Fast-burning high-calorific-value heating powder and preparation method thereof

By using a specific proportion combination of metal alloy powder, iron powder and potassium perchlorate in the heating powder of the thermal battery, the combustion speed and heat generation of the heating powder are improved, and the problems of rapid activation of thermal batteries and high heat generation in the prior art are solved. Ensures efficient activation and long battery life of the thermal battery.

CN119069732APending Publication Date: 2024-12-03GUIZHOU MEILING POWER SUPPLY CO LTD

Patent Information

Application Number
CN202411145341.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing thermal battery heating powder has shortcomings in terms of rapid activation and high heat generation, which cannot meet the requirements of modern equipment for rapid activation of thermal batteries. At the same time, the introduced materials may reduce the conductivity of the heating plate after combustion and affect the performance of the thermal battery.

Method used

The fast-burning and high-heat heating powder consisting of metal alloy powder, metal iron powder and potassium perchlorate in a specific proportion is used to ensure that the alloy powder is completely consumed in the combustion reaction and avoid affecting the conductivity of the heating sheet.

Benefits of technology

It achieves the dual improvement of heating powder combustion speed and heat generation, shortens the activation time of the thermal battery, meets the requirements of fast activation and long battery life, and does not affect the discharge performance of the thermal battery, and broadens the application field of thermal battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069732A_ABST
    Figure CN119069732A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermal battery materials, and particularly relates to high-burning-rate and high-calorific-value heating powder and a preparation method thereof.The method of adding alloy powder is adopted, and the burning rate and the calorific value of the heating powder can be increased; the heating powder is obtained by weighing magnesium / aluminum-containing binary or ternary metal alloy powder, metal iron powder and potassium perchlorate according to a certain proportion and mechanically and uniformly mixing. Due to the strong chemical reaction between the metal alloy powder and the potassium perchlorate, the heating powder containing the metal alloy has high burning speed and heat productivity. Meanwhile, the introduction amount is small and can be completely consumed by the reaction, the battery performance is not influenced, and the method has an obvious guiding effect on development of thermal batteries with special requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal battery materials, and particularly relates to a fast-burning-rate and high-calorific-value heating powder and a preparation method thereof. Background Art

[0002] Thermal batteries are a type of molten salt battery, where the electrolyte is a non-conductive solid at room temperature. When in use, an electric current is used to ignite the ignition head or a physical component hits the primer, igniting the heating powder inside the battery, causing the temperature inside the battery to rise rapidly. The electrolyte melts at high temperatures to form an ion conductor with high conductivity, forming a discharge path. Therefore, thermal batteries are non-conductive under natural conditions, and have the advantages of long storage time, short activation time, high specific energy, high specific power, and maintenance-free.

[0003] With the continuous development of science and technology, higher requirements are put forward for the discharge performance of thermal batteries, one of which is the ability to activate the battery and discharge in a short time. From the characteristics of the battery structure, it can be seen that in the "activation-discharge" process of the thermal battery, the heat is mainly provided by the internal heating plate. In order to achieve the purpose of rapid activation of the thermal battery, the development of heating powder with fast burning speed and high calorific value, so that the electrolyte melts and conducts the circuit in a very short time is one of the most effective ways. At present, the raw materials of the heating powder that has been realized in engineering applications only contain two substances, iron and potassium perchlorate. Its burning speed and calorific value are gradually unable to meet the requirements of some equipment at this stage for rapid activation of thermal batteries.

[0004] In order to improve the burning rate and calorific value of heating powder, domestic and foreign researchers have conducted a series of studies on this. On the one hand, the performance of heating powder is improved by introducing a single metal powder (including molybdenum powder, titanium powder, etc.). The results show that the introduction of metal powder has a certain improvement effect and does not affect the conductivity of the heating plate; on the other hand, catalysts (metal oxides, etc.) can be added to reduce the reaction barrier of iron and potassium perchlorate, thereby increasing the reaction rate and calorific value of the mixture; or carbon materials can be added as heat-conducting agents to improve the thermal conductivity of the heating powder and increase the burning rate. The patent document with publication number CN102244206A discloses a formula for heating powder for thermal batteries, which is to add a eutectic salt with a weight percentage of 7 to 12% to the heating powder for thermal batteries composed of a mixture of iron powder and potassium perchlorate. The weight ratio of iron powder to potassium perchlorate is 84:16, or 83:17, or 82:18. The eutectic salt is a mixture of NaCl and Li2SO4, with the weight percentage of NaCl in the eutectic salt being 38% to 45% and the weight percentage of Li2SO4 being 55% to 62%. This formula can extend the thermal life of the thermal battery, thereby extending the working life of the thermal battery. Although the above strategies can all increase the burning rate and calorific value of the heating powder, they still cannot meet the current requirements for rapid activation of thermal batteries; at the same time, the introduction of materials with poor electron transmission capacity will reduce the conductivity of the heating sheet after combustion, affecting the performance of the thermal battery.

[0005] Based on this, in order to achieve the current requirement for rapid activation of thermal batteries, it is urgent to develop a heating powder that has both fast burning speed and high heat generation. In order not to affect the conductivity of the heating sheet after the reaction, the best solution is to introduce a material that can react with potassium perchlorate so that the additive is completely consumed after the combustion reaction. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention provides a heating powder with fast burning speed and high calorific value and a preparation method thereof.

[0007] This is achieved specifically through the following technical solutions:

[0008] A fast burning and high calorific value heating powder, characterized in that the raw materials of the heating powder are composed of 0.5-3.0% of metal alloy powder, 80-88% of metal iron powder and 12-19% of potassium perchlorate by weight percentage.

[0009] Furthermore, the metal alloy powder is a binary / ternary metal alloy powder containing aluminum or magnesium, including but not limited to magnesium-zinc alloy, aluminum-manganese alloy, magnesium-aluminum alloy, aluminum-copper alloy, and magnesium-aluminum-zinc alloy.

[0010] Furthermore, the particle size of the metal alloy powder is 50 to 200 nm.

[0011] Furthermore, the particle size of the metal iron powder is less than 250 meshes, and the purity is greater than 98%. Before use, the metal iron powder is dried in a vacuum drying oven at 90 to 110° C. for 10 to 12 hours to remove residual moisture in the iron powder.

[0012] Furthermore, the potassium perchlorate is placed in a tube furnace and dried at 100-120° C. for 4-6 hours in an inert gas atmosphere.

[0013] The preparation method of the above-mentioned fast burning high calorific value heating powder:

[0014] Put the metal alloy powder, pretreated metal iron powder and potassium perchlorate into a glove box (water and oxygen content are both less than 0.01ppm), weigh them according to a certain mass ratio, put them in a sealed can and mix them mechanically for 4 to 8 hours to obtain a fast burning rate and high calorific value heating powder. The evenly mixed powder is placed in the glove box to avoid long-term exposure to the air.

[0015] The molding and performance testing of fast burning and high calorific value heating powder, the specific operation steps are as follows:

[0016] Weigh the uniformly mixed heating powder according to the required mass and put it into the mold. Apply a molding pressure of 20-30MPa to the heating powder. After standing for a period of time, demould it to prepare the heating sheet for burning rate test. Weigh an appropriate amount of uniformly mixed heating powder and put it into the crucible for calorific value test. The burning rate and calorific value of the powder can be tested by conventional tests. The burning rate and calorific value of the traditional heating powder are compared with the alloy heating powder of the present application. The results are as follows: Figure 1 shown.

[0017] Beneficial effects:

[0018] The present invention discloses a method for preparing a heating powder with a fast burning rate and a high calorific value. The method of adding alloy powder can achieve a dual increase in the burning rate and the heat output of the heating powder. At the same time, due to the small amount introduced, the discharge performance of the thermal battery will not be affected, and the requirements of some devices for the thermal battery to have fast activation and long endurance are met.

[0019] (1) The preparation process of the heating powder is simple, the additives are cheap, easy to obtain and cause little pollution. The prepared heating powder has the advantages of fast burning speed and high calorific value, and therefore has a good profit effect.

[0020] (2) The introduced alloy powder can be completely consumed during the combustion reaction of the heating plate and will not affect the conductivity of the material after the heating plate is burned.

[0021] (3) The heating powder can shorten the activation time of the thermal battery and is less affected by the environment inside the battery. It can meet the requirements of rapid activation and long-term storage of the thermal battery, greatly broadening the application field of the thermal battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The burning rate and calorific value of the heating powder of Example 1 and Example 2 are compared;

[0023] Figure 2 The burning rate test results of the heating plate of Example 1 are shown;

[0024] Figure 3 The calorific value test result of the heating powder in Example 1;

[0025] Figure 4 The burning rate test results of the heating plate prepared in Example 2;

[0026] Figure 5 The calorific value test result of the heating powder prepared in Example 2. DETAILED DESCRIPTION

[0027] The specific embodiments of the present invention are further described in detail below, but the present invention is not limited to these embodiments, and any improvement or substitution based on the basic spirit of the present embodiment still falls within the scope of protection required by the claims of the present invention.

[0028] Example 1

[0029] Step 1: Preparation of conventional heating powder

[0030] Put the metal iron powder and potassium perchlorate into a glove box (water and oxygen content are both less than 0.01ppm), weigh them according to the mass ratio of 84%:16%, and evenly disperse the mixed powder. Place the evenly mixed powder in the glove box to avoid long-term exposure to air.

[0031] Step 2: Forming and performance testing of conventional heating powder:

[0032] Weigh 6g of evenly mixed heating powder and put it into the mold. Apply a molding pressure of 40MPa to the heating powder. After standing for a period of time, demold the heating sheet for burning rate test. Weigh 2g of evenly mixed heating powder and put it into a crucible to test the calorific value of the heating powder. The burning rate and calorific value of the powder can be tested by conventional tests.

[0033] The burning rate test of the heating powder prepared in Example 1 is as follows Figure 2 As shown in FIG. 1 , the burning speeds of the three samples are 11.8 cm / s, 12.9 cm / s and 11.2 cm / s respectively, and the average burning speed is 12.0 cm / s. The calorific value test results of the heating powder prepared in Example 1 are shown in FIG. Figure 3 As shown, the calorific values ​​of the three samples are 1290.8 J / g, 1282.9 J / g and 1288.3 J / g respectively, and the average calorific value is 1287.3 J / g.

[0034] Example 2

[0035] Step 1: Pretreatment of heating powder raw materials

[0036] Aluminum-manganese alloy powder with an average particle size of 150 nm was used as an additive. A certain amount of iron powder (particle size 250 mesh, purity > 98%) was placed in a vacuum drying oven and dried at 90°C for 10 hours. Potassium perchlorate was placed in a tube furnace and dried at 100°C for 4 hours under an argon atmosphere.

[0037] Step 2: Preparation of fast burning and high calorific value heating powder

[0038] The pretreated metal iron powder, potassium perchlorate and aluminum-manganese alloy were placed in a glove box (water and oxygen contents were both <0.01ppm), weighed according to a mass ratio of 82%:16%:2%, and the mixed powder was placed in a sealed tank and mechanically mixed for 4 hours to make it evenly dispersed. The evenly mixed powder was placed in a glove box to avoid long-term exposure to the air.

[0039] Step 3: Forming and performance testing of a fast burning and high calorific value heating powder:

[0040] Weigh 6g of the evenly mixed heating powder and put it into the mold. The molding pressure applied to the heating powder is 20MPa. After standing for a period of time, demold the mold to prepare the heating sheet for burning rate test. Weigh 2g of the evenly mixed heating powder and put it into a crucible to test the calorific value of the heating powder. The burning rate and calorific value of the powder can be tested by conventional tests.

[0041] The burning rate test results of the heated powder tablets with 150nm aluminum-manganese metal alloy powder as additive are as follows: Figure 4 As shown in the figure, the burning speeds of the three samples are 50.2cm / s, 52.4cm / s and 51.5cm / s respectively, and the average burning speed of the heating sheet is 51.4cm / s. Figure 5 As shown in the figure, the calorific values ​​of the three samples are 1554.3 J / g, 1569.7 J / g and 1582.1 J / g respectively, and the average calorific value of the powder is 1568.8 J / g. The test results show that the introduction of aluminum-manganese alloy powder can increase the burning rate and calorific value by 328% and 21% respectively, which has a significant improvement effect.

[0042] Example 3

[0043] Step 1: Pretreatment of heating powder raw materials

[0044] Magnesium-zinc alloy powder with an average particle size of 100 nm was used as an additive. A certain amount of iron powder (particle size 300 mesh, purity > 98%) was placed in a vacuum drying oven and dried at 90°C for 10 hours. Potassium perchlorate was placed in a tube furnace and dried at 100°C for 4 hours in an argon atmosphere.

[0045] Step 2: Preparation of fast burning and high calorific value heating powder

[0046] The pretreated metal iron powder, potassium perchlorate and magnesium-zinc alloy were placed in a glove box (water and oxygen content were both <0.01ppm), and the mixed powder was placed in a sealed tank and mechanically mixed for 4 hours to make it evenly dispersed. The evenly mixed powder was placed in a glove box to avoid long-term exposure to the air.

[0047] Step 3: Forming and performance testing of a fast burning and high calorific value heating powder:

[0048] Weigh 6g of the evenly mixed heating powder and put it into the mold. The molding pressure applied to the heating powder is 20MPa. After standing for a period of time, demold it to prepare the heating sheet for burning rate test. Weigh 2g of the evenly mixed heating powder and put it into a crucible to test the calorific value of the heating powder. The burning rate and calorific value of the powder can be tested by conventional tests.

[0049] The burning rate test results of the heating powder tablets with 100nm magnesium-zinc metal alloy powder as an additive were 65.3cm / s, 67.5cm / s and 69.6cm / s respectively, and the average burning rate of the heating tablets was 67.5cm / s. The calorific value of the heating powder was 1439.2J / g, 1455.8J / g and 1443.6J / g respectively, and the average calorific value of the powder was 1446.2J / g. The test results show that the introduction of magnesium-zinc alloy powder can increase the burning rate and calorific value by 463% and 12% respectively.

[0050] Example 4

[0051] Step 1: Pretreatment of heating powder raw materials

[0052] A magnesium-zinc alloy with an average particle size of 50 nm was used as an additive. A certain amount of iron powder (particle size 250 mesh, purity > 98%) was placed in a vacuum drying oven and dried at 110°C for 12 hours. Potassium perchlorate was placed in a tube furnace and dried at 120°C for 6 hours under a nitrogen atmosphere.

[0053] Step 2: Preparation of fast burning and high calorific value heating powder

[0054] The pretreated metal iron powder, potassium perchlorate and magnesium-zinc alloy were placed in a glove box (water and oxygen contents were both <0.01ppm), weighed according to a mass ratio of 86%:12%:2%, and the mixed powder was placed in a sealed tank and mechanically mixed for 8 hours to make it evenly dispersed. The evenly mixed powder was placed in a glove box to avoid long-term exposure to the air.

[0055] Step 3: Forming and performance testing of a fast burning and high calorific value heating powder:

[0056] Weigh 6g of the evenly mixed heating powder and put it into the mold. The molding pressure applied to the heating powder is 30MPa. After standing for a period of time, demold the heating sheet for burning rate test. Weigh 2g of the evenly mixed heating powder and put it into a crucible to test the calorific value of the heating powder. The burning rate and calorific value of the powder can be tested by conventional tests.

[0057] The burning rate test results of the heating powder tablets with 50nm magnesium-zinc metal alloy powder as an additive were 77.8cm / s, 79.2cm / s and 78.5cm / s respectively, and the average burning rate of the heating tablets was 78.5cm / s. The calorific value of the heating powders was 1513.0J / g, 1533.1J / g and 1525.6J / g respectively, and the average calorific value of the powder was 1523.9J / g. The test results show that the introduction of magnesium-zinc alloy powder can increase the burning rate and calorific value by 554% and 18% respectively.

[0058] Example 5

[0059] Step 1: Pretreatment of heating powder raw materials

[0060] A magnesium-aluminum alloy with an average particle size of 200 nm was used as an additive. A certain amount of iron powder (particle size 400 mesh, purity > 98%) was placed in a vacuum drying oven and dried at 100°C for 11 hours. Potassium perchlorate was placed in a tube furnace and dried at 110°C for 5 hours under a nitrogen atmosphere.

[0061] Step 2: Preparation of fast burning and high calorific value heating powder

[0062] The pretreated metal iron powder, potassium perchlorate and magnesium-aluminum alloy were placed in a glove box (water and oxygen contents were both <0.01ppm), weighed according to a mass ratio of 80.5%:19%:0.5%, and the mixed powder was placed in a sealed tank and mechanically mixed for 6 hours to make it evenly dispersed. The evenly mixed powder was placed in a glove box to avoid long-term exposure to the air.

[0063] Step 3: Forming and performance testing of a fast burning and high calorific value heating powder:

[0064] Weigh 6g of the evenly mixed heating powder and put it into the mold. The molding pressure applied to the heating powder is 25MPa. After standing for a period of time, demold the heating sheet for burning rate test. Weigh 2g of the evenly mixed heating powder and put it into a crucible to test the calorific value of the heating powder. The burning rate and calorific value of the powder can be tested by conventional tests.

[0065] The burning rate test results of the heating powder tablets with 200nm magnesium-aluminum alloy powder as additives were 69.8cm / s, 65.7cm / s and 70.3cm / s respectively, and the average burning rate of the heating tablets was 68.6cm / s. The calorific value of the heating powders was 1433.0J / g, 1483.5J / g and 1454.0J / g respectively, and the average calorific value of the powders was 1456.8J / g. The test results show that the introduction of magnesium-aluminum alloy powder can increase the burning rate and calorific value by 572% and 13% respectively.

[0066] Example 6

[0067] Step 1: Pretreatment of heating powder raw materials

[0068] A magnesium-aluminum-zinc alloy with an average particle size of 150 nm was used as an additive. A certain amount of iron powder (particle size 400 mesh, purity > 98%) was placed in a vacuum drying oven and dried at 90°C for 10 hours. Potassium perchlorate was placed in a tube furnace and dried at 120°C for 6 hours in an argon atmosphere.

[0069] Step 2: Preparation of fast burning and high calorific value heating powder

[0070] The pretreated metal iron powder, potassium perchlorate and magnesium aluminum zinc alloy were placed in a glove box (water and oxygen contents were both <0.01ppm), weighed according to a mass ratio of 80%:19%:1%, and the mixed powder was placed in a sealed tank and mechanically mixed for 6 hours to make it evenly dispersed. The evenly mixed powder was placed in a glove box to avoid long-term exposure to the air.

[0071] Step 3: Forming and performance testing of a fast burning and high calorific value heating powder:

[0072] Weigh 6g of the evenly mixed heating powder and put it into the mold. The molding pressure applied to the heating powder is 25MPa. After standing for a period of time, demold the heating sheet for burning rate test. Weigh 2g of the evenly mixed heating powder and put it into a crucible to test the calorific value of the heating powder. The burning rate and calorific value of the powder can be tested by conventional tests.

[0073] The burning rate test results of the heating powder tablets with 150nm magnesium aluminum zinc metal alloy powder as additive were 45.2cm / s, 39.6cm / s and 42.8cm / s respectively, and the average burning rate of the heating tablets was 42.5cm / s. The calorific value of the heating powder was 1435.3J / g, 1443.9J / g and 1435.6J / g respectively, and the average calorific value of the powder was 1438.3J / g. The test results show that the introduction of magnesium aluminum zinc alloy powder can increase the burning rate and calorific value by 254% and 12% respectively.

[0074] Although the present invention has selected the preferred embodiments disclosed above, it is not intended to limit the present invention. Any researcher in the field can use the design parameters and contents in the above disclosed embodiments to change and modify the research scheme of the present invention without departing from the spirit and scope of the present invention. Therefore, any simple modification, parameter change and modification made to the above embodiments based on the research essence of the present invention without departing from the content of the present invention, all belong to the protection scope of the present invention.

Claims

1. A fast burning high calorific value heating powder, characterized in that: The raw materials of the heating powder are composed of 0.5-3.0% of metal alloy powder, 80-88% of metal iron powder and 12-19% of potassium perchlorate in terms of weight percentage.

2. A fast burning high calorific value heating powder as claimed in claim 1, characterized in that: The metal alloy powder is a binary / ternary metal alloy powder containing aluminum or magnesium, including but not limited to magnesium-zinc alloy, aluminum-manganese alloy, magnesium-aluminum alloy, aluminum-copper alloy, and magnesium-aluminum-zinc alloy.

3. A fast burning high calorific value heating powder as claimed in claim 1, characterized in that: The particle size of the metal alloy powder is 50 to 200 nm.

4. A fast burning high calorific value heating powder as claimed in claim 1, characterized in that: The particle size of the metal iron powder is less than 250 meshes and the purity is greater than 98%. Before use, the metal iron powder is dried in a vacuum drying oven at 90 to 110° C. for 10 to 12 hours to remove residual moisture in the iron powder.

5. The fast burning and high calorific value heating powder according to claim 1, characterized in that: The potassium perchlorate is placed in a tube furnace and dried at 100-120° C. for 4-6 hours in an inert gas atmosphere.

6. A method for preparing a fast burning high calorific value heating powder, characterized in that: Specifically, the three materials are weighed in a glove box according to the raw material mass ratio described in claim 1, and the weighed raw materials are placed in a sealed can and mechanically mixed evenly for 4 to 8 hours to obtain a fast burning rate and high calorific value heating powder.

Citation Information

Patent Citations

  • Formula of heating powder for thermal battery

    CN102244206A

Cited By

  • A high-heat-value fast-burning heating powder and a preparation method thereof

    CN122940504A