Conductive carbon material and preparation method thereof, pole piece, battery and electric device
The capture of manganese ions by conductive carbon materials with high porosity and high nitrogen content solves the problem of poor circulation performance of manganese-containing positive electrode active materials, improves the energy density and cycle stability of the battery, and achieves cost reduction and improved conductivity.
Patent Information
- Application Number
- CN202310637466.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
The manganese-containing positive electrode active material has poor circulation performance during the charge and discharge cycle, which causes manganese ions to migrate to the negative electrode sheet, causing problems of battery cycle life and capacity to decrease.
Using conductive carbon materials with a porosity of more than or equal to 90%, combined with conductive carbon materials with high nitrogen content and appropriate pore size, it is prepared by heating treatment of covalent organic frame materials. It is used to capture manganese ions and improve conductivity and reduce free manganese ions. The quantity of the conductive agent is directly applied to the electrode sheet.
It effectively improves the energy density and cycle stability of the battery, reduces the damage of manganese ions to the negative electrode sheet, reduces the cost of the battery, and does not require additional conductive agents.
Smart Images

Figure BDA0004260808970000071 
Figure BDA0004260808970000141 
Figure BDA0004260808970000151
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and specifically, to conductive carbon materials and preparation methods thereof, pole pieces, batteries, and electrical devices. Background Art
[0002] With the development of lithium-ion battery technology, lithium-ion batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations due to their high energy density, long cycle life and green environmental protection. They are also widely used in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the advantages of low cost, high reliability and high working voltage, manganese-containing positive electrode active materials are considered to be a promising positive electrode active material for power lithium-ion batteries. However, the poor cycle performance of manganese-containing positive electrode active materials means that there are still many problems to be solved in the application of manganese-containing positive electrode active material batteries.
[0003] The above statements are only used to provide background information related to the present application and do not necessarily constitute prior art. Summary of the invention
[0004] In a first aspect of the present application, the present application provides a conductive carbon material, wherein the porosity of the conductive carbon material is greater than or equal to 90%, and the mass fraction of nitrogen in the conductive carbon material is 0.5%-5%, and optionally, the mass fraction of nitrogen in the conductive carbon material is 0.5%-1%. Thus, the conductive carbon material can capture manganese ions and reduce the number of free manganese ions.
[0005] According to an embodiment of the present application, the pore size of the conductive carbon material is 0.1 nm-1 nm. Therefore, the internal pore structure of the conductive carbon material can be used to capture manganese ions, further reducing the amount of free manganese ions.
[0006] According to an embodiment of the present application, the particle size of the conductive carbon material is 4 μm-10 μm, preferably, the particle size of the conductive carbon material is 5 μm-8 μm. Therefore, the conductive carbon material has high dispersibility and processability.
[0007] According to an embodiment of the present application, the specific surface area of the conductive carbon material is 1200 m 2 / g-1800m 2 / g. As a result, the conductive carbon material can capture more manganese ions.
[0008] According to an embodiment of the present application, the electronic conductivity of the conductive carbon material is greater than or equal to 550 S / m. Therefore, the conductive carbon material has a relatively good electrical conductivity.
[0009] In the second aspect of the present application, the present application proposes a method for preparing the aforementioned conductive carbon material, comprising: providing a covalent organic framework material, and heating the covalent organic framework material. Thus, the aforementioned conductive carbon material can be prepared by a relatively simple method.
[0010] According to an embodiment of the present application, providing a covalent organic framework material comprises: mixing a first monomer and a second monomer; wherein at least one of the following conditions is met: the first monomer comprises p-phenylenediamine, 4,4'-diaminobiphenyl, 1,3,5-triaminobenzene, 1,3,5-tri(4-aminophenyl)benzene, 1,3,5,7-tetra(4-aminophenyl)methane, 1,3,5,7-tetra(4-aminophenyl)adamantane, 1,3,6,8-tetraaminopyrene, 5,10,15,20- The second monomer includes at least one of terephthalaldehyde, 4,4'-biphenyldicarboxaldehyde, 1,3,5-trialdehyde benzene, 1,3,5-tri(4-formylphenyl)benzene, tetra(4-formylphenyl)methane, tetra(4-formylphenyl)adamantane, trialdehyde phloroglucinol, 2,4,6-triformyl phloroglucinol, 1,3,6,8-tetra(4-formaldehydephenyl)pyrene, and 5,10,15,20-tetra(4-formylphenyl)porphyrin. Thus, a covalent organic framework material can be prepared by a simple method.
[0011] According to an embodiment of the present application, when the first monomer and the second monomer are mixed, the molar number of the first monomer is n1, the molar number of the second monomer is n2, and n1:n2=(1-5):3. Thus, a covalent organic framework material with a higher nitrogen content can be obtained.
[0012] According to an embodiment of the present application, the heating treatment satisfies at least one of the following conditions: the temperature of the heating treatment is 500°C-1000°C; the time of the heating treatment is 3h-8h; the heating rate of the heating treatment is 1°C / min-5°C / min. This helps to obtain a conductive carbon material with a moderate pore structure and high conductivity.
[0013] In a third aspect of the present application, the present application proposes a pole piece, the pole piece comprising the aforementioned conductive carbon material, and / or the conductive carbon material prepared by the aforementioned method, thereby obtaining a pole piece with higher energy density and cycle stability.
[0014] According to an embodiment of the present application, the electrode sheet is a positive electrode sheet, and the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located at least on one side of the positive electrode current collector, and the positive electrode active material layer includes the conductive carbon material. Thus, a positive electrode sheet with a higher positive electrode active material loading can be obtained.
[0015] According to an embodiment of the present application, the mass fraction of the conductive carbon material in the positive electrode active material layer is 0.2%-3.5%, thereby improving the conductivity of the positive electrode sheet and the energy density of the battery.
[0016] According to an embodiment of the present application, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes at least one of lithium manganese oxide and lithium manganese phosphate. Thus, the operating voltage of a battery containing the electrode sheet can be increased.
[0017] According to an embodiment of the present application, the mass fraction of the positive electrode active material in the positive electrode active material layer is 96.5%-98.5%, thereby increasing the energy density of the positive electrode sheet.
[0018] According to an embodiment of the present application, the electrode sheet is a negative electrode sheet, and the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located at least on one side of the negative electrode current collector, and the negative electrode active material layer includes the conductive carbon material. Thus, the conductivity of the negative electrode sheet and the cycle performance of the battery can be improved.
[0019] According to an embodiment of the present application, the electrode sheet is a negative electrode sheet, and the negative electrode sheet includes a negative electrode current collector and a functional coating located at least on one side of the negative electrode current collector, and the functional coating includes the conductive carbon material. Thus, the conductivity of the negative electrode sheet and the volume energy density of the battery can be improved.
[0020] According to an embodiment of the present application, the pole piece further includes a conductive agent, the mass of the conductive carbon material in the pole piece is m1, the mass of the conductive agent in the pole piece is m2, and m1:m2=(0.5-2.5): 1. Thus, the cycle stability of the pole piece can be improved and the cost of the pole piece can be reduced.
[0021] In a fourth aspect of the present application, the present application proposes a battery, comprising the aforementioned pole piece, thereby obtaining a battery with higher energy density and better cycle performance.
[0022] In the fifth aspect of the present application, the present application proposes an electrical device, comprising the aforementioned battery. Therefore, the electrical device has all the features and advantages of the aforementioned battery, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0024] Figure 1 A schematic diagram of a battery according to an embodiment of the present application is shown;
[0025] Figure 2 yes Figure 1 An exploded view of a battery according to an embodiment of the present application is shown;
[0026] Figure 3 A schematic diagram of a battery module according to an embodiment of the present application is shown;
[0027] Figure 4 A schematic diagram of a battery pack according to an embodiment of the present application is shown;
[0028] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown;
[0029] Figure 6 A schematic diagram of an electric device using a battery as a power source according to an embodiment of the present application is shown.
[0030] Description of reference numerals:
[0031] Battery pack 1, upper box body 2, lower box body 3, battery module 4, battery 5, shell 51, electrode assembly 52, top cover assembly 53. DETAILED DESCRIPTION
[0032] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0033] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.
[0034] In the description of this application, in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. "First feature" and "second feature" may include one or more of the features.
[0035] In the description of the present application, “plurality” means two or more.
[0036] Unless otherwise specified, all scientific and technological terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. All patents and publications related to this application are incorporated herein by reference in their entirety. The term "comprising" or "including" is an open expression, i.e., including the content specified in this application, but does not exclude the content of other aspects.
[0037] In the description of this application, regardless of whether the words "about" or "approximately" are used, all the numbers disclosed herein are approximate values. The value of each number may differ by less than 10% or a reasonable difference considered by those skilled in the art, such as 1%, 2%, 3%, 4% or 5%.
[0038] Positive electrode active materials containing manganese have advantages such as high discharge voltage and low cost, but they also have disadvantages such as poor cycle performance during charge and discharge cycles. Take lithium manganate as an example. In spinel structured lithium manganate, manganese ions are easily separated from the crystal structure. For example, the average valence state of manganese in lithium manganate is +3.5, and a portion of Mn exists in the +3 valence form, while Mn 3+ Very unstable, easily undergoes disproportionation reaction to generate Mn 4+ (solid) and Mn 2+ (solution), the generated Mn 2+ Dissolved in liquid electrolytes; for example, when water is contained in a liquid electrolyte containing lithium hexafluorophosphate as a lithium salt, water reacts with the lithium salt to generate HF, which reacts with lithium manganate to form Mn dissolved in the electrolyte. 2+ As well as the generation of water, the generated water will further aggravate the side reactions, thus creating a vicious cycle. When manganese ions are dissolved in the liquid electrolyte, they will migrate to the surface of the negative electrode plate, and then be reduced to metallic manganese on the surface of the negative electrode plate and deposited on the negative electrode plate. The deposited metallic manganese will cause the solid electrolyte membrane of the negative electrode plate to be destroyed, the lithium insertion channel of the negative electrode active material to be blocked, and the negative electrode active material layer to be deposited on the interface between the negative electrode active material layer and the negative electrode current collector, causing the negative electrode active material layer to peel off, etc., resulting in a significant decrease in the battery cycle life and capacity.
[0039] Typically, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0040] In some embodiments, in order to improve the conductivity of the electrode sheets, a coating containing a conductive agent may be provided on the surface of the positive electrode sheet and the negative electrode sheet.
[0041] Based on the above considerations, in this application, a conductive carbon material with a higher porosity and a higher nitrogen content is proposed. Taking the positive electrode active material as an example, when the manganese ions are separated from the crystal structure during the charge and discharge cycle, the conductive carbon material with a higher porosity can adsorb the manganese ions into the internal pore structure of the conductive carbon material. Since the conductive carbon material has a higher nitrogen content, the nitrogen atoms will chelate with the free manganese ions, and then capture the manganese ions and fix them in the conductive carbon material, thereby reducing the free manganese ions in the liquid electrolyte, and then reducing the damage of manganese ions to the structure of the negative electrode sheet. While the conductive carbon material can capture manganese ions, it can also be used as a conductive agent, without the need to add other conductive agent materials to the surface coating of the positive electrode sheet and the negative electrode sheet, thereby greatly improving the energy density and cycle performance of the battery.
[0042] The battery disclosed in the embodiments of the present application can be used in an electrical device that uses the battery as a power source, or a power supply system that uses the battery disclosed in the present application to form the electrical device, or various energy storage systems that use the battery as an energy storage element. Electrical devices may include mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, etc. Among them, electric toys may include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc., and spacecraft may include airplanes, rockets, space shuttles, and spacecrafts, etc.
[0043] It should be understood that the technical solutions described in the embodiments of the present application are not limited to the batteries and electrical devices described above, but can also be applied to all other batteries and electrical devices using batteries. However, for the sake of simplicity, the following embodiments are described using electric vehicles as examples.
[0044] In the first aspect of the present application, the present application proposes a conductive carbon material, the porosity of the conductive carbon material is greater than or equal to 90%, and the mass fraction of nitrogen in the conductive carbon material is 0.5%-5%. While acting as a conductive agent, the conductive carbon material can also use its own pore structure to adsorb manganese ions, and use the chelation effect of nitrogen atoms to effectively capture manganese ions, and fix free manganese ions inside the conductive carbon material. When used as a conductive agent in a manganese-containing battery, when the manganese ions in the manganese-containing positive active material escape from the crystal structure, the manganese ions will be in a free state, and the nitrogen atoms rich in the conductive carbon material can capture free manganese ions, thereby reducing the number of free manganese ions, thereby reducing the occurrence of adverse effects such as increased negative electrode sheet resistance and reduced lithium insertion capacity due to the migration of manganese ions to the negative electrode sheet, thereby improving the battery's cycle performance.
[0045] In some embodiments, the mass fraction of nitrogen in the conductive carbon material may be 0.5%-5%. In other embodiments, the mass fraction of nitrogen in the conductive carbon material may be 0.5%-1%.
[0046] As an example, the mass fraction of nitrogen in the conductive carbon material can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0% or 5%.
[0047] As an example, the porosity of the conductive carbon material may be 90%, 90.5%, 91%, 91.5%, 92%, 92.5%, 93%, 93.5%, 94%, 95%, 96% or 97%.
[0048] As an example, the porosity of the conductive carbon material of the present application is a well-known meaning in the art and can be measured by instruments and methods well-known in the art. For example, the porosity of the conductive carbon material can be obtained by a conventional water immersion test, specifically, the dry weight M0 of the sample to be tested is recorded, the mass M1 is recorded after the sample to be tested is heated and boiled in deionized water for at least 2 hours, the mass M2 is recorded after the moisture of the sample to be tested is wiped off, and the porosity is obtained by dividing the difference between M2-M0 by the difference between M2-M1.
[0049] As an example, the mass fraction of nitrogen in the conductive carbon material of the present application has a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, the mass fraction of nitrogen in the conductive carbon material can be tested and obtained by referring to the following method: the weight percentage of nitrogen in the conductive carbon material can be measured by performing elemental analysis on the conductive carbon material using a scanning electron microscope.
[0050] In some embodiments, the pore size of the conductive carbon material may be 0.1 nm-1 nm.
[0051] The pore structure inside the conductive carbon material can be used to capture manganese ions. When the pore size of the conductive carbon material is 0.1nm-1nm, the pore structure inside the conductive carbon material is mainly micropores. By utilizing the confinement effect of the micropore channel, the adsorption capacity of the conductive carbon material for manganese ions can be effectively improved.
[0052] As an example, the pore size of the conductive carbon material may be 0.1 nm, 0.2 nm, 0.3 nm, 0.4 nm, 0.5 nm, 0.6 nm, 0.7 nm, 0.8 nm, 0.9 nm, or 1 nm.
[0053] As an example, the pore size of the conductive carbon material of the present application is a well-known meaning in the art and can be measured by instruments and methods well-known in the art. For example, the pore size of the conductive carbon material can be tested by referring to the following method: the pore size of the conductive carbon material is obtained by nitrogen adsorption and desorption test, wherein at least 50 mg of the sample to be tested should be taken during the test, and the sample to be tested should be vacuum dried at 150° C. for 3 hours before the test.
[0054] In some embodiments, the particle size of the conductive carbon material may be 4 μm-10 μm, and in other embodiments, the particle size of the conductive carbon material may be 5 μm-8 μm.
[0055] As an example, the particle size of the conductive carbon material may be 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm or 10 μm.
[0056] When the particle size of the conductive carbon material is 4μm-10μm, when preparing the slurry, the conductive carbon material has good dispersibility in the slurry solvent and is not prone to sedimentation; when the coating formed by the slurry is roller-pressed, the conductive carbon material of the above particle size helps to increase the compaction density of the coating.
[0057] As an example, the particle size of the conductive carbon material of the present application is a well-known meaning in the art and can be measured using instruments and methods well-known in the art. For example, the particle size of the conductive carbon material can be obtained by testing according to the following method: 10 mg of the conductive carbon material to be tested is uniformly dispersed in anhydrous ethanol, and then the suspension is added to the surface of the microgrid copper mesh, and after drying, a transmission electron microscope test is performed, and the copper mesh is observed under the transmission electron microscope to obtain the particle size of the conductive carbon material.
[0058] In some embodiments, the specific surface area of the conductive carbon material can be 1200 m 2 / g-1800m 2 / g.
[0059] When the specific surface area of the conductive carbon material is 1200m 2 / g-1800m 2 / g, the conductive carbon material has a larger specific surface area, which can expose more chelating sites that can bind to free manganese ions, thereby capturing more free manganese ions.
[0060] As an example, the specific surface area of the conductive carbon material of the present application is a well-known meaning in the art and can be measured by instruments and methods well-known in the art. For example, the specific surface area of the conductive carbon material can be tested by referring to the following method: the specific surface area of the conductive carbon material is obtained by nitrogen adsorption and desorption test, wherein at least 50 mg of the sample to be tested should be taken during the test, and the sample to be tested should be vacuum dried at 150°C for 3 hours before the test.
[0061] In some embodiments, the electronic conductivity of the conductive carbon material may be greater than or equal to 550 S / m.
[0062] When the electronic conductivity of the conductive carbon material is greater than or equal to 550 S / m, the conductive carbon material has excellent conductivity and can be used as a conductive agent in positive and negative electrode sheets without the need to add other conductive agents, thereby effectively improving the energy density of the battery.
[0063] As an example, the electronic conductivity of the conductive carbon material of the present application is a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, the electronic conductivity of the conductive carbon material can be tested by referring to the following method: placing the conductive carbon material powder in a test mold, using stainless steel gaskets on both sides as blocking electrodes, and pressing at a pressure of 350MPa for 3min to form a conductive mold battery. The electronic conductivity is obtained by performing a constant voltage DC test on the mold battery using an electrochemical workstation;
[0064] The calculation formula is shown below:
[0065]
[0066] Among them, σ represents conductivity, d represents the thickness of the electrode to be tested, R represents electrochemical impedance (the electronic impedance value is measured by the electrochemical workstation), and S represents the effective area of the electrode to be tested.
[0067] In the second aspect of the present application, the present application proposes a method for preparing the aforementioned conductive carbon material, by in-situ pyrolysis of a covalent organic framework to form a conductive carbon material, and utilizing the confinement effect of the microporous channels of the carbon skeleton of the conductive carbon material to produce a strong interaction between the dissolved manganese ions and the carbon atoms, so that the free manganese ions are highly dispersed in the pores of the carbon skeleton of the conductive carbon material, and then the manganese ions are fixed in the internal pore structure of the conductive carbon material through the chelation of nitrogen atoms and manganese ions, effectively reducing the reduction deposition of free manganese ions on the surface of the negative electrode. In addition. The conductive carbon material derived from the covalent organic framework has a porous framework with well-arranged channels inside, which can provide a continuous channel for electron movement, thereby improving the electronic conductivity of the conductive carbon material. Specifically, the method for preparing the aforementioned conductive carbon material may include:
[0068] S100: Providing covalent organic framework materials
[0069] In some embodiments, providing the covalent organic framework material includes mixing the first monomer and the second monomer, for example, adding the first monomer and the second monomer into a solvent and mixing them.
[0070] In some embodiments, the first monomer may be a monomer containing an amino group, thereby providing more nitrogen atoms for the final covalent organic framework. For example, the first monomer may include at least one of p-phenylenediamine, 4,4'-diaminobiphenyl, 1,3,5-triaminobenzene, 1,3,5-tris(4-aminophenyl)benzene, 1,3,5,7-tetrakis(4-aminophenyl)methane, 1,3,5,7-tetrakis(4-aminophenyl)adamantane, 1,3,6,8-tetraaminopyrene, and 5,10,15,20-tetrakis(4-aminophenyl)porphyrin.
[0071] In some embodiments, a crystalline material having an ordered pore structure, i.e., a covalent organic framework (COF) material, can be formed by a first monomer and a second monomer through a covalent bond. For example, the second monomer may include at least one of terephthalaldehyde, 4,4'-biphenyldicarboxaldehyde, 1,3,5-trialdehyde benzene, 1,3,5-tri(4-formylphenyl)benzene, tetra(4-formylphenyl)methane, tetra(4-formylphenyl)adamantane, trialdehyde phloroglucinol, 2,4,6-triformyl phloroglucinol, 1,3,6,8-tetra(4-formaldehydephenyl)pyrene, and 5,10,15,20-tetra(4-formylphenyl)porphyrin;
[0072] In some embodiments, the organic monomer is added to an organic solvent or a non-aqueous solution, and the covalent organic framework material is obtained by mixing. For example, the solvent may include at least one of an alcohol solvent, an ether solvent, an ester solvent, and an aromatic hydrocarbon solvent.
[0073] As an example, the solvent may include at least two of methanol, ethanol, toluene, n-butanol, o-dichlorobenzene, 1,4-dioxane, and mesitylene.
[0074] As an example, the mixing process may include heating, grinding (such as ball milling), solvent addition, centrifugation, washing, drying and the like. The synthesis efficiency and yield of the covalent organic framework material may be improved through the mixing process.
[0075] In some embodiments, when the first monomer and the second monomer are mixed, the mole number of the first monomer is n1, the mole number of the second monomer is n2, and n1:n2=(1-5):3.
[0076] When the first monomer and the second monomer are mixed, when the molar number n1 of the first monomer and the molar number n2 of the second monomer satisfy the above-mentioned proportional relationship, the nitrogen content in the covalent organic framework material is relatively high, and the mass fraction of nitrogen in the conductive carbon material obtained after in-situ pyrolysis of the covalent organic framework can be 0.5%-5%.
[0077] S200: Heat treatment of covalent organic framework materials
[0078] In some embodiments, the conductive carbon material can be obtained by heat treating the covalent organic framework.
[0079] In some embodiments, the temperature of the heat treatment may be 500°C-1000°C.
[0080] As an example, the temperature of the heat treatment may be 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, or 1000°C.
[0081] When the heating temperature is 500℃-1000℃, the degree of in-situ pyrolysis of the covalent organic framework material is high, and the heteroatoms can be volatilized as much as possible, reducing the residual organic monomers. While retaining the original covalent organic framework carbon skeleton, a conductive carbon material with a high degree of graphitization is generated, which has good conductivity.
[0082] In some embodiments, the heating treatment time may be 3 hours to 8 hours.
[0083] As an example, the heating treatment time can be 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h or 8 h.
[0084] When the heating treatment time is 3h-8h, the covalent organic framework material can be fully pyrolyzed in situ to generate a conductive carbon material with a high degree of graphitization and a moderate pore structure without causing excessive energy consumption.
[0085] In some embodiments, the heating rate of the heating process may be 1° C. / min-5° C. / min.
[0086] As an example, the heating rate of the heating treatment may be 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min.
[0087] When the heating rate of the heating treatment is 1°C / min-5°C / min, the conductive carbon material obtained by the heating treatment has good density, the crystal form and pore structure are easy to control, and the energy consumption is low, so that a conductive carbon material with a high degree of graphitization can be obtained.
[0088] In some embodiments, the pore size of the covalent organic framework material changes before and after the heat treatment. For example, the pore size of the conductive carbon material is about 15%-20% lower than that of the covalent organic framework material. When selecting the monomer ratio, monomer type and heat treatment conditions of the covalent organic framework material, it is necessary to make adaptive adjustments to the pore size of the conductive carbon material to meet the pore size of the conductive carbon material after the heat treatment of 0.1nm-1nm.
[0089] In some embodiments, the method for providing a covalent organic framework material is not particularly limited, as long as the conductive carbon material obtained after the covalent organic framework material is heated can meet the aforementioned requirements. For example, the covalent organic framework material can be synthesized by the aforementioned method, or a commercially available covalent organic framework material can be used.
[0090] Those skilled in the art will appreciate that, in the above method of a specific embodiment, the order in which the steps are written does not imply a strict execution order and does not constitute any limitation on the implementation process. The specific execution order of the steps should be determined by their functions and possible internal logic.
[0091] In a third aspect of the present application, the present application proposes a pole piece, which includes the aforementioned conductive carbon material and / or the conductive carbon material prepared by the aforementioned method, thereby obtaining a pole piece with higher energy density and cycle stability.
[0092] In some embodiments, the electrode sheet may be a positive electrode sheet, and the positive electrode sheet may include a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector.
[0093] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is disposed on any one or both of the two facing surfaces of the positive electrode current collector.
[0094] According to some embodiments of the present application, the positive electrode active material layer includes a conductive carbon material. While serving as a conductive agent, the conductive carbon material can also absorb manganese ions using its own pore structure and effectively capture manganese ions through nitrogen atoms, thereby fixing free manganese ions inside the conductive carbon material.
[0095] In some embodiments, the mass fraction of the conductive carbon material in the positive electrode active material layer is 0.2%-3.5%.
[0096] As an example, the mass fraction of the conductive carbon material in the positive electrode active material layer can be 0.2%, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.8%, 3.0%, 3.2% or 3.5%.
[0097] When the mass fraction of the conductive carbon material in the positive electrode active material layer is 0.2%-3.5%, the conductive carbon material can effectively improve the conductivity of the positive electrode active material layer, reduce the internal resistance of the positive electrode active material layer and the resistor, and at the same time, the conductive carbon material has a small adsorption force on the binder in the positive electrode active material layer, thereby improving the toughness and structural stability of the positive electrode active material layer.
[0098] As an example, the positive electrode current collector can be a metal foil, a foam metal or a composite current collector. For example, as a metal foil, aluminum or stainless steel, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium with a silver surface treatment can be used. The composite current collector may include a polymer material base and a metal layer. The foam metal may be a nickel foam, a copper foam, an aluminum foam, an alloy foam, or carbon foam. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0099] In some embodiments, the positive electrode active material layer may include a positive electrode active material including at least one of lithium manganese oxide and lithium manganese phosphate.
[0100] As an example, the lithium manganese oxide may include a nickel-cobalt-manganese ternary material, a lithium-rich manganese-based solid solution, lithium manganate, a sodium-rich manganese-based layered oxide, and the like.
[0101] As an example, the lithium manganese phosphate may include lithium manganese phosphate, lithium manganese iron phosphate, and the like.
[0102] In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer may be 96.5%-98.5%.
[0103] In some embodiments, the electrode sheet is a negative electrode sheet, and the negative electrode sheet may include a negative electrode current collector and a negative electrode active material layer located at least on one side of the negative electrode current collector, and the negative electrode active material layer may include a conductive carbon material. The conductive carbon material in the negative electrode active material layer can adsorb and capture manganese ions that migrate to the negative electrode sheet, and even if the manganese ions are reduced and deposited, it will not cause significant damage to the structure of the negative electrode sheet.
[0104] As an example, the negative electrode active material layer may include a negative electrode active material, which may be a material with a high gram capacity. For example, the negative electrode active material may include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate.
[0105] As an example, the silicon-based material may include at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy material; the tin-based material may include at least one of elemental tin, tin oxide, and tin alloy material.
[0106] In some embodiments, the pole piece may be a negative pole piece, and a negative active material layer may not be actively provided on the negative pole piece side, that is, a "negative pole-free" sodium battery is formed. For example, in the manufacturing process of the battery 5, a negative active material layer is not provided on the negative current collector by coating or deposition. During the first charge, the sodium ions obtain electrons on the anode side and deposit metallic sodium on the surface of the negative current collector to form a sodium metal phase. During discharge, the metallic sodium can be converted into sodium ions and return to the positive pole piece, thereby realizing cyclic charge and discharge. Compared with other sodium batteries, the "negative pole-free" sodium battery can obtain a higher energy density due to the absence of a negative active material layer. In order to improve the performance of the battery 5, for the "negative pole-free" sodium battery, the negative pole piece may include a negative current collector and a functional coating located at least on one side of the negative current collector, and the functional coating may include a conductive carbon material. The conductive carbon material in the functional coating can adsorb and capture manganese ions that migrate to the negative pole piece, and even if the manganese ions are reduced and deposited, the structure of the negative pole piece will not be greatly damaged.
[0107] In some embodiments, the negative electrode plate may include a negative electrode current collector, and the negative electrode current collector may be a metal foil, a foam metal, or a composite current collector. For example, as a metal foil, aluminum or stainless steel treated with silver surface, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc. may be used. The foam metal may be foam nickel, foam copper, foam aluminum, foam alloy, or foam carbon, etc. The composite current collector may include a polymer material base layer and a metal layer, and the composite current collector may be formed by placing a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0108] In some embodiments, the negative electrode plate may be a rolled metal foil or a surface-coated inert layer of metal powder coated on a current collector.
[0109] In some embodiments, the negative electrode current collector may be a composite current collector, for example, the composite current collector may include at least one of carbon cloth, carbon film, carbonaceous material, porous current collector, alloyed modified current collector, lithium-philic modified current collector and sodium-philic modified current collector.
[0110] In some embodiments, the pole piece may further include a conductive agent, the mass of the conductive carbon material in the pole piece is m1, the mass of the conductive agent in the pole piece is m2, and m1:m2=(0.5-2.5): 1. Thus, the cycle stability of the pole piece can be improved and the cost of the pole piece can be reduced.
[0111] As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0112] In a fourth aspect of the present application, the present application proposes a battery, comprising the aforementioned pole piece, thereby obtaining a battery with higher energy density and better cycle performance.
[0113] In the embodiment of the present application, the battery 5 may be a metal battery.
[0114] As an example, the battery 5 may be a sodium metal battery, a lithium metal battery, or the like.
[0115] In some embodiments, reference Figure 2 The electrode assembly 52 may be a winding structure. The positive electrode sheet and the negative electrode sheet are wound to form a winding structure.
[0116] In some embodiments, the electrode assembly 52 is a laminate structure.
[0117] As an example, a plurality of positive electrode sheets and a plurality of negative electrode sheets may be provided respectively, and the plurality of positive electrode sheets and the plurality of negative electrode sheets may be alternately stacked.
[0118] As an example, a plurality of positive electrode sheets may be provided, and the negative electrode sheet is folded to form a plurality of stacked folded segments, with a positive electrode sheet sandwiched between adjacent folded segments.
[0119] As an example, both the positive electrode sheet and the negative electrode sheet are folded to form a plurality of stacked folded sections.
[0120] In some embodiments, the isolation membrane is disposed between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive electrode sheet and the negative electrode sheet from short-circuiting, while allowing ions to pass through.
[0121] As an example, a plurality of separators may be provided, each of which is provided between any adjacent positive electrode sheets or negative electrode sheets.
[0122] As an example, the separator may be disposed continuously, and disposed between any adjacent positive electrode sheets or negative electrode sheets by folding or winding.
[0123] In some embodiments, the shape of the electrode assembly can be cylindrical, flat, or polygonal.
[0124] In some embodiments, the electrode assembly is provided with tabs, which can lead current out of the electrode assembly. The tabs include a positive tab and a negative tab.
[0125] The present application has no particular limitation on the type of isolation membrane, and any porous isolation membrane with good chemical stability and mechanical stability can be selected.
[0126] As an example, the main material of the separator may include at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, ceramic and polyvinylidene fluoride. The number of layers of the separator is not particularly limited, and the separator may be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer are not particularly limited, and the materials of each layer may be the same or different. The separator may be a separate component located between the positive electrode sheet and the negative electrode sheet, or it may be attached to the surface of the positive electrode sheet and / or the negative electrode sheet.
[0127] As an example, the present application has no particular limitation on the shape of the battery, which may be cylindrical, square, or any other shape. Figure 1 The square structure battery 5 is used as an example. Figure 2 The outer package of the battery 5 may include a shell 51 and a top cover assembly 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the top cover assembly 53 can be covered on the opening to close the receiving cavity.
[0128] As an example, the positive electrode sheet, the negative electrode sheet and the separator can be wound or laminated to form an electrode assembly 52. The electrode assembly 52 is encapsulated in the accommodating cavity, and the electrolyte impregnates the electrode assembly 52. The number of electrode assemblies 52 included in the battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0129] As an example, batteries may be assembled into a battery module. The number of batteries contained in the battery module may be one or more. The specific number may be selected by those skilled in the art according to the application and capacity of the battery module. Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the multiple batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. The multiple batteries 5 may further be fixed by fasteners. The battery module 4 may also include a housing having a storage space, and the multiple batteries 5 are stored in the storage space.
[0130] As an example, the above-mentioned battery modules can also be assembled into a battery pack. The number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack. Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0131] In the fifth aspect of the present application, the present application proposes an electrical device, comprising the aforementioned battery. Therefore, the electrical device has all the features and advantages of the aforementioned battery, which will not be described in detail here.
[0132] Batteries, battery modules, or battery packs can be used as power sources for electrical devices, or as energy storage units for electrical devices. Electrical devices may include mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Electrical devices may select batteries, battery modules, or battery packs according to their usage requirements.
[0133] As an example, Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the battery, a battery pack or a battery module can be used.
[0134] As an example, the power-consuming device may also be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and a battery may be used as a power source.
[0135] The scheme of the present application is described below by specific examples. It should be noted that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this area or the product instructions are used. The reagents or instruments used are not specified by the manufacturer, and are all conventional products that can be obtained commercially.
[0136] Example 1
[0137] 1. Synthesis of covalent organic framework materials
[0138] Paraphenylenediamine is selected as the first monomer, 2,4,6-triformylphloroglucinol is selected as the second monomer, and anhydrous ethanol is selected as the solvent. The first monomer and the second monomer are weighed in a molar ratio of 2:3 and then ground and mixed evenly, wherein the ratio of the sum of the molar number of the first monomer and the molar number of the second monomer to the molar number of the solvent is 1:0.03, 1-2 drops of solvent are added during grinding, and grinding is continued to be uniform, the final ground product is centrifuged and washed with dichloromethane as the solvent, the ground product is collected with methanol, and then placed in a drying oven at 60°C to obtain a covalent organic framework material.
[0139] 2. Heat treatment of covalent organic framework materials
[0140] The covalent organic framework material powder in step 1 is transferred to a ceramic ark and placed in a tube furnace, and the temperature is gradually increased to 800°C at a heating rate of 5°C / min. Heat treatment is performed at 800°C for 4 hours under argon atmosphere protection, and then cooled to room temperature to obtain a black powdery conductive carbon material.
[0141] 3. Preparation of batteries
[0142]
Preparation of positive electrode
[0143] The positive electrode active material (lithium manganate), the above-mentioned conductive carbon material, the binder (polyvinylidene fluoride), and the solvent (N-methylpyrrolidone) are stirred and mixed evenly in a weight ratio of 95.81:1.5:1.55:1.14 to obtain a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained after cold pressing.
[0144]
Preparation of negative electrode sheet
[0145] The negative electrode active material (graphite), conductive agent (carbon black), binder (styrene-butadiene rubber), and thickener (sodium hydroxymethyl cellulose) are dissolved in deionized water at a weight ratio of 97.2:0.8:0.8:1.2, and mixed evenly to prepare a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained after cold pressing.
[0146]
Preparation of electrolyte
[0147] In an argon atmosphere glove box, ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / diethyl carbonate (DEC) were mixed evenly in a volume ratio of 36 / 29 / 35, 1M LiPF6 lithium salt was added and dissolved in an organic solvent, and stirred evenly to obtain an electrolyte.
[0148]
Isolation film
[0149] Polypropylene film is used as the isolation film.
[0150]
Battery Assembly
[0151] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then wound to obtain an electrode assembly, the electrode assembly is welded with a pole ear, and the electrode assembly is placed in an aluminum shell and baked at 100°C to remove water, and then the electrolyte is injected and sealed to obtain an uncharged battery. The uncharged battery is then subjected to the processes of static, hot and cold pressing, formation, shaping, and capacity testing in sequence to obtain a battery.
[0152] Example 2 to Example 11 and Comparative Example 1 are consistent with Example 1, except for the molar ratio of the first monomer to the second monomer, the conditions for the heating treatment, etc.;
[0153] Among them, carbon black is also added to the positive electrode slurry of Example 10, and the mass fraction of carbon black in the positive electrode slurry is 1%, and the mass fraction of the conductive carbon material is 0.5%; carbon black is also added to the positive electrode slurry of Example 11, and the mass fraction of carbon black in the positive electrode slurry is 0.5%, and the mass fraction of the conductive carbon material is 1%; no conductive carbon material is added to the positive electrode slurry of Comparative Example 1, and only carbon black is used as a conductive agent, see Table 1 for details.
[0154] Table 1
[0155]
[0156] The following tests were performed on the conductive carbon materials in Examples 1-11 and Comparative Example 1. The test results are shown in Table 2.
[0157] Porosity of conductive carbon materials: record the dry weight M0 of the sample to be tested, heat the sample to be tested in deionized water and boil it for at least 2 hours, then record the mass M1, wipe off the moisture of the sample to be tested and record the mass M2, and divide the difference between M2-M0 by the difference between M2-M1 to get the porosity.
[0158] Mass fraction of nitrogen in the conductive carbon material: The weight percentage of nitrogen in the conductive carbon material can be measured by performing elemental analysis on the conductive carbon material using a scanning electron microscope.
[0159] Pore size of conductive carbon material: The pore size of the conductive carbon material is obtained by nitrogen adsorption and desorption test, wherein at least 50 mg of the sample to be tested should be taken during the test, and the sample to be tested should be vacuum dried at 150°C for 3 hours before the test.
[0160] Particle size of conductive carbon material: Take 10 mg of the conductive carbon material to be tested and evenly disperse it in anhydrous ethanol, then take the suspension and add it to the surface of the microgrid copper mesh. After drying, perform transmission electron microscopy test and observe the copper mesh under the transmission electron microscope to obtain the particle size of the conductive carbon material.
[0161] Specific surface area of conductive carbon material: The specific surface area of conductive carbon material is obtained by nitrogen adsorption and desorption test, wherein at least 50 mg of the sample to be tested should be taken during the test, and the sample to be tested should be vacuum dried at 150°C for 3 hours before the test.
[0162] Electronic conductivity of conductive carbon materials:
[0163] The conductive carbon material powder is placed in the test mold, stainless steel gaskets are used as blocking electrodes on both sides, and pressed at a pressure of 350MPa for 3min to make a conductivity mold battery. The electronic conductivity is obtained by constant voltage DC test of the mold battery using an electrochemical workstation;
[0164] The calculation formula is shown below:
[0165]
[0166] Among them, σ represents conductivity, d represents the thickness of the electrode to be tested, R represents electrochemical impedance (the electronic impedance value is measured by the electrochemical workstation), and S represents the effective area of the electrode to be tested.
[0167] Table 2
[0168]
[0169]
[0170] The following tests were performed on the batteries in Examples 1-11 and Comparative Example 1. The test results are shown in Table 3.
[0171] Cyclic capacity retention rate test: At 45°C, charge the battery to 4.4V at a constant current of 1 / 3C, then charge at a constant voltage of 4.4V to a current of 0.05C, leave for 5 minutes, and then discharge to 2.5V at 1 / 3C. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery, and record the discharge capacity Cn of the battery after the nth cycle at the same time. The battery capacity retention rate after each cycle is Pn = Cn / C0×100%. When n is 500, record P500 as the battery's cyclic capacity retention rate.
[0172] Mn dissolution ICP test: The fully charged negative electrode plates after 500 cycles were disassembled, and the Mn content in the negative electrode plates was tested using inductively coupled plasma (ICP) to confirm the manganese dissolution.
[0173] Table 3
[0174]
[0175] In the description of this specification, the description of reference terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.
[0176] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A conductive carbon material, characterized in that: The porosity of the conductive carbon material is greater than or equal to 90%, and the mass fraction of nitrogen in the conductive carbon material is 0.5%-5%. Optionally, the mass fraction of nitrogen in the conductive carbon material is 0.5%-1%.
2. The conductive carbon material according to claim 1, characterized in that: The pore size of the conductive carbon material is 0.1 nm-1 nm.
3. The conductive carbon material according to claim 1 or 2, characterized in that: The particle size of the conductive carbon material is 4 μm-10 μm, preferably, the particle size of the conductive carbon material is 5 μm-8 μm.
4. The conductive carbon material according to any one of claims 1 to 3, characterized in that: The specific surface area of the conductive carbon material is 1200 m 2 / g-1800m 2 / g.
5. The conductive carbon material according to any one of claims 1 to 4, characterized in that: The electronic conductivity of the conductive carbon material is greater than or equal to 550 S / m.
6. A method for preparing the conductive carbon material according to any one of claims 1 to 5, characterized in that: include: Provide covalent organic framework materials, The covalent organic framework material is subjected to a heating treatment.
7. The method according to claim 6, characterized in that The provision of a covalent organic framework material comprises: Mixing the first monomer and the second monomer; Among them, at least one of the following conditions is met: The first monomer includes at least one of p-phenylenediamine, 4,4'-diaminobiphenyl, 1,3,5-triaminobenzene, 1,3,5-tris(4-aminophenyl)benzene, 1,3,5,7-tetrakis(4-aminophenyl)methane, 1,3,5,7-tetrakis(4-aminophenyl)adamantane, 1,3,6,8-tetraaminopyrene, and 5,10,15,20-tetrakis(4-aminophenyl)porphyrin; The second monomer includes at least one of terephthalaldehyde, 4,4'-biphenyldicarboxaldehyde, 1,3,5-trialdehyde benzene, 1,3,5-tri(4-formylphenyl)benzene, tetra(4-formylphenyl)methane, tetra(4-formylphenyl)adamantane, trialdehyde phloroglucinol, 2,4,6-triformyl phloroglucinol, 1,3,6,8-tetra(4-formaldehydephenyl)pyrene, and 5,10,15,20-tetra(4-formylphenyl)porphyrin.
8. The method according to claim 7, characterized in that When the first monomer and the second monomer are mixed, the mole number of the first monomer is n1, the mole number of the second monomer is n2, and n1:n2=(1-5):
3.
9. The method according to any one of claims 6 to 8, characterized in that: The heating treatment satisfies at least one of the following conditions: The temperature of the heating treatment is 500°C-1000°C; The heating time is 3h-8h; The heating rate of the heating treatment is 1°C / min-5°C / min.
10. A pole piece, characterized in that: The pole piece comprises the conductive carbon material according to any one of claims 1 to 5, and / or the conductive carbon material prepared by the method according to any one of claims 6 to 9.
11. The pole piece according to claim 10, characterized in that: The electrode sheet is a positive electrode sheet, and the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer at least located on one side of the positive electrode current collector, and the positive electrode active material layer comprises the conductive carbon material.
12. The pole piece according to claim 11, characterized in that: The mass fraction of the conductive carbon material in the positive electrode active material layer is 0.2%-3.5%.
13. The pole piece according to claim 11 or 12, characterized in that: The positive electrode active material layer includes a positive electrode active material including at least one of lithium manganese oxide and lithium manganese phosphate.
14. The pole piece according to claim 13, characterized in that: The mass fraction of the positive electrode active material in the positive electrode active material layer is 96.5%-98.5%.
15. The pole piece according to claim 10, characterized in that: The electrode sheet is a negative electrode sheet, and the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer at least located on one side of the negative electrode current collector, and the negative electrode active material layer comprises the conductive carbon material.
16. The pole piece according to claim 10, characterized in that: The electrode sheet is a negative electrode sheet, and the negative electrode sheet includes a negative electrode current collector and a functional coating located at least on one side of the negative electrode current collector, and the functional coating includes the conductive carbon material.
17. The pole piece according to any one of claims 10 to 16, characterized in that: The pole piece further includes a conductive agent, the mass of the conductive carbon material in the pole piece is m1, the mass of the conductive agent in the pole piece is m2, and m1:m2=(0.5-2.5):
1.
18. A battery, characterized in that: A pole piece comprising any one of claims 10-17.
19. An electrical device, characterized in that: Comprising the battery of claim 18.