G-C3N4 coupled Fe-N / MPC dual-carbon photoelectric synergistic oxygen catalytic material as well as preparation method and application thereof

The active position of the catalyst was solved by mixing the g-C3N4-coupled Fe-N/MPC catalyst with mixed ball mill of iron-nitrogen co-doped porous carbon Fe-N/MPC with graphitized carbon nitride in zinc air batteries. The insufficient point exposure and stability problems have achieved efficient photoelectric synergistic catalysis, significantly improving the performance and stability of zinc air batteries.

CN119069726APending Publication Date: 2024-12-03DONGHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411052770.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing Fe-N-C materials are used as catalysts as catalysts in zinc-air batteries, including insufficient exposure of active sites, corrosion of carbon support and falling off of metal centers, resulting in insufficient catalytic performance and stability, and the need for a higher load, resulting in excessive thickness of the catalytic layer. The mass transfer of the reaction gas is limited.

Method used

Iron-nitrogen co-doped porous carbon Fe-N/MPC was prepared by template method, and bicarbonate photoelectric synergistic oxygen with g-C3N4 coupled Fe-N/MPC was formed by mixing ball mill with graphitized carbon nitride (g-C3N4) Catalytic materials are prepared by calcining method, and the N-C active site exposure and energy level structure are optimized to form an efficient photoelectric synergistic catalyst.

Benefits of technology

The activity and stability of the catalyst are improved, the aggregation and detachment of active sites are reduced, the light absorption range is expanded, the transfer of photogenerated charge carriers is promoted, and the specific capacity and cyclic stability of zinc air batteries are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069726A_ABST
    Figure CN119069726A_ABST
Patent Text Reader

Abstract

The invention relates to a g-C3N4 coupled Fe-N / MPC dual-carbon photoelectric synergistic oxygen catalytic material and a preparation method and application thereof, iron-nitrogen co-doped porous carbon Fe-N / MPC is prepared by a template method, g-C3N4 is prepared by a calcination method, and finally, Fe-N / MPC and g-C3N4 are mixed and ball-milled to obtain the g-C3N4 coupled Fe-N / MPC dual-carbon photoelectric synergistic oxygen catalytic material. The material disclosed by the invention has a staggered p-n heterostructure, a proper band gap width and a relatively large specific surface area, so that light energy can be effectively captured, and oxygen reduction and oxygen evolution reaction kinetics are remarkably improved; meanwhile, the visual zinc-air battery assembled by the material can realize high specific capacity and high charge-discharge cycle stability under auxiliary light driving, and has a good market application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photocatalysis, and particularly relates to a g-C3N4 coupled Fe-N / MPC dual-carbon photoelectric synergistic oxygen catalytic material and a preparation method and application thereof. Background Art

[0002] With the increasing demand for energy and environmental pollution, the development of clean alternative energy has become the top priority. Among them, zinc-air batteries (ZABs) are considered to be one of the new energy representatives with great application prospects in the future due to their high energy density, low cost and environmental friendliness. It mainly generates and stores energy through oxygen reduction reaction (ORR) and oxygen evolution reaction (OER). However, the slow kinetics of ORR and OER prevent zinc-air batteries from achieving maximum efficiency and often produce high overpotentials, limiting their actual performance. Therefore, how to construct efficient bifunctional catalysts to reduce the reaction activation energy of ORR / OER is the key to solving this problem.

[0003] Transition metal iron-nitrogen-carbon materials (Fe-NC) have attracted great attention from researchers due to their high conductivity and excellent catalytic performance. However, the practical application of this material still faces the following challenges: (1) Fe-NC is a good ORR catalyst, but its electrocatalytic performance for OER is poor. Its complex synthesis process will seriously hinder the precise regulation and exposure of active sites; (2) The electrocatalytic process will lead to corrosion of the carbon support and shedding of the metal center, resulting in insufficient catalytic performance and stability; (3) Due to the non-precious metal catalyst characteristics of Fe-NC, it is often necessary to work at a higher loading, resulting in an overly thick catalytic layer, which limits the mass transfer of the reaction gas. Therefore, it is crucial to achieve high catalytic activity and stability of the air electrode in ZABs and to open up effective mass transfer of thick-layer electrodes.

[0004] With the development of photocatalytic technology, researchers have proposed strategies for light-assisted zinc-air batteries in recent years, and found that the combination of photochemistry and electrochemistry is an effective way to improve the intrinsic catalytic activity of catalysts and realize high-performance zinc-air batteries, which mainly involves the construction and application of photocatalytic materials, and the collection and utilization of light energy to improve the performance of zinc-air batteries. Graphitized carbon nitride (g-C3N4) is a common photocatalyst, but its photoelectric conversion efficiency is low. It is usually combined with other semiconductor materials to form a heterojunction to improve its photocatalytic activity and stability. Therefore, it is of great significance to couple the two materials to design and develop a bifunctional catalyst with high catalytic activity and stable photoelectric synergy to realize high-performance light-assisted zinc-air batteries. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC and its preparation method and application, so as to solve the problems in the prior art of insufficient exposure of catalyst active sites, corrosion of carbon carriers and shedding of metal centers, resulting in insufficient catalytic performance and stability.

[0006] The present invention provides a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC. The iron-nitrogen co-doped porous carbon Fe-N / MPC is prepared by a template method, the g-C3N4 is prepared by a calcination method, and finally the Fe-N / MPC and g-C3N4 are mixed and ball-milled to obtain the material.

[0007] The present invention also provides a method for preparing a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC, comprising the following steps:

[0008] (1) adding nitrogen-containing polymer polyquaternary ammonium salt, nano-SiO2 and FeSO4 into HCl solution and stirring to react to obtain a precursor;

[0009] (2) carbonizing the precursor once, then alkali washing and acid washing, and then carbonizing it again to obtain Fe-N / MPC;

[0010] (3) Fe-N / MPC and g-C3N4 were mixed and ball-milled to obtain the dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC.

[0011] Preferably, the mass ratio of the nitrogen-containing polymer polyquaternary ammonium salt, nano-SiO2 and FeSO4 in step (1) is 4.5:1:0.3-0.9.

[0012] Preferably, the stirring reaction time in step (1) is 1-10 h.

[0013] Preferably, the primary carbonization and secondary carbonization in step (2) are carried out under N2 conditions, with a heating rate of 20-50°C / min, a temperature of 700-900°C, and a time of 1-2h.

[0014] Preferably, the alkaline washing in step (2) is to place the product in a NaOH solution for alkaline washing and stirring, then filter the solution with deionized water until it is neutral, and dry it in an oven.

[0015] Preferably, the acid washing in step (2) is to place the product in a H2SO4 solution for acid washing and stirring, then filter the solution with deionized water until it is neutral, and dry it in an oven.

[0016] Preferably, the g-C3N4 in step (3) accounts for 5-15% of the mass of Fe-N / MPC.

[0017] Preferably, the ball milling speed in step (3) is 300-500 rpm and the time is 1-5 h.

[0018] The present invention also provides an application of a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC in a visualized light-enhanced zinc-air battery.

[0019] Beneficial Effects

[0020] (1) The present invention forms new NC active sites through g-C3N4 in coordination with Fe-N / MPC, promotes good exposure of active sites in the electrode, and reduces the degree of agglomeration, migration and detachment of the catalyst active sites, which is beneficial to improving the catalytic activity and stability of the catalyst.

[0021] (2) Based on the doping effect of iron and nitrogen atoms on porous carbon and their energy level structure matching regulation with g-C3N4, the present invention can form an efficient light-assisted porous carbon-based ORR / OER dual-effect catalyst with a suitable band gap width and staggered pn heterostructure. The π-π reconstruction between g-C3N4 and doped porous carbon is beneficial to expand the light absorption range, while promoting the transfer of photogenerated charge carriers, stimulating more electrons to participate in ORR / OER, and improving catalytic activity and battery performance.

[0022] (3) The present invention combines the advantages of solar cell light energy conversion and rechargeable metal battery high energy storage, and actually applies the catalyst to light-assisted liquid flow zinc-air batteries to achieve high specific capacity and high charge and discharge cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 a, b are SEM images of g-C3N4@Fe-N / MPC-10 prepared in Example 2; c, d are TEM images of g-C3N4@Fe-N / MPC-10 prepared in Example 2;

[0024] Figure 2 a is a comparison chart of the ORR performance of the catalysts prepared in Examples 1-3 in 0.1 M KOH under light and darkness, respectively;

[0025] Figure 2 b is a comparison of the OER performance of the catalysts prepared in Examples 1-3 in 1 M KOH under light and darkness;

[0026] Figure 3a The discharge specific capacity diagram of the zinc-air battery assembled with g-C3N4@Fe-N / MPC-10 prepared in Example 2 as a photocatalyst;

[0027] Figure 3bThis is the charge and discharge cycle performance diagram of the rechargeable zinc-air battery assembled using g-C3N4@Fe-N / MPC-10 prepared in Example 2 as a photocatalyst. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0029] Performance measurement: The microstructure of the product of the present invention was tested by TEM (JEOL JEM-2100F system) and SEM (Hitachi S-4800). The electrochemical performance test was carried out on a Chenhua CHI760D electrochemical workstation using a three-electrode system. The cycling performance of the light-assisted zinc-air battery was tested by a blue electric test system.

[0030] Example 1

[0031] Step 1): Take a nitrogen-containing polymer polyquaternary ammonium salt (PQ-7), nano-SiO2 powder and transition metal salt FeSO4 in a mass ratio of 4.5:1:0.6 and add them to a 1M HCl solution and stir for 2 hours to obtain a uniform solution, with a mass fraction of 34.9% PQ-7 solution, 16.7% SiO2 solution and 23.1% FeSO4 solution. After magnetic stirring for 5 hours, put it in an oven at 85°C and dry it for 48 hours, take it out and grind it into a yellow powder precursor.

[0032] Step 2): The precursor obtained in step 1) is placed in a tube furnace for primary carbonization, and the temperature is raised to 800°C at a rate of 20°C / min under N2 conditions and maintained for 1 hour, and then cooled to room temperature to obtain a black powder.

[0033] Step 3): The primary carbonization product obtained in step 2) was placed in 100 mL of 4M NaOH solution for alkaline washing and stirring for 48 h, and then the solution was filtered with deionized water until it was neutral, and dried in an oven at 85° C. for 24 h.

[0034] Step 4): The dried product obtained in step 3) was placed in 100 mL of 0.5 M H2SO4 solution and acid-washed at 85°C with stirring for 8 h, then the solution was filtered with deionized water until it was neutral, and dried in an oven at 85°C for 24 h.

[0035] Step 5): The dried product obtained in step 4) is placed in a tubular furnace for secondary carbonization, and the temperature is raised to 800°C at a rate of 20°C / min under N2 conditions and maintained for 1 hour. After cooling to room temperature, a black powder is obtained, namely Fe-N / MPC.

[0036] Step 6): Take urea and place it in a muffle furnace, heat it to 550°C at a rate of 3°C / min and keep it warm for 3 hours. After cooling to room temperature, grind it to obtain light yellow powder g-C3N4.

[0037] Step 7): Take the g-C3N4 in step 5) and step 6) and Fe-N / MPC (g-C3N4 accounts for 5% of the mass of Fe-N / MPC) and ball mill them at 400 rpm for 3 hours to obtain a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC, recorded as g-C3N4@Fe-N / MPC-5.

[0038] Example 2

[0039] Step 1): Take nitrogen-containing polymer polyquaternary ammonium salt (PQ-7), nano-SiO2 powder and transition metal salt FeSO4 in a mass ratio of 4.5:1:0.6, add 1M HCl and stir for 2 hours to obtain a uniform solution, with mass fractions of 34.9% PQ-7 solution, 16.7% SiO2 solution and 23.1% FeSO4 solution. After magnetic stirring for 5 hours, put it in an oven at 85°C and dry it for 48 hours, take it out and grind it into a yellow powder precursor.

[0040] Step 2): The precursor obtained in step 1) is placed in a tube furnace for primary carbonization, and the temperature is raised to 800°C at a rate of 20°C / min under N2 conditions and maintained for 1 hour, and then cooled to room temperature to obtain a black powder.

[0041] Step 3): The primary carbonization product obtained in step 2) was placed in 100 mL of 4M NaOH solution for alkaline washing and stirring for 48 h, and then the solution was filtered with deionized water until it was neutral, and dried in an oven at 85° C. for 24 h.

[0042] Step 4): The dried product obtained in step 3) was placed in 100 mL of 0.5 M H2SO4 solution and acid-washed at 85°C with stirring for 8 h, then the solution was filtered with deionized water until it was neutral, and dried in an oven at 85°C for 24 h.

[0043] Step 5): The dried product obtained in step 4) is placed in a tubular furnace for secondary carbonization, and the temperature is raised to 800°C at a rate of 20°C / min under N2 conditions and maintained for 1 hour. After cooling to room temperature, a black powder is obtained, namely Fe-N / MPC.

[0044] Step 6): Take urea and place it in a muffle furnace, heat it to 550°C at a rate of 3°C / min and keep it warm for 3 hours. After cooling to room temperature, grind it to obtain light yellow powder g-C3N4.

[0045] Step 7): Take the g-C3N4 in step 5) and step 6) and Fe-N / MPC (g-C3N4 accounts for 10% of the mass of Fe-N / MPC) and ball mill them at 400 rpm for 3 hours to obtain a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC, recorded as g-C3N4@Fe-N / MPC-10.

[0046] Example 3

[0047] Step 1): Take nitrogen-containing polymer polyquaternary ammonium salt (PQ-7), nano-SiO2 powder and transition metal salt FeSO4 in a mass ratio of 4.5:1:0.6, add appropriate amount of 1M HCl and stir for 2 hours to obtain a uniform solution, with mass fractions of 34.9% PQ-7 solution, 16.7% SiO2 solution and 23.1% FeSO4 solution. After magnetic stirring for 5 hours, put it in an oven at 85°C and dry it for 48 hours, take it out and grind it into a yellow powder precursor.

[0048] Step 2): The precursor obtained in step 1) is placed in a tube furnace for primary carbonization, and the temperature is raised to 800°C at a rate of 20°C / min under N2 conditions and maintained for 1 hour, and then cooled to room temperature to obtain a black powder.

[0049] Step 3): The primary carbonization product obtained in step 2) was placed in 100 mL of 4M NaOH solution for alkaline washing and stirring for 48 h, and then the solution was filtered with deionized water until it was neutral, and dried in an oven at 85° C. for 24 h.

[0050] Step 4): The dried product obtained in step 3) was placed in 100 mL of 0.5 M H2SO4 solution and acid-washed at 85°C with stirring for 8 h, then the solution was filtered with deionized water until it was neutral, and dried in an oven at 85°C for 24 h.

[0051] Step 5): The dried product obtained in step 4) is placed in a tubular furnace for secondary carbonization, and the temperature is raised to 800°C at a rate of 20°C / min under N2 conditions and maintained for 1 hour. After cooling to room temperature, a black powder is obtained, namely Fe-N / MPC.

[0052] Step 6): Take urea and place it in a muffle furnace, heat it to 550°C at a rate of 3°C / min and keep it warm for 3 hours. After cooling to room temperature, grind it to obtain light yellow powder g-C3N4.

[0053] Step 7): Take the g-C3N4 in step 5) and step 6) and Fe-N / MPC (g-C3N4 accounts for 15% of the mass of Fe-N / MPC) and ball mill them at 400 rpm for 3 hours to obtain a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC, recorded as g-C3N4@Fe-N / MPC-15.

[0054] Example 4

[0055] 30 mg of the catalyst of Example 2 was mixed with 10 mL of ethanol and 80 μL of 5 wt% Nafion solution and ultrasonicated for 30 min to obtain a uniform catalyst slurry. 2 mg of the slurry was evenly sprayed onto a 1 cm 2 The photoactive cathode was obtained by drying on carbon paper. The above air electrode, anode (polished Zn plate) and electrolyte (6M KOH) were assembled into a visual light-enhanced zinc-air battery using a homemade acrylic plate model. The battery performance was tested using a blue electric system.

[0056] Figure 1 a, b are SEM images of g-C3N4@Fe-N / MPC-10 prepared in Example 2; it can be seen that g-C3N4@Fe-N / MPC-10 shows the coexistence of pore structure and nanosheets. Figure 1 The TEM images of c and d correspond to each other. g-C3N4@Fe-N / MPC-10 has a two-dimensional nanosheet structure with wrinkled edges and a three-dimensional network structure with significantly different pore sizes, indicating that the two monomer photoactive materials are successfully coupled.

[0057] Figure 2 a is a comparison chart of the oxygen reduction performance of the catalyst materials prepared in Examples 1-3. It can be seen that the starting potential, half-wave potential and limiting current density of g-C3N4@Fe-N / MPC-10 under light are significantly improved, significantly higher than those under dark conditions and other materials. This shows that the light-driven synergistically doped carbon hierarchical porous structure is not only conducive to accelerating the electron transfer process, but also can more effectively open up the mass transfer channel and improve the ORR kinetic performance. Figure 2 b is a comparison chart of oxygen evolution performance of catalyst materials prepared in Examples 1-3. It can be seen from the figure that g-C3N4@Fe-N / MPC-10 has a high oxygen evolution performance when the current density is 10 mA cm -2 When , it has the smallest overpotential. This shows that g-C3N4@Fe-N / MPC-10 not only has excellent OER electrochemical catalytic activity, but also has excellent OER photocatalytic activity.

[0058] Figure 3a is 10mA cm -2Comparison of discharge capacity under dark and light conditions. The specific capacity of the light-assisted zinc-air battery based on g-C3N4@Fe-N / MPC-10 driven by visible light reaches 896 mAh g -1 zn , which is 43.8% higher than the specific capacity under dark conditions. This indicates that the photogenerated holes of g-C3N4@Fe-N / MPC-10 can drive Zn / ZnO oxidation through an external circuit, thereby increasing the Zn 2+ utilization rate. Figure 3b The zinc-air battery assembled by g-C3N4@Fe-N / MPC-10 was placed under light and dark conditions at 5 mA cm -2 Comparison of long-term constant current charge and discharge measurement curves. It can be seen that the zinc-air battery under light has a long cycle life of more than 800h, which shows a higher cycle life than 670h under dark conditions. In addition, compared with dark conditions, g-C3N4@Fe-N / MPC-10-based ZABs under light have a smaller charge voltage and a larger discharge voltage. This shows that g-C3N4@Fe-N / MPC-10 not only has excellent photocatalytic activity among photoactive ZABs, but also has excellent stability and has good market application prospects.

Claims

1. A dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC, characterized in that: Iron-nitrogen co-doped porous carbon Fe-N / MPC was prepared by template method, g-C3N4 was prepared by calcination method, and finally Fe-N / MPC and g-C3N4 were obtained by mixed ball milling.

2. A method for preparing a dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC, comprising the following steps: (1) adding nitrogen-containing polymer polyquaternary ammonium salt, nano-SiO2 and FeSO4 into HCl solution and stirring to react to obtain a precursor; (2) carbonizing the precursor once, then alkali washing and acid washing, and then carbonizing it again to obtain iron-nitrogen co-doped porous carbon Fe-N / MPC; (3) Fe-N / MPC and g-C3N4 were mixed and ball-milled to obtain the dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC.

3. The preparation method according to claim 2, characterized in that: The mass ratio of nitrogen-containing polymer polyquaternary ammonium salt, nano-SiO2 and FeSO4 in step (1) is 4.5:1:0.3-0.

9.

4. The preparation method according to claim 2, characterized in that: The stirring reaction time in step (1) is 1-10h.

5. The preparation method according to claim 2, characterized in that: The primary carbonization and secondary carbonization in step (2) are carried out under N2 conditions, with a heating rate of 20-50°C / min, a temperature of 700-900°C, and a time of 1-2h.

6. The preparation method according to claim 2, characterized in that: The alkaline washing in step (2) is to place the product in a NaOH solution for alkaline washing and stirring, then filter the solution with deionized water until it is neutral, and dry it in an oven.

7. The preparation method according to claim 2, characterized in that: The acid washing in step (2) is to place the product in a H2SO4 solution for acid washing and stirring, then filter the solution with deionized water until it is neutral, and dry it in an oven.

8. The preparation method according to claim 2, characterized in that: The g-C3N4 in step (3) accounts for 5-15% of the mass of Fe-N / MPC.

9. The preparation method according to claim 2, characterized in that: The ball milling speed in step (3) is 300-500 rpm and the time is 1-5 h.

10. An application of the dual-carbon photoelectric synergistic oxygen catalytic material of g-C3N4 coupled with Fe-N / MPC as claimed in claim 1 in a visualized light-enhanced zinc-air battery.