Positive plate, preparation method thereof and lithium ion battery

By using the synergistic effect of TiOF2 cladding and LiPSCl composite layer on the positive electrode material of lithium-ion battery, the dissolution and deposition of high-valent metal ions is solved, significantly improving the circulation and storage performance of the battery, and achieving efficient capacity preservation and storage capacity recovery.

CN119069636AActive Publication Date: 2024-12-03BYD CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202310639030.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

In lithium-ion batteries, the dissolution and deposition of high-valent metal ions (such as Mn2+, Fe2+) on the negative electrode surface affects the cycling and storage performance of the battery. The existing technology is difficult to effectively solve this problem, especially in cost and performance. It is difficult to find a balance between them.

Method used

A manganese-based or iron-based positive electrode active material with a TiOF2 cladding layer is used, and a composite layer containing LiPSCl is formed on the surface of the active material layer. Through the synergy between TiOF2 and LiPSCl, the migration and deposition of highly regular metal ions are prevented.

Benefits of technology

The circulation and storage performance of lithium-ion batteries have been significantly improved. The capacity retention rate after 300 cycles of 0.5C/1C under 25℃ is greater than 85%, and the storage capacity recovery rate of 28 days is greater than 83%, and the optimization is It reaches 93% and above 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069636A_ABST
    Figure CN119069636A_ABST
Patent Text Reader

Abstract

The invention relates to the field of lithium ion batteries, in particular to a positive plate, a preparation method thereof and a lithium ion battery. The positive plate comprises a current collector, an active material layer and a composite layer, wherein the active material layer is arranged between the current collector and the composite layer; wherein the active material layer comprises an active material having a TiOF2 coating layer; the composite layer contains LiPSCl; the active material with the TiOF2 coating layer comprises a manganese-based positive electrode active material with the TiOF2 coating layer and / or an iron-based positive electrode active material with the TiOF2 coating layer. According to the positive plate, a material formed by coating manganese-based and / or iron-based positive electrode active material particles with TiOF2 is adopted as a pole plate active main body, and a composite layer containing LiPSCl is arranged on an active material layer, so that migration and deposition of high-positive-valence metal ions of a positive electrode to the surface of a negative electrode can be greatly reduced, and the cycle performance and the storage performance of the battery are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium ion batteries, and in particular to a positive electrode sheet and a preparation method thereof, and a lithium ion battery. Background Art

[0002] In lithium-ion batteries, the positive electrode material is usually a material containing high positive ions. During battery cycling and high-rate operation, high positive metal ions dissolve and deposit on the negative electrode surface, greatly affecting the battery's cycling performance and storage performance. In order to solve the problem of dissolution and deposition of high positive metal ions and optimize battery performance, the industry has explored a variety of methods.

[0003] CN109346768A discloses a non-aqueous electrolyte for an ion battery, comprising an electrolyte lithium salt, a non-aqueous organic solvent and a film-forming additive, wherein the film-forming additive comprises a boric acid compound, which can form a dense protective film on the surface of a positive electrode material, reduce the oxidation reaction of the electrolyte on the surface of the battery material, and at the same time complex the divalent manganese ions in the electrolyte to avoid the reduction and deposition of the divalent manganese ions on the surface of the negative electrode.

[0004] CN103972490A discloses a coating method for lithium manganese oxide positive electrode materials for lithium batteries. The method uses graphene to coat the lithium manganese oxide positive electrode material, which can effectively reduce the dissolution of manganese ions, while helping to improve the conductivity of lithium manganese oxide, and can improve the specific capacity and rate performance of the lithium manganese oxide positive electrode material.

[0005] Adding additives to the electrolyte may reduce the conductivity of the electrolyte, increase the risk of gas production in the battery, increase the internal resistance of the battery, and deteriorate the battery performance. Coating with high-cost positive electrode materials such as graphene can optimize the conductivity of the positive electrode material and alleviate the deposition problem to a certain extent, but it will increase production costs and is not conducive to marketization.

[0006] Therefore, there is still a need to provide an optimized solution that can solve the problem of dissolution and deposition of high positive-valent metal ions in the positive electrode sheet, thereby improving the battery cycle performance and storage performance. Summary of the invention

[0007] The purpose of the present invention is to overcome the problem in the prior art that high positive metal ions in the positive electrode of a lithium ion battery are dissolved and deposited on the surface of the negative electrode, thereby affecting the battery's cycle performance and storage performance, and to provide a positive electrode sheet and a preparation method thereof and a lithium ion battery.

[0008] In order to achieve the above-mentioned object, the first aspect of the present invention provides a positive electrode sheet, which comprises: a current collector, an active material layer and a composite layer, wherein the active material layer is arranged between the current collector and the composite layer; wherein:

[0009] The active material layer comprises TiOF2 Active material of the coating layer; the composite layer contains LiPSCl;

[0010] The TiOF 2 The active material of the coating layer includes TiOF 2 Manganese-based positive electrode active material with coating layer and / or TiOF 2 The iron-based positive electrode active material of the coating layer.

[0011] A second aspect of the present invention provides a method for preparing a positive electrode sheet, the method comprising:

[0012] (1) coating a slurry containing an active material on the surface of a current collector, and after drying, forming an active material layer on the surface of the current collector;

[0013] Wherein, the active material comprises TiOF 2 Manganese-based positive electrode active material with coating layer and / or TiOF 2 An iron-based positive electrode active material of the coating layer;

[0014] (2-1) coating a slurry containing LiPSCl on the surface of the active material layer, and after drying, forming a composite layer on the surface of the active material layer to obtain a positive electrode sheet;

[0015] or

[0016] (2-2) A slurry containing LiPSCl is coated to form a film, and after drying, a film layer is formed; then, the film layer is hot-pressed to form a composite layer on the surface of the active material layer, thereby obtaining a positive electrode sheet.

[0017] The third aspect of the present invention provides a positive electrode sheet made by the method described in the second aspect.

[0018] A fourth aspect of the present invention provides a lithium-ion battery, which includes the positive electrode sheet described in the first aspect or the third aspect.

[0019] Through the above technical solution, compared with the prior art, the positive electrode provided by the present invention adopts TiOF 2 The positive electrode active material of the coating layer, TiOF 2 The coating layer can combine with the high positive metal ions dissolved from the positive active material to form metal fluoride, thereby preventing the migration of the high positive metal ions. The positive electrode sheet has a composite structure, and a composite layer containing LiPSCl (lithium phosphorus sulfur chloride) is arranged on the outer surface of the active material layer, wherein LiPSCl forms a dense isolation layer at the microscopic level, which can further prevent the migration of large-sized high positive metal ions. 2The synergistic effect between the coating layer and the LiPSCl composite layer can effectively inhibit the migration and deposition of positive high-valent metal ions to the negative electrode surface, thereby significantly improving the performance of lithium-ion batteries. The capacity retention rate can be greater than 85% after 300 cycles of 0.5C / 1C at 25°C, and the storage capacity recovery rate can be greater than 83% after 28 days at 45°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0021] Figure 1 This is a SEM test image of the raw material lithium manganate used in Preparation Example 1 of the present invention.

[0022] Figure 2 Lithium manganate@TiOF prepared in Preparation Example 1 of the present invention 2 SEM test picture. DETAILED DESCRIPTION

[0023] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0024] A first aspect of the present invention provides a positive electrode sheet, the positive electrode sheet comprising: a current collector, an active material layer and a composite layer, wherein the active material layer is arranged between the current collector and the composite layer; wherein:

[0025] The active material layer comprises TiOF 2 Active material of the coating layer; the composite layer contains LiPSCl;

[0026] The TiOF 2 The active material of the coating layer includes TiOF 2 Manganese-based positive electrode active material with coating layer and / or TiOF 2 The iron-based positive electrode active material of the coating layer.

[0027] According to the present invention, the current collector in the positive electrode sheet can be any conventional current collector for lithium-ion batteries in the art, and the present invention does not impose any particular limitation on the material selection and specification parameters of the current collector.

[0028] According to the present invention, the active material layer is located on the surface of the current collector, wherein the active material has a core and a TiOF coated on the surface of the core. 2 Coating layer. The core is made of manganese-based positive electrode active material and / or iron-based positive electrode active material. In the present invention, the manganese-based positive electrode active material and the iron-based positive electrode active material are defined broadly. Preferably, the manganese-based positive electrode active material can be selected from at least one of lithium-rich manganese-based positive electrode material, lithium manganate, lithium manganese nickelate and lithium manganese iron phosphate; the iron-based positive electrode active material can be selected from at least one of lithium iron phosphate, lithium iron silicate and lithium iron borate.

[0029] Generally, the above-mentioned manganese-based positive electrode active materials and / or iron-based positive electrode active materials will generate high positive metal ions (such as Mn 2+ , Fe 2+ ) are dissolved, and these high positive metal ions migrate to the negative electrode surface through the electrolyte and are reduced and deposited, resulting in a decrease in battery capacity and a decrease in cycle performance. The positive electrode provided by the present invention uses a TiOF 2 Active material of coating layer, TiOF 2 The presence of the coating layer can reduce the direct contact between the positive electrode active material in the core and the electrolyte, slowing down the dissolution of high positive metal ions. 2 The material can combine with dissolved high positive metal ions to convert them into metal fluorides (such as MnF 2 , FeF 2 ), reducing the migration of high positive metal ions to the negative electrode. In addition, TiOF 2 It is a wide bandgap ionic material with a cubic structure, and can also improve the battery kinetic performance.

[0030] According to the present invention, based on the TiOF 2 The total weight of the active material of the coating layer, the TiOF 2 TiOF in the active material of the coating layer 2 The content is 0.1-10wt%, preferably 4-6wt%.

[0031] In the present invention, the TiOF 2 TiOF in the active material of the coating layer 2 The content can be determined by EDS testing of elements using a scanning electron microscope (ie, SEM-EDS).

[0032] According to the present invention, the active material layer in the positive electrode sheet further contains a conductive agent and a first binder.

[0033] According to the present invention, based on the total weight of the active material layer, in the active material layer, TiOF 2 The content of the active material layer is 3-5wt%, preferably 3.5-4wt%; the content of the conductive agent is 2-20wt%; the content of the first binder is 2-15wt%. When the components of the active material layer meet the above content ranges, they can better inhibit the migration and deposition of high positive metal ions and bring better battery cycle life.

[0034] According to the present invention, the composite layer has a selective isolation function, wherein the LiPSCl contained therein forms a dense isolation layer at the microscopic level, which can prevent high-valent and large-sized metal ions from passing through. Since LiPSCl has a high ionic conductivity, it allows relatively small-sized Li + Rapidly pass through the composite layer, while ensuring that Li + While migrating, it prevents large-sized high-positive metal ions from migrating to the negative electrode.

[0035] According to the present invention, the composite layer in the positive electrode sheet further contains a second binder.

[0036] According to the present invention, based on the total weight of the composite layer, in the composite layer, the content of LiPSCl is 5-50wt%, preferably 20-40wt%; the content of the second binder is 45-90wt%. When the components of the composite layer meet the above content ranges, the migration and deposition of high positive metal ions can be better prevented.

[0037] In the present invention, there is no particular limitation on the conductive agent and the binder, and they can be any conventional conductive agent and binder for lithium-ion battery pole pieces in the art. For example, the conductive agent can be selected from at least one of acetylene black, carbon nanotubes, graphene, conductive carbon black and conductive graphite; the first binder and the second binder can be independently selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylate, polyurethane, polyethylene glycol, polyethylene oxide, epoxy resin, styrene-butadiene rubber, polymethyl cellulose, sodium polymethyl cellulose, hydroxypropyl methyl cellulose and polypropylene alcohol.

[0038] According to the present invention, preferably, in the positive electrode sheet, TiOF 2 :LiPSCl weight ratio is 1:(0.1-2).

[0039] According to the present invention, preferably, the thickness of the active material layer is 60-100 μm.

[0040] According to the present invention, preferably, the composite layer has a thickness of 5-30 μm.

[0041] The positive electrode sheet provided by the present invention is prepared by treating the manganese-based and / or iron-based positive electrode active material particles with TiOF 2 The material formed by the coating is used as the active body of the electrode, and a composite layer containing LiPSCl is set on the surface of the active material layer. The above factors form a synergistic effect, which can greatly reduce the migration and deposition of high positive metal ions in the positive electrode active material to the negative electrode surface, so that the cycle performance and storage performance of the battery are greatly improved. When the active material layer and the composite layer in the positive electrode sheet each have the above-defined composition and component content, the capacity retention rate of the lithium-ion battery after 300 cycles at 0.5C / 1C at 25°C can be greater than 85%, and the storage capacity recovery rate at 45°C for 28 days is greater than 83%. Furthermore, on the basis of meeting the above-mentioned limited conditions, the TiOF in the positive electrode sheet 2 The weight ratio of manganese to LiPSCl satisfies 1:(0.1-2), which can achieve a further preferred effect of the present invention, and can achieve a capacity retention rate of greater than 93% for manganese-based and iron-based lithium-ion batteries after 300 cycles of 0.5C / 1C at 25°C, and a storage capacity recovery rate of greater than 90% for 28 days at 45°C.

[0042] A second aspect of the present invention provides a method for preparing a positive electrode sheet, the method comprising:

[0043] (1) coating a slurry containing an active material on the surface of a current collector, and after drying, forming an active material layer on the surface of the current collector;

[0044] Wherein, the active material comprises TiOF 2 Manganese-based positive electrode active material with coating layer and / or TiOF 2 An iron-based positive electrode active material of the coating layer;

[0045] (2-1) coating a slurry containing LiPSCl on the surface of the active material layer, and after drying, forming a composite layer on the surface of the active material layer to obtain a positive electrode sheet;

[0046] or

[0047] (2-2) A slurry containing LiPSCl is coated to form a film, and after drying, a film layer is formed; then, the film layer is hot-pressed to form a composite layer on the surface of the active material layer, thereby obtaining a positive electrode sheet.

[0048] According to the present invention, in step (1), the current collector can be any conventional current collector for lithium-ion batteries in the art, and the present invention does not impose any particular limitation on the material selection and specification parameters thereof.

[0049] According to the present invention, in step (1), the active material comprises a core and a TiOF coated on the surface of the core. 2The core is made of a manganese-based positive electrode active material and / or an iron-based positive electrode active material. Preferably, the manganese-based positive electrode active material can be selected from at least one of lithium-rich manganese-based positive electrode materials, lithium manganate, lithium manganese nickelate and lithium manganese iron phosphate; the iron-based positive electrode active material can be selected from at least one of lithium iron phosphate, lithium iron silicate and lithium iron borate.

[0050] In the present invention, TiOF 2 The active material of the coating layer is the active main body of the positive electrode sheet. On the one hand, the coating layer can play a barrier role, reducing the direct contact between the positive electrode active material in the core and the electrolyte in the lithium-ion battery, slowing down the dissolution of high positive metal ions during battery operation. On the other hand, the coating layer can play a conversion role, converting the dissolved high positive metal ions into metal fluorides (such as MnF 2 , FeF 2 ), reducing the migration of high positive metal ions to the negative electrode of the battery. In addition, TiOF 2 It can also improve battery kinetics.

[0051] According to the present invention, based on the total weight of the active material, the TiOF in the active material is 2 The content is 0.1-10wt%, preferably 4-6wt%.

[0052] According to the present invention, the preparation process of the active material in step (1) comprises:

[0053] (i) mixing a titanium source, a manganese-based positive electrode active material and / or an iron-based positive electrode active material, and a solvent to obtain a mixed solution;

[0054] (ii) mixing the mixed solution with aqueous ammonia, and then performing solid-liquid separation and drying to obtain a precursor;

[0055] (iii) mixing the precursor with a fluorine source, and calcining the resulting mixture to obtain an active material.

[0056] According to the present invention, in the above step (i), it is preferred to first perform a first mixing of the titanium source and the solvent, and then add the manganese-based positive electrode active material and / or the iron-based positive electrode active material for a second mixing to obtain the mixed solution; wherein, preferably, the first mixing time is 0.5-1h; the second mixing time is 1-2h; the solvent may be an alcohol solution.

[0057] According to the present invention, in the above step (ii), preferably, aqueous ammonia is slowly added to the mixed solution for the third mixing, and then the obtained mixed system is centrifuged, and the separated solid phase is washed and dried to obtain a precursor; wherein, preferably, the amount of aqueous ammonia is such that the pH value of the mixed system obtained by the third mixing is 7.5-8.5; the time of the third mixing is 2-3h; and the drying temperature is 100-120°C.

[0058] According to the present invention, in the above step (iii), the precursor is preferably ball-milled with a fluorine source and then calcined in an oxygen-containing atmosphere, and the calcined product obtained is the active material; wherein the calcination conditions include: a temperature of 200-400°C and a time of 3-5h.

[0059] According to the present invention, during the preparation of the active material, the titanium source is selected from at least one of tetrabutyl titanate and / or titanium tetrachloride, preferably tetrabutyl titanate; the fluorine source is selected from at least one of ammonium fluoride, ammonium hydrogen fluoride and tetramethylammonium fluoride, preferably ammonium fluoride.

[0060] According to the present invention, in the preparation process of the active material, the titanium source, the manganese-based positive electrode active material and / or the iron-based positive electrode active material, and the fluorine source are fed in such an amount that the TiOF 2 The content is 0.1-10wt%.

[0061] According to the present invention, the slurry containing the active material further contains a conductive agent and a first binder.

[0062] According to the present invention, in step (1), the composition and amount of the slurry containing the active material are such that, based on the total weight of the active material layer, in the active material layer, TiOF 2 The content of is 3-5wt%, the content of the conductive agent is 2-20wt%, the content of the first binder is 2-15wt%, and the thickness of the active material layer is 60-100 μm.

[0063] According to the present invention, in step (1), the solvent used to prepare the slurry containing the active material, the preparation of the slurry and the coating can all adopt conventional material selection, operation and parameters in the art, and the present invention does not make any special limitation on this.

[0064] According to the present invention, in steps (2-1) and (2-2), for the slurry containing LiPSCl, the concentration of LiPSCl is preferably 5-50 wt %.

[0065] According to the present invention, the slurry containing LiPSCl further contains a second binder.

[0066] According to the present invention, the slurry containing LiPSCl can be prepared by mixing the components contained therein. Preferably, the LiPSCl powder can be mixed with the second binder first, and then added to the organic solvent and continued to mix to obtain a uniform slurry. Wherein, the organic solvent can be selected from at least one of toluene, xylene, trimethylbenzene, chlorobenzene, acetone, acetonitrile, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, diethylformamide, tetrahydrofuran and dimethyl sulfoxide.

[0067] According to the present invention, in steps (2-1) and (2-2), the coating can be carried out using conventional operations and parameters in the art, and the film is dried after coating to remove the organic solvent in the wet film. Preferably, the drying conditions include: a temperature of 90-120° C. and a time of 1-3 hours.

[0068] According to the present invention, in step (2-2), the hot pressing conditions include: pressure of 0.1-5 MPa, temperature of 25-65° C., and time of 0.1-0.5 h.

[0069] According to the present invention, in order to enable better adhesion between the active material layer and the composite layer, it is preferred to form the composite layer on the surface of the active material layer in the manner of step (2-1).

[0070] According to the present invention, in steps (2-1) and (2-2), the components and feeding amount of the slurry containing LiPSCl are such that, based on the total weight of the composite layer, the content of LiPSCl in the composite layer is 5-50wt%, the content of the second binder is 45-90wt%, and the thickness of the composite layer is 5-30um.

[0071] In the present invention, there is no particular limitation on the conductive agent and the binder, and they can be any conventional conductive agent and binder for lithium-ion battery pole pieces in the art. For example, the conductive agent can be selected from at least one of acetylene black, carbon nanotubes, graphene, conductive carbon black and conductive graphite; the first binder and the second binder can be independently selected from at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylate, polyurethane, polyethylene glycol, polyethylene oxide, epoxy resin, styrene-butadiene rubber, polymethyl cellulose, sodium polymethyl cellulose, hydroxypropyl methyl cellulose and polypropylene alcohol.

[0072] In the present invention, a composite layer having a selective isolation function is formed on the active material layer of the positive electrode sheet, wherein the LiPSCl contained in the composite layer has a high ionic conductivity, allowing a relatively small size of Li + LiPSCl forms a dense isolation layer at the microscopic level, which can prevent high-valent and large-sized metal ions from passing through the composite layer, thereby preventing them from migrating and depositing on the negative electrode of the battery.

[0073] According to a preferred embodiment of the present invention, on the basis that the components and feed amounts of the slurry containing active materials and the slurry containing LiPSCl meet the above-mentioned limitations, further, the feed amounts of the slurry containing active materials and the slurry containing LiPSCl are such that the TiOF 2 : The weight ratio of LiPSCl in the composite layer is 1:(0.1-2), which can better play the role of TiOF 2 The synergistic effect between the coated active material and the composite layer further inhibits the migration and deposition of high-positive metal ions, greatly improving the battery's cycle performance and storage performance.

[0074] The third aspect of the present invention provides a positive electrode sheet made by the method described in the second aspect.

[0075] According to the present invention, the structure, composition and performance of the positive electrode sheet prepared by the method described in the second aspect are the same as the positive electrode sheet described in the first aspect of the present invention, and will not be described in detail here.

[0076] A fourth aspect of the present invention provides a lithium-ion battery, which includes the positive electrode sheet described in the first aspect or the third aspect.

[0077] The lithium-ion battery provided by the present invention has a greatly reduced phenomenon of dissolution and deposition of high positive-valent metal ions from the positive electrode, and the capacity of the positive electrode material does not decay rapidly, so that the battery has significantly improved cycle performance and storage performance.

[0078] The present invention will be described in detail below by way of examples. In the following preparation examples, examples and comparative examples, unless otherwise specified, all reagents used are commercially available products.

[0079] Preparation Example 1

[0080] This preparation example is used to illustrate the 2 Preparation of manganese-based positive electrode active materials with coating layers

[0081] (i) adding 0.12 g of tetrabutyl titanate to 50 mL of ethanol aqueous solution, stirring and mixing for 1 h; then adding 3 g of lithium manganate, and continuing to stir and mix for 2 h to obtain a mixed solution;

[0082] (ii) slowly adding 0.8 mL of aqueous ammonia to the mixture, stirring for 2 h, and adjusting the pH value of the mixture to 7.5-8.5; then centrifuging the mixture, washing the separated solid phase with deionized water and ethanol in turn, and drying the washed solid phase in a drying oven at 120° C. under vacuum for 3 h to obtain a precursor;

[0083] (iii) The above precursor and ammonium fluoride were mixed by ball milling at a weight ratio of 1:1.5, and the mixed product was placed in a kiln and calcined at 350°C for 5 hours to obtain lithium manganese oxide @ TiOF 2 (denoted as A1).

[0084] A1 and raw material lithium manganese oxide were tested by scanning electron microscope, and the results are as follows: Figure 1 and Figure 2 As shown, Figure 1 This is the raw material lithium manganese oxide before coating. It can be observed that its particles have clear edges and corners. Figure 2 LiMnO3@TiOF 2 (i.e. A1), it can be observed that the edges of its particles are Figure 1 The edges of the raw material lithium manganese oxide particles in the process are smoother. This is due to the change in the particle appearance caused by the formation of a coating layer on the surface of the lithium manganese oxide. According to EDS testing, the chemical composition of the coating layer is TiOF 2 , TiOF in A1 2 The content of the coating layer is 4.3 wt%.

[0085] Preparation Example 2

[0086] This preparation example is used to illustrate the 2 Preparation of manganese-based positive electrode active materials with coating layers

[0087] (i) adding 0.15 g of tetrabutyl titanate to 50 mL of ethanol aqueous solution, stirring and mixing for 1 h; then adding 3 g of lithium manganate, and continuing to stir and mix for 2 h to obtain a mixed solution;

[0088] (ii) slowly adding 1 mL of aqueous ammonia to the mixture, stirring for 2 h, and adjusting the pH value of the resulting mixture to 7.5-8.5; then centrifuging the resulting mixture, washing the separated solid phase with deionized water and ethanol in turn, and drying the washed solid phase in a drying oven at 120° C. under vacuum for 3 h to obtain a precursor;

[0089] (iii) The above precursor and ammonium fluoride were mixed by ball milling at a weight ratio of 1:2, and the mixed product was placed in a kiln and calcined at 350°C for 5 hours to obtain lithium manganese oxide @ TiOF 2 (denoted as A2).

[0090] According to EDS test, TiOF in A2 2 The content of the coating layer is 7 wt%.

[0091] Preparation Example 3

[0092] This preparation example is used to illustrate the 2 Preparation of iron-based cathode active materials with coating layer

[0093] (i) adding 0.08 g of tetrabutyl titanate to 50 mL of ethanol aqueous solution, stirring and mixing for 1 h; then adding 3 g of lithium iron manganese phosphate, and continuing to stir and mix for 2 h to obtain a mixed solution;

[0094] (ii) slowly adding 0.5 mL of aqueous ammonia to the mixture, stirring for 2 h, and adjusting the pH value of the mixture to 7.5-8.5; then centrifuging the mixture, washing the separated solid phase with deionized water and ethanol in turn, and drying the washed solid phase in a drying oven at 120° C. under vacuum for 3 h to obtain a precursor;

[0095] (iii) The above precursor and ammonium fluoride were mixed by ball milling at a weight ratio of 1:0.5, and the mixed product was placed in a kiln and calcined at 350°C for 5 hours to obtain lithium manganese iron phosphate @TiOF 2 (denoted as A3).

[0096] According to EDS test, TiOF in A3 2 The content of the coating layer is 3 wt%.

[0097] Example 1

[0098] This example is used to illustrate the preparation of the positive electrode sheet.

[0099] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 92:5:3:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 4wt%, the content of conductive carbon black is 5wt%, and the content of PVDF is 3wt%);

[0100] (2) LiPSCl powder and PVDF were mixed at a weight ratio of 0.5:1, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 20 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 33 wt% and the content of PVDF was 67 wt%), thereby obtaining a positive electrode sheet (denoted as P1).

[0101] In P1, TiOF 2 :LiPSCl weight ratio is 1:0.5.

[0102] Example 2

[0103] This example is used to illustrate the preparation of the positive electrode sheet.

[0104] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 92:5:3:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 4wt%, the content of conductive carbon black is 5wt%, and the content of PVDF is 3wt%);

[0105] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.5:0.8, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the concentration of LiPSCl was 22wt%); the slurry was coated on the active material layer in step (1), and dried at 120°C for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 38wt% and the content of PVDF was 62wt%), thereby obtaining a positive electrode sheet (denoted as P2).

[0106] In P2, TiOF 2 :LiPSCl weight ratio is 1:0.8.

[0107] Example 3

[0108] This example is used to illustrate the preparation of the positive electrode sheet.

[0109] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 80:15:5:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 3.4wt%, the content of conductive carbon black is 15wt%, and the content of PVDF is 5wt%);

[0110] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.5:2.5, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 12.5 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 17 wt% and the content of PVDF was 83 wt%), thereby obtaining a positive electrode sheet (denoted as P3).

[0111] In P3, TiOF2 :LiPSCl weight ratio is 1:0.2.

[0112] Example 4

[0113] This example is used to illustrate the preparation of the positive electrode sheet.

[0114] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 70:18:12:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 3wt%, the content of conductive carbon black is 18wt%, and the content of PVDF is 12wt%);

[0115] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.5:0.6, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 24 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 45 wt% and the content of PVDF was 55 wt%), thereby obtaining a positive electrode sheet (denoted as P4).

[0116] In P4, TiOF 2 :LiPSCl weight ratio is 1:1.2.

[0117] Example 5

[0118] This example is used to illustrate the preparation of the positive electrode sheet.

[0119] (1) The active material A2, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 70:18:12:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 5wt%, the content of conductive carbon black is 18wt%, and the content of PVDF is 12wt%);

[0120] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.5:0.6, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 24 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 45 wt% and the content of PVDF was 55 wt%), thereby obtaining a positive electrode sheet (denoted as P5).

[0121] In P5, TiOF 2 :LiPSCl weight ratio is 1:0.3.

[0122] Example 6

[0123] This example is used to illustrate the preparation of the positive electrode sheet.

[0124] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 70:18:12:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 3wt%, the content of conductive carbon black is 18wt%, and the content of PVDF is 12wt%);

[0125] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.5:0.6, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 24 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 20 μm on the surface of the active material layer (wherein the content of LiPSCl was 45 wt% and the content of PVDF was 55 wt%), thereby obtaining a positive electrode sheet (denoted as P6).

[0126] In P6, TiOF 2 :LiPSCl weight ratio is 1:1.8.

[0127] Example 7

[0128] This example is used to illustrate the preparation of the positive electrode sheet.

[0129] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 70:18:12:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 3wt%, the content of conductive carbon black is 18wt%, and the content of PVDF is 12wt%);

[0130] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.2:1.8, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 24 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 10 wt% and the content of PVDF was 90 wt%), thereby obtaining a positive electrode sheet (denoted as P7).

[0131] In P7, TiOF 2 :LiPSCl weight ratio is 1:0.1.

[0132] Example 8

[0133] This example is used to illustrate the preparation of the positive electrode sheet.

[0134] (1) The active material A3, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 75:13:12:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 3.2wt%, the content of conductive carbon black is 13wt%, and the content of PVDF is 12wt%);

[0135] (2) LiPSCl powder and PVDF were mixed in a weight ratio of 0.5:0.6, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 24wt%); the slurry was coated on a stainless steel substrate, dried at 120°C for 3 hours to form a film layer, and then the film layer was hot pressed (hot pressing temperature of 60°C, hot pressing time of 0.5h, pressure of 1MPa) to form a composite layer with a thickness of 10μm on the surface of the active material layer (wherein the content of LiPSCl was 45wt%, and the content of PVDF was 55wt%), to obtain a positive electrode sheet (denoted as P8).

[0136] In P8, TiOF2 :LiPSCl weight ratio is 1:1.6.

[0137] Example 9

[0138] This example is used to illustrate the preparation of the positive electrode sheet.

[0139] (1) The active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 70:18:12:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector (wherein TiOF 2 The content of is 3wt%, the content of conductive carbon black is 18wt%, and the content of PVDF is 12wt%);

[0140] (2) LiPSCl powder and PVDF binder were mixed in a weight ratio of 1:18, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 24 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 5.2 wt% and the content of PVDF was 94.8 wt%), thereby obtaining a positive electrode sheet (denoted as P9).

[0141] In P9, TiOF 2 :LiPSCl weight ratio is 1:0.05.

[0142] Comparative Example 1

[0143] Lithium manganate, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 92:5:3:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector to obtain a positive electrode sheet (denoted as DP1).

[0144] Comparative Example 2

[0145] (1) lithium manganese oxide, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 92:5:3:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90° C. for 2 hours to form an active material layer with a thickness of 85 μm on the current collector;

[0146] (2) LiPSCl powder and PVDF were mixed at a weight ratio of 0.5:1, and then added to toluene and stirred for 5 hours to obtain a slurry containing LiPSCl (wherein the LiPSCl concentration was 20 wt%); the slurry was coated on the active material layer in step (1), and dried at 120° C. for 3 hours to form a composite layer with a thickness of 10 μm on the surface of the active material layer (wherein the content of LiPSCl was 33 wt% and the content of PVDF was 67 wt%), thereby obtaining a positive electrode sheet (denoted as DP2).

[0147] Comparative Example 3

[0148] The above-mentioned active material A1, conductive carbon black, PVDF, and N-methylpyrrolidone were mixed and stirred at a weight ratio of 92:5:3:22 for 4 hours to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on an aluminum foil current collector with a thickness of 15 μm, and dried at 90°C for 2 hours to form an active material layer with a thickness of 85 μm on the current collector to obtain a positive electrode sheet (denoted as DP3).

[0149] Test Case

[0150] The positive electrode sheets P1-P9 and DP1-DP3 are mixed with the negative electrode and sheet (graphite, conductive carbon black, PVDF and N-methylpyrrolidone are mixed in a weight ratio of 95:3:2:100 to prepare a negative electrode slurry, which is evenly coated on a copper foil, and then baked and rolled to prepare a negative electrode sheet), an electrolyte (lithium hexafluorophosphate (LiPF 6 ), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) mixed in a weight ratio of 10:30:30:30) were assembled into lithium-ion batteries (respectively designated as B1-B9 and DB1-DB3).

[0151] After the above lithium-ion batteries were placed at 45°C, formed in a high-temperature fixture and sealed for the second time, conventional capacity division was carried out, and then the cycle performance and storage performance tests were carried out.

[0152] 1. Cycle performance test:

[0153] At 25°C, the lithium-ion battery after the capacity division was allowed to stand for 120 minutes, then charged to 4.3V at a constant current of 0.5C, allowed to stand for 60 minutes after the charging, and then discharged to 3.0V at a constant current of 1C. After the above steps were cycled 300 times, the capacity retention rate of the 300th cycle was calculated (the 300th cycle capacity retention rate (%) = 300th cycle discharge capacity / first cycle discharge capacity × 100%). The results are shown in Table 1.

[0154] 2. Storage performance test:

[0155] The lithium-ion battery after the above capacity division was charged to 4.3V at 0.33C, left to stand for 60min, and then discharged to 3.0V at 0.33C (record the discharge capacity C 0 ), and then the battery was charged to 4.3V at 0.33C, and then left to stand for 60 minutes. The battery was then placed in a 45°C environment box, and after 28 days, it was taken out and discharged to 3.0V at 0.33C (record the discharge capacity C 1 ), let it stand for 60 minutes, charge to 4.3V at 0.33C, let it stand for 60 minutes, and finally discharge to 3.0V at 0.33C, let it stand for 60 minutes, end the test, and record the discharge capacity C 2 Calculate the 28-day storage capacity recovery rate at 45°C (Storage capacity recovery rate (%) = C 2 / C 0 ×100%), the results are shown in Table 1.

[0156] Table 1

[0157]

[0158] As can be seen from Table 1, the positive electrode sheet provided by the present invention has the advantages of TiOF 2 The specific active material layer is formed by coating, and a composite layer containing LiPSCl is arranged on the surface of the active material layer. Through the synergistic effect of the active material layer and the composite layer, the migration and deposition of high positive metal ions of the positive electrode to the negative electrode surface during the battery cycle can be significantly reduced, so that the cycle life and storage performance of the battery are significantly improved. Specifically, the battery B1-B9 can achieve a capacity retention rate of more than 85% after 300 cycles of 0.5C / 1C at 25°C, up to about 96%, and a 28-day storage capacity recovery rate of more than 83% at 45°C, up to about 94%. In particular, the positive electrode sheet used by DB1 is an ordinary positive electrode sheet, and the active material in the positive electrode sheet used by DB2 does not have TiOF 2 The coating layer, the positive electrode sheet used by DB3 does not contain a composite layer, resulting in their cycle life and storage performance being worse than B1-B9.

[0159] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A positive electrode sheet, characterized in that: The positive electrode sheet comprises: a current collector, an active material layer and a composite layer, wherein the active material layer is arranged between the current collector and the composite layer; wherein, The active material layer comprises an active material having a TiOF2 coating layer; the composite layer comprises LiPSCl; The active material having a TiOF2 coating layer includes a manganese-based positive electrode active material having a TiOF2 coating layer and / or an iron-based positive electrode active material having a TiOF2 coating layer.

2. The positive electrode sheet according to claim 1, wherein: The manganese-based positive electrode active material is selected from at least one of lithium-rich manganese-based positive electrode materials, lithium manganese oxide, lithium manganese nickel oxide and lithium iron manganese phosphate; And / or, the iron-based positive electrode active material is selected from at least one of lithium iron phosphate, lithium iron silicate and lithium iron borate.

3. The positive electrode sheet according to claim 1 or 2, wherein: The content of TiOF2 in the active material having a TiOF2 coating layer is 0.1-10wt%, preferably 4-6wt%.

4. The positive electrode sheet according to any one of claims 1 to 3, wherein: The active material layer further contains a conductive agent and a first binder; Preferably, based on the total weight of the active material layer, in the active material layer, the content of TiOF2 is 3-5wt%, preferably 3.5-4wt%; the content of the conductive agent is 2-20wt%; and the content of the first binder is 2-15wt%.

5. The positive electrode sheet according to any one of claims 1 to 4, wherein: The composite layer further comprises a second binder; Preferably, based on the total weight of the composite layer, in the composite layer, the content of LiPSCl is 5-50wt%, preferably 20-40wt%; and the content of the second binder is 45-90wt%.

6. The positive electrode sheet according to any one of claims 1 to 5, wherein: The weight ratio of TiOF2:LiPSCl is 1:(0.1-2).

7. The positive electrode sheet according to any one of claims 1 to 6, wherein: The thickness of the active material layer is 60-100 μm; And / or, the composite layer has a thickness of 5-30 μm.

8. A method for preparing a positive electrode sheet, characterized in that: include: (1) coating a slurry containing an active material on the surface of a current collector, and after drying, forming an active material layer on the surface of the current collector; Wherein, the active material comprises a manganese-based positive electrode active material having a TiOF2 coating layer and / or an iron-based positive electrode active material having a TiOF2 coating layer; (2-1) coating a slurry containing LiPSCl on the surface of the active material layer, and after drying, forming a composite layer on the surface of the active material layer to obtain a positive electrode sheet; or (2-2) A slurry containing LiPSCl is coated to form a film, and after drying, a film layer is formed; then, the film layer is hot-pressed to form a composite layer on the surface of the active material layer, thereby obtaining a positive electrode sheet.

9. The method according to claim 8, wherein: The manganese-based positive electrode active material is selected from at least one of lithium-rich manganese-based positive electrode materials, lithium manganese oxide, lithium manganese nickel oxide and lithium iron manganese phosphate; And / or, the iron-based positive electrode active material is selected from at least one of lithium iron phosphate, lithium iron silicate and lithium iron borate.

10. The method according to claim 8 or 9, wherein: The content of TiOF2 in the active material is 0.1-10 wt%, preferably 4-6 wt%, based on the total weight of the active material.

11. The method according to claim 10, wherein: The preparation process of the active material comprises: (i) mixing a titanium source, a manganese-based positive electrode active material and / or an iron-based positive electrode active material, and a solvent to obtain a mixed solution; (ii) mixing the mixed solution with aqueous ammonia, and then performing solid-liquid separation and drying to obtain a precursor; (iii) mixing the precursor with a fluorine source, and calcining the resulting mixture to obtain an active material.

12. The method according to claim 11, wherein: The titanium source, manganese-based positive electrode active material and / or iron-based positive electrode active material and fluorine source are fed in such amounts that the content of TiOF2 in the prepared active material is 0.1-10wt%; And / or, the titanium source is selected from tetrabutyl titanate and / or titanium tetrachloride; And / or, the fluorine source is selected from at least one of ammonium fluoride, ammonium bifluoride and tetramethylammonium fluoride; And / or, the calcination conditions include: temperature of 200-400° C. and time of 3-5 h.

13. The method according to any one of claims 8 to 12, wherein: The slurry containing the active material also contains a conductive agent and a first binder; Preferably, the components and feeding amount of the slurry containing active material are such that, based on the total weight of the active material layer, the content of TiOF2 in the active material layer is 3-5wt%, the content of the conductive agent is 2-20wt%, the content of the first binder is 2-15wt%, and the thickness of the active material layer is 60-100μm.

14. The method according to any one of claims 8 to 13, wherein: The slurry containing LiPSCl also contains a second binder; Preferably, the components and feeding amount of the slurry containing LiPSCl are such that, based on the total weight of the composite layer, the content of LiPSCl in the composite layer is 5-50wt%, the content of the second binder is 45-90wt%, and the thickness of the composite layer is 5-30μm.

15. The method according to any one of claims 8 to 14, wherein: The feeding amounts of the slurry containing the active material and the slurry containing LiPSCl are such that the weight ratio of TiOF2 in the active material layer to LiPSCl in the composite layer is 1:(0.1-2).

16. A positive electrode sheet prepared by the method according to any one of claims 8 to 15.

17. A lithium ion battery comprising the positive electrode sheet according to any one of claims 1 to 7 and 16.

Citation Information

Patent Citations

  • Lithium ion battery

    CN102544576A

  • Positive pole, preparation method thereof and lithium-ion battery

    CN103022415A

  • Modifying method for restraining discharge medium voltage attenuation of positive electrode material

    CN105552311A

  • Cathode material for lithium sulphur cells

    CN106663789A

  • Positive electrode active material, method of manufacturing the same and all-solid battery including the same

    CN108206269A