of the composite positive electrode is 12μm. The porosity of the composite positive electrode is 5.2%. The ion conductivity of Li3YCl3Br3 is 2.34mS / cm. The melting point of Li3YCl3Br3 is 115℃.

[0092] A composite negative electrode, the composite positive electrode includes a current collector copper foil and a negative electrode active layer formed on the surface of the copper foil, the negative electrode active layer includes active materials graphite and Li3YCl3Br3, the surface roughness of the composite negative electrode is 14μm. The porosity of the composite negative electrode is 8.5%. The ion conductivity of Li3YCl3Br3 is 2.34mS / cm.

[0093] This embodiment provides a method for preparing a composite positive electrode, comprising the following steps:

[0094] To prepare a composite positive electrode, NCM811, PTFE, super-P, and Li3YCl3Br3 were uniformly mixed in a mass ratio of 80:3:2:15, placed in a high shear equipment mixer, subjected to fiberization treatment to form a first mixture, and the first mixture was rolled to form a first positive electrode layer; the rolling temperature was 60°C and the rolling time was 5 min.

[0095] The positive electrode current collector and the first positive electrode layer are stacked, hot pressed, and cooled to form a composite positive electrode, wherein the hot pressing temperature is 150°C, the hot pressing time is 10 minutes, and the hot pressing pressure is 120 MPa.

[0096] This embodiment provides a method for preparing a composite negative electrode, comprising the following steps:

[0097] The first negative electrode layer was prepared by mixing the negative electrode active materials graphite, (CMC+SBR), super-P and Li3YCl3Br3 in a mass ratio of 69:4:2:25, putting them into a high shear force equipment mixer, and performing fiberization treatment to form a second mixture, and rolling the second mixture to form the first negative electrode layer; the rolling temperature was 60° C., and the rolling time was 5 min;

[0098] The negative electrode current collector and the first negative electrode layer are stacked, heat-pressed, and cooled to form a composite negative electrode, wherein the heat-pressing temperature is 120° C., the time is 12 minutes, and the pressure is 200 MPa.

[0099] This embodiment also provides a solid-state battery, comprising the composite positive electrode, the composite negative electrode and a solid electrolyte layer. The solid electrolyte layer comprises a halide solid electrolyte Li2ZrCl6 and a binder PTFE, and the mass ratio of the two is 97:3.

[0100] Example 2

[0101] The difference between Example 2 and Example 1 is that: in the composite positive electrode, the mass proportion of Li3YCl3Br3 is 40%, the surface roughness of the composite positive electrode is 1.5 μm, the ion conductivity of Li3YCl3Br3 is 2.34 mS / cm, and the melting point of Li3YCl3Br3 is 115°C.

[0102] In the composite negative electrode, the mass of Li3YCl3Br3 accounts for 50%, and the surface roughness of the composite negative electrode is 1.5μm. The ionic conductivity of Li3YCl3Br3 is 2.34mS / cm. The melting point of Li3YCl3Br3 is 115℃.

[0103] Example 3

[0104] The difference between Example 3 and Example 1 is that: in the composite positive electrode, the mass proportion of Li3YCl3Br3 is 5%, the surface roughness of the composite positive electrode is 30 μm, the ion conductivity of Li3YCl3Br3 is 2.34 mS / cm, and the melting point of Li3YCl3Br3 is 115°C.

[0105] In the composite negative electrode, the mass proportion of Li3YCl3Br3 is 8%, and the surface roughness of the composite negative electrode is 30μm. The ion conductivity of Li3YCl3Br3 is 2.34mS / cm. The melting point of Li3YCl3Br3 is 115℃.

[0106] Example 4

[0107] The difference between Example 4 and Example 1 is that in the composite positive electrode, the active layer includes active materials NCM811 and Li3Y 0.5 Dy 0.5 Cl3Br3, Li3Y 0.5 Dy 0.5 The mass proportion of Cl3Br3 is 15%, and the surface roughness of the composite positive electrode is 15μm. 0.5 Dy 0.5 The ionic conductivity of Cl3Br3 is 2.72 mS / cm. Li3Y 0.5 Dy 0.5 The melting point of Cl3Br3 is 120℃.

[0108] In the composite negative electrode, the active layer includes negative electrode active materials graphite and Li3Y 0.5 Dy 0.5 Cl3Br3, Li3Y 0.5 Dy 0.5 The mass proportion of Cl3Br3 is 25%, and the surface roughness of the composite negative electrode is 17μm. 0.5 Dy 0.5 The ionic conductivity of Cl3Br3 is 2.72 mS / cm. Li3Y 0.5 Dy 0.5 The melting point of Cl3Br3 is 120℃.

[0109] Example 5

[0110] The difference between Example 5 and Example 1 is that in the composite positive electrode, the active layer includes active materials NCM811 and Li3In 0.5 Fe 0.5 Cl3Br3, Li3In 0.5 Fe 0.5 The mass proportion of Cl3Br3 is 15%, and the surface roughness of the composite positive electrode is 17μm. 0.5 Fe 0.5The ionic conductivity of Cl3Br3 is 2.48 mS / cm. Li3In 0.5 Fe 0.5 The melting point of Cl3Br3 is 125℃.

[0111] In the composite negative electrode, the active layer includes negative electrode active materials graphite and Li3In 0.5 Fe 0.5 Cl3Br3, Li3Y 0.5 Dy 0.5 The mass proportion of Cl3Br3 is 25%, and the surface roughness of the composite negative electrode is 19μm. 0.5 Fe 0.5 The ionic conductivity of Cl3Br3 is 2.48 mS / cm. Li3In 0.5 Fe 0.5 The melting point of Cl3Br3 is 125℃.

[0112] Example 6

[0113] This embodiment provides a composite positive electrode, the composite positive electrode includes a current collector aluminum foil and an active layer formed on the surface of the aluminum foil, the active layer includes active materials NCM811 and Li3YCl3Br3, and the surface roughness of the composite positive electrode is 18μm. The porosity of the composite positive electrode is 7.2%. The ion conductivity of Li3YCl3Br3 is 2.34mS / cm. The melting point of Li3YCl3Br3 is 115℃.

[0114] A composite negative electrode, the composite positive electrode includes a current collector copper foil and a negative electrode active layer formed on the surface of the copper foil, the negative electrode active layer includes active materials graphite and Li3YCl3Br3, the surface roughness of the composite negative electrode is 23μm. The porosity of the composite negative electrode is 11%. The ion conductivity of Li3YCl3Br3 is 2.34mS / cm.

[0115] This embodiment provides a method for preparing a composite positive electrode, comprising the following steps:

[0116] Prepare the first positive electrode layer, mix NCM811, Li3YCl3Br3, PTFE and super-P in a mass ratio of 90:5:3:2, put them into a high shear equipment mixer, and perform fiberization treatment to form a first mixture, and roll the first mixture to form a first positive electrode layer; the rolling temperature is 60°C, and the rolling time is 5 minutes.

[0117] To prepare the second positive electrode layer, NCM811, Li3YCl3Br3, PTFE and super-P were uniformly mixed in a mass ratio of 75:20:3:2, placed in a high shear equipment mixer, subjected to fiberization treatment to form a second mixture, and the second mixture was rolled to form a second positive electrode layer; the rolling temperature was 60°C and the rolling time was 5 min.

[0118] NCM811, Li3YCl3Br3, PVDF and super-P were mixed uniformly in a mass ratio of 55:40:3:2, put into a high shear force equipment mixer, and subjected to fiberization treatment to form a third mixture, which was then rolled to form a second positive electrode layer; the rolling temperature was 60°C, and the rolling time was 5 min.

[0119] The positive electrode current collector, the first positive electrode layer, the second first positive electrode layer, and the second second positive electrode layer are stacked in sequence, hot pressed, and cooled to form a composite positive electrode. The hot pressing temperature is 150°C, the hot pressing time is 10 minutes, and the hot pressing pressure is 120MPa.

[0120] This embodiment provides a method for preparing a composite negative electrode, comprising the following steps:

[0121] Prepare the first negative electrode layer, mix the negative electrode active materials graphite, Li3YCl3Br3, (CMC+SBR) and super-P in deionized water in a mass ratio of 86:8:4:2, stir evenly, and obtain the first negative electrode layer slurry; apply the first negative electrode layer slurry on the surface of copper foil, dry it, and obtain the first negative electrode layer on the surface of copper foil; the drying temperature is 70°C.

[0122] Prepare a second negative electrode layer, mix the negative electrode active materials graphite, Li3YCl3Br3, (CMC+SBR) and super-P in deionized water in a mass ratio of 74:20:4:2, stir evenly to obtain a second negative electrode layer slurry, apply the second negative electrode layer slurry on the surface of the first negative electrode layer, dry it, and obtain the second negative electrode layer;

[0123] The negative electrode active materials Li-In alloy, Li3YCl3Br3, (CMC+SBR) and super-P are mixed in deionized water in a mass ratio of 54:40:4:2, stirred evenly to obtain a second negative electrode layer slurry, and the second negative electrode layer slurry is coated on the surface of the second negative electrode layer, and dried to obtain a negative electrode precursor;

[0124] The negative electrode precursor is subjected to hot pressing to obtain a composite negative electrode. The hot pressing temperature is 120° C., the time is 12 minutes, and the pressure is 200 MPa.

[0125] This embodiment also provides a solid-state battery, comprising the composite positive electrode, the composite negative electrode and a solid electrolyte layer. The solid electrolyte layer comprises a first halide solid electrolyte Li2ZrCl6 and a binder PTFE, and the mass ratio of the two is 97:3.

[0126] Comparative Example 1

[0127] The difference between Comparative Example 1 and Example 1 is that:

[0128] The composite cathode does not include Li3YCl3Br3, and the mass ratio of NCM811, PTFE, and super-P is 95:3:2;

[0129] The composite negative electrode does not include Li3YCl3Br3, and the mass ratio of graphite, (CMC+SBR) and super-P is 94:4:2.

[0130] Comparative Example 2

[0131] The difference between Comparative Example 2 and Example 1 is that:

[0132] Replace Li3YCl3Br3 in the composite positive electrode and the composite negative electrode with Li2ZrCl6.

[0133] Comparative Example 3

[0134] The difference between Comparative Example 3 and Example 1 is that:

[0135] Replace Li3YCl3Br3 in the composite positive electrode and the composite negative electrode with LLZO.

[0136] Comparative Example 4

[0137] The preparation method of Comparative Example 4 is substantially the same as that of Example 1, except that:

[0138] No heat pressing process.

[0139] The raw materials A, B, C and Drying, calcination (just an example), etc. The process parameters are listed in Table 1:

[0140] Table 1

[0141]

[0142] The composite positive electrodes and composite positive electrodes prepared in Examples 1 to 6 and Comparative Examples 1 to 3 and the solid-state batteries further prepared were subjected to performance tests. The test results are shown in Tables 1 and 2.

[0143] Among them, the test conditions or test standards for each performance test item are:

[0144] (1) Melting point test

[0145] The test was carried out using a differential scanning calorimeter. The solid electrolyte material was placed in a crucible and heated from 30°C to 1000°C at a rate of 10°C / min in a nitrogen atmosphere to measure the melting point of the solid electrolyte material.

[0146] (2) Porosity test

[0147] True density test: The true density of the composite positive electrode is obtained by testing with a true density meter. The test process is as follows: After the power is turned on, the instrument is preheated according to the requirements of the instrument manual to ensure that the instrument reaches a stable working state. Place the sample to be tested in the sample pool, press the measurement button, and the instrument will automatically measure the density. After the measurement is completed, the instrument will automatically record the data and calculate the true density value ρ 真 .

[0148] Compacted density test: Add 100 mg of powder into a φ10 mm mold, apply a pressure of 375 MPa and maintain the pressure for 3 minutes, then remove the mold to obtain a compacted sheet, measure its thickness, and calculate its compacted density ρ 压实 .

[0149] Porosity: Porosity is (ρ 真 -ρ 压实 ) / ρ 真

[0150] (3) Surface roughness test

[0151] The electrolyte sheet is placed under a high-precision optical microscope for observation. In the 3D imaging mode, the electrolyte sheet can be obtained at 200*300μm 2 The surface height distribution information inside the electrolyte sheet can be obtained by counting the maximum surface height difference of the electrolyte sheet.

[0152] (4) Battery performance test

[0153] The battery performance was tested using the LAND CT2001A battery testing system. The composite positive electrodes and composite negative electrodes of Examples 1-6 and Comparative Examples 1-4 were prepared into button-type batteries and subjected to charge and discharge tests, rate tests, and cycle tests in the voltage range of 2.45-4.2 V. The battery performance tests were all completed in a 25°C constant temperature box.

[0154] Table 2

[0155]

[0156] As can be seen from Table 2 above, the battery rate performance is significantly improved by providing a continuous halide solid electrolyte in the composite electrode. The surface roughness of the composite electrode is low, which can effectively improve the interface contact between the composite electrode and the solid electrolyte layer and effectively reduce the internal resistance of the battery.

[0157] By hot pressing, the porosity of the electrode is within an appropriate range, forming a continuous conduction channel that is conducive to the formation of lithium ions, thereby improving the lithium ion transmission capacity and improving the electrochemical performance of the all-solid-state battery.

[0158] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0159] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. A composite pole piece, characterized in that: The composite pole piece includes a current collector layer and an active layer formed on the surface of the current collector layer, the active layer includes an active material and a halide solid electrolyte, wherein the second halide solid electrolyte changes from a solid state to a liquid state, and then changes from a liquid state to a solid state; the surface roughness of the composite pole piece is 1.5 μm~30 μm.

2. The composite pole piece according to claim 1, characterized in that: The halide solid electrolyte includes Li3MCl 6- x Br x , and at least part of Li3MCl 6-x Br x A continuous structure is formed in the active layer, wherein M is a trivalent metal element and x satisfies 0<x<6; Preferably, the melting point of the halide solid electrolyte is 80°C to 200°C.

3. The composite pole piece according to claim 1, characterized in that: The porosity of the composite electrode is 0.1% to 10%.

4. The composite pole piece according to claim 2, characterized in that: The Li3MCl 6-x Br x The ionic conductivity λ satisfies λ ≥ 1 mS / cm.

5. The composite pole piece according to claim 1, characterized in that: Along the direction away from the current collector layer, the mass proportion of the halide solid electrolyte in the active layer gradually increases.

6. The composite pole piece according to claim 5, characterized in that: The composite pole piece includes a first pole layer and multiple second pole layers, the first pole layer includes an active material, and the second pole layer includes an active material and the halide solid electrolyte; wherein the first pole layer is formed on the composite pole piece, and the second pole layer is formed on the first pole layer.

7. The composite pole piece according to claim 1, characterized in that: The composite electrode is a composite positive electrode, and the mass proportion of the halide solid electrolyte in the active layer is 5% to 40%; or, The composite electrode is a composite negative electrode, and in the active layer, the mass proportion of the halide solid electrolyte is 8% to 50%.

8. A method for preparing a composite electrode, characterized in that: The following steps are involved: Prepare a pole piece precursor; the pole piece precursor comprises a current collector layer and an active layer, and the active layer comprises an active material and a halide solid electrolyte; The electrode precursor is subjected to hot pressing treatment to obtain a composite electrode; wherein the temperature of the hot pressing treatment is greater than or equal to the melting point temperature of the halide solid electrolyte.

9. The preparation method according to claim 8, characterized in that: The temperature of the hot pressing treatment is 80°C to 200°C; and / or, The time of hot pressing treatment is 0.5min ~30min; and / or, The pressure of hot pressing treatment is 10MPa ~500MPa.

10. A solid-state battery, characterized in that: The solid-state battery comprises the composite pole piece according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Method of coating solid electrolyte with electrode material, coating material, and electrode prepared using coating method

    CN111146425A

  • Positive electrode material layer suitable for all-solid-state battery, preparation method of positive electrode material layer, positive plate and all-solid-state battery

    CN112133921A

  • All-solid-state lithium battery composite positive electrode prepared based on melt permeation method and preparation method thereof

    CN113437249A

  • Novel positive electrode structure, preparation method thereof and battery

    CN114464765A

  • Preparation method of pole piece, positive pole piece and lithium ion battery

    CN115714164A

Cited By

  • Composite positive pole piece, preparation method thereof and solid-state battery

    CN120637642A

  • Solid-state battery cell, positive electrode material and preparation method therefor, battery device and electric device