Preparation method of high-pressure gel polymer electrolyte based on interface modification

By using high-pressure gel polymer electrolyte with interface modification in lithium metal batteries, a stable inorganic solid electrolyte interface is formed, which solves the problem of instability of the electrode/electrolyte interface of lithium metal battery, and realizes a lithium battery with high energy density and long life. .

CN119069785APending Publication Date: 2024-12-03UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411200496.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The electrode/electrolyte interface instability of traditional lithium-ion batteries limits the development of high energy density lithium metal batteries, especially the instability of lithium metal and the instability of carbonate solvent anodes lead to battery short circuits and low Coulomb efficiency.

Method used

Using the high-pressure gel polymer electrolyte preparation method based on interface modification, a stable inorganic solid electrolyte interface (SEI) rich in LiF and Li3N is formed to improve lithium metal by introducing fluorine-based groups and amide groups on the lithium metal anode. Cycling stability and electrochemical properties of the battery.

Benefits of technology

The stable cycle of lithium batteries at high voltage is achieved, the stability of lithium metal anode and the energy density of the battery are improved, the battery life is extended, and the safety and Coulomb efficiency are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069785A_ABST
    Figure CN119069785A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-pressure gel polymer electrolyte based on interface modification, which comprises the following steps: 1) adding a lithium salt into a mixed solvent of methyl ethyl carbonate and fluoroethylene carbonate, and uniformly stirring and mixing to obtain a basic electrolyte; 2) adding a polymer monomer, a cross-linking agent and an initiator into the basic electrolyte, and uniformly mixing through magnetic stirring to obtain a precursor solution; and 3) putting the precursor solution into a drying oven at the temperature of 60-80 DEG C to react for 1-6 hours, so that the polymer monomer is subjected to polymerization reaction, and the gel-state polymer electrolyte is formed. According to the high-pressure gel polymer electrolyte based on interface modification, an amide functional group is introduced into a polymer matrix, so that ion conduction and construction of a stable anode-electrolyte interface are facilitated, growth of lithium dendrites can be inhibited, and side reactions of the electrolyte are reduced, so that the stability of a lithium metal anode is improved; the method is suitable for matching a high-voltage lithium battery cathode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrochemistry, and in particular relates to a method for preparing a high-voltage gel polymer electrolyte based on interface modification. Background Art

[0002] Lithium batteries are energy storage devices that play a key role in modern society. In recent years, the rapid development of consumer electronics and electric vehicles has posed a huge challenge to the energy density of lithium batteries. However, the limited energy density of traditional lithium-ion batteries can no longer meet the current development, so lithium metal anodes have attracted people's attention due to their high energy density (3860mAh / g) and lowest redox potential (-3.04V). At the same time, the energy density can be further improved when lithium metal is matched with cathode materials with high operating voltage and high specific capacity, such as layered transition metal oxides-nickel-rich oxides (LiNi x Co y Mn 1-x-y O2), which is an ideal cathode for high energy density lithium metal battery (LMB) applications due to its high cut-off voltage, high specific capacity and electrochemical cycling stability.

[0003] However, the instability of the electrode / electrolyte interface has limited the development of high-energy-density lithium metal batteries. In particular, the instability of lithium metal, such as the uncontrolled growth of lithium dendrites, can lead to battery short circuits and even thermal runaway. In addition, the traditional carbonate solvent anode has poor stability, and the polycarbonate formed by oxidative polymerization on the electrode surface is not stable enough under high pressure to form a stable SEI, which leads to low coulombic efficiency of the battery. The gel polymer electrolyte composed of a polymer network skeleton and a liquid electrolyte exhibits good physical and electrochemical properties. The polymer network skeleton can not only load the liquid electrolyte by swelling, thereby eliminating the leakage problem of the liquid battery, but also introduce special groups that can be used to modify the anode and electrolyte interface, such as fluorine groups can form a LiF-rich inorganic solid electrolyte interface (SEI) on the lithium metal side, ultimately improving the stability of the electrolyte to the anode, so that the battery can be stably cycled under high-voltage conditions. Therefore, by designing and screening polymer groups, skeleton structures and electrolyte components with good high voltage adaptability, high-voltage gel polymer electrolytes based on interface modification are developed to promote the formation of stable anode / electrolyte interfaces under high voltages, improve the cycle stability of gel polymer electrolytes in high-voltage cathode lithium metal batteries, and promote the application of gel polymer electrolytes in the field of high energy density batteries. Summary of the invention

[0004] The purpose of the present invention is to propose a method for preparing a high-voltage gel polymer electrolyte based on interface modification in view of the problems existing in the background technology. The preparation process of the present invention is simple, and the prepared gel polymer electrolyte has a stable electrochemical window close to 5V, which can be used in lithium batteries with high-voltage cathode materials, and is of great significance for obtaining lithium batteries with high energy density, high safety and long life.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a high-voltage gel polymer electrolyte based on interface modification comprises the following steps:

[0007] Step 1, preparing a basic electrolyte: adding lithium salt to a mixed solvent of ethyl methyl carbonate (EMC) and fluoroethylene carbonate (FEC), stirring and mixing evenly to obtain a basic electrolyte;

[0008] Step 2, preparing a precursor solution: adding a polymer monomer, a cross-linking agent and an initiator to the basic electrolyte obtained in step 1, and mixing them evenly by magnetic stirring to obtain a precursor solution;

[0009] Step 3: Polymerization reaction to generate a gel polymer electrolyte: The precursor solution obtained in step 2 is placed in an oven at 60-80° C. for 1-6 hours to allow the polymer monomers to undergo polymerization reaction to form a gel polymer electrolyte.

[0010] Furthermore, the lithium salt in step 1 is at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate), lithium tetrafluoroborate, and lithium difluorooxalatoborate.

[0011] Furthermore, the volume ratio of ethyl methyl carbonate to fluoroethylene carbonate in step 1 is (1-9):1.

[0012] Furthermore, the molar concentration of the lithium salt in the basic electrolyte in step 1 is 1 to 2 mol / L.

[0013] Furthermore, the polymer monomer in step 2 is N-isopropylacrylamide, N-ethylacrylamide or 3-acrylamidophenylboronic acid.

[0014] Furthermore, the cross-linking agent in step 2 is at least one of neopentyl glycol diacrylate, pentaerythritol tetraacrylate, tetraethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate.

[0015] Furthermore, the initiator in step 2 is azobisisobutyronitrile.

[0016] Furthermore, in the precursor solution prepared in step 2, the mass fraction of the polymer monomer is 1.8-6wt.%, the mass fraction of the cross-linking agent is 1.2-4wt.%, and the mass fraction of the initiator is 0.2wt%.

[0017] The present invention also provides the use of the interface-modified high-voltage gel polymer electrolyte prepared by the above method in a high-voltage high-nickel cathode lithium battery.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The present invention uses thermal initiation to cause a copolymerization reaction between the liquid phase monomer and the crosslinking agent, wherein the crosslinking agent contains two or more C=C bonds, which can form a three-dimensional crosslinked polymer network structure to improve the rigidity of the polymer network; the polymer monomer contains only one C=C bond, which is used to adjust the crosslinking degree of the three-dimensional crosslinked polymer, which is beneficial for the polymer electrolyte to maintain a higher Li + Conductivity;

[0020] 2. The amide group (NH-C=O) monomer used in the present invention has the following three main effects: First, the NH bond on the amide group can form a hydrogen bond with the C=O in the skeleton, which can be used as a polymer skeleton enhancer to greatly improve the stretchability and toughness of the electrolyte; second, the amide group has a high dielectric constant, has an affinity for lithium ions, and is conducive to ion conduction; finally, the amide group can construct a stable anode-electrolyte interface at the lithium metal anode, and spontaneously construct a composite organic / inorganic SEI structure containing rich nitrides at the anode, and this SEI structure has high ionic conductivity. For example, the inorganic Li3N structure (SEI) can inhibit the growth of lithium dendrites and reduce electrolyte side reactions, thereby improving the stability of the lithium metal anode and adapting to high-voltage high-nickel cathodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Cycling performance diagram of the gel polymer electrolyte prepared in Example 1 and the electrolyte prepared in Comparative Example 1 in NCM811 / / Li battery;

[0022] Figure 2 Linear voltage scanning curves of the gel polymer electrolyte prepared in Example 1 and the electrolyte prepared in Comparative Example 1 in a stainless steel (SS) / / Li battery;

[0023] Figure 3 This is an electrochemical floating test diagram after the gel polymer electrolyte prepared in Example 1 is matched with the NCM811 cathode;

[0024] Figure 4 The electrochemical floating test diagram after the electrolyte prepared in comparative example 1 is matched with the NCM811 cathode;

[0025] Figure 5 Impedance spectrum of SS / / SS symmetric battery assembled with gel electrolyte prepared in Example 1;

[0026] Figure 6 LiNi 0.8 Co 0.1 Mn 0.1 Li 1s diagram of the O2 / gel electrolyte / Li battery prepared in Example 1 after 100 cycles measured on the lithium metal anode side by X-ray photoelectron spectroscopy;

[0027] Figure 7 LiNi 0.8 Co 0.1 Mn 0.1 Li 1s diagram of the lithium metal anode measured by X-ray photoelectron spectroscopy after the O2 / electrolyte prepared in Comparative Example 1 / Li battery was cycled for 100 cycles. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, embodiments and comparative examples.

[0029] Example 1

[0030] A method for preparing a high-voltage gel polymer electrolyte based on interface modification specifically comprises the following steps:

[0031] Step 1, preparing a basic electrolyte: adding lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) to a mixed solvent of EMC and FEC, stirring and mixing evenly, to obtain a basic electrolyte containing 1 mol / L LiTFSI; wherein the volume ratio of EMC to FEC is 7:3;

[0032] Step 2, preparing a precursor solution: adding N-isopropylacrylamide, pentaerythritol tetraacrylate and azobisisobutyronitrile (AIBN) to the basic electrolyte obtained in step 1, and mixing them evenly by magnetic stirring to obtain a precursor solution; wherein, in the precursor solution, the mass fraction of N-isopropylacrylamide is 4.8wt.%, the mass fraction of pentaerythritol tetraacrylate is 3.2wt.%, and the mass fraction of azobisisobutyronitrile (AIBN) is 0.2wt.%;

[0033] Step 3: Polymerization reaction to generate a gel polymer electrolyte: The precursor solution obtained in step 2 is placed in an oven at 70° C. for 3 hours to allow the polymer monomers to undergo a polymerization reaction to form a high-pressure gel polymer electrolyte.

[0034] Comparative Example 1

[0035] The difference between Comparative Example 1 and Example 1 is that step 2 and step 3 are not implemented, and a liquid electrolyte containing 1 mol / L LiTFSI and a solvent of EMC / FEC (7:3) is obtained.

[0036] The polymer electrolytes prepared in Example 1 and Comparative Example 1 were assembled on LiNi 0.8 Co 0.1 Mn 0.1 The cycle stability of the battery, the oxidation resistance voltage of the electrolyte and the interface composition were tested in O2 / / Li, SS / / Li and SS / / SS button cells. 0.8 Co 0.1 Mn 0.1 The charge and discharge voltage range of the O2 / / Li battery is 3 to 4.4V. The first three cycles of the battery are activated at a rate of 0.1C, and then the cyclic charge and discharge test is carried out at a rate of 0.5C.

[0037] Figure 1 The cycle performance diagram of the gel polymer electrolyte prepared in Example 1 and the electrolyte prepared in Comparative Example 1 in the NCM811 / / Li battery. It can be seen that the NCM811 / / Li battery assembled in Example 1 can be stably cycled within a voltage range of 3 to 4.4V. Under 0.5C charge and discharge conditions, the initial specific capacity is 179.4mAh / g, and after 200 cycles, the capacity is still 131.4mAh / g, and the capacity retention rate is 73.3%. However, the NCM811 / / Li battery assembled in Comparative Example 1 has poor cycle stability, with an initial specific capacity of 191.3mAh / g. After 200 cycles at a rate of 0.5C, the capacity retention rate is only 53.2%.

[0038] Figure 2 The linear voltage scanning curves of the gel polymer electrolyte prepared in Example 1 and the electrolyte prepared in Comparative Example 1 in a stainless steel (SS) / / Li battery are used to measure the oxidation resistance voltage of the electrolyte. It can be seen that the electrochemical window of the polymer electrolyte is 5.0V, which is significantly better than the electrolyte prepared in Comparative Example 1 (4.5V), indicating that the gel polymer has high oxidation resistance and can be applied to lithium batteries with high voltage cathodes.

[0039] Figure 3 The electrochemical floating test diagram of the gel polymer electrolyte / Li battery prepared by NCM811 / Example 1 shows that the NCM811 battery assembled in Example 1 did not show large current fluctuations at a voltage of 4.5V, confirming the high stability of the SEI structure, once again indicating that this gel electrolyte can be applied to lithium batteries with high-voltage cathodes.

[0040] Figure 4The electrochemical floating test diagram of the NCM811 / electrolyte prepared in Comparative Example 1 / Li battery shows that the NCM811 battery assembled with this electrolyte has a large current fluctuation at a voltage of 4.3V, indicating that this electrolyte cannot form a stable SEI structure. Figure 1 This is consistent with the poor cycling performance of the electrolyte.

[0041] Figure 5 The impedance spectrum of the SS / / SS symmetrical battery assembled with the gel electrolyte prepared in Example 1. It can be calculated by the formula that the ionic conductivity of the gel electrolyte obtained in Example 1 is 6.10×10 -4 S / cm, which is close to that of traditional liquid electrolytes.

[0042] Figure 6 LiNi 0.8 Co 0.1 Mn 0.1 After the gel electrolyte / Li battery prepared in Example 1 was cycled 100 times, the Li 1s diagram measured on the lithium metal anode side by X-ray photoelectron spectroscopy showed that SEI film components such as LiF, Li3N and Li2CO3 were formed on the lithium metal surface. LiF mainly came from the decomposition of the lithium salt LiTFSI, Li3N came from the decomposition of LiTFSI and the amide group, and Li2CO3 came from the carbonate. LiF and Li3N, as effective components of the SEI film, can stabilize the lithium metal interface, inhibit the growth of lithium dendrites, and improve the cycle performance of the battery.

[0043] Figure 7 LiNi 0.8 Co 0.1 Mn 0.1 After the O2 / comparative example 1 electrolyte / Li battery was cycled for 100 cycles, the Li 1s graph measured by X-ray photoelectron spectroscopy on the lithium metal anode showed that although LiF and Li2CO3 were formed on the lithium metal surface, no Li3N was formed. Figure 1 The cycling performance indicates that the stability of the lithium metal interface can be further improved after gelling the electrolyte and introducing amide groups.

Claims

1. A method for preparing a high-pressure gel polymer electrolyte based on interface modification, characterized in that: The following steps are involved: Step 1, preparing a basic electrolyte: adding lithium salt to a mixed solvent of ethyl methyl carbonate and fluoroethylene carbonate, stirring and mixing evenly to obtain a basic electrolyte; Step 2, preparing a precursor solution: adding a polymer monomer, a crosslinking agent and an initiator to the basic electrolyte obtained in step 1, stirring and mixing to obtain a precursor solution; Step 3: Polymerization reaction to form a gel polymer electrolyte: The precursor solution obtained in step 2 is placed in an oven at 60 to 80° C. for reaction for 1 to 6 hours to form a gel polymer electrolyte.

2. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: The lithium salt in step 1 is at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(oxalatoborate), lithium tetrafluoroborate, and lithium difluorooxalatoborate.

3. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: The volume ratio of ethyl methyl carbonate to fluoroethylene carbonate in step 1 is (1-9):

1.

4. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: The molar concentration of the lithium salt in the basic electrolyte in step 1 is 1 to 2 mol / L.

5. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: The polymer monomer in step 2 is N-isopropylacrylamide, N-ethylacrylamide or 3-acrylamidophenylboronic acid.

6. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: The cross-linking agent in step 2 is at least one of neopentyl glycol diacrylate, pentaerythritol tetraacrylate, tetraethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate.

7. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: The initiator in step 2 is azobisisobutyronitrile.

8. The method for preparing a high-pressure gel polymer electrolyte based on interface modification according to claim 1, characterized in that: In the precursor solution prepared in step 2, the mass fraction of the polymer monomer is 1.8-6wt.%, the mass fraction of the cross-linking agent is 1.2-4wt.%, and the mass fraction of the initiator is 0.2wt%.

9. Use of the high-voltage gel polymer electrolyte prepared by the method according to any one of claims 1 to 8 in a high-voltage high-nickel cathode lithium battery.