Lithium battery diaphragm and preparation method thereof

By modifying nano silicon nitride and chitosan, the thermal stability and compatibility problems of lithium battery separator materials were solved, and heat-resistant, flame-retardant and highly breathable separators were prepared, which improved the safety of lithium batteries. and cycle performance.

CN119069950AActive Publication Date: 2024-12-03SHENZHEN GUANGXU TECH APPL NEW MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411117759.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-12-03
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing lithium battery separator materials have low thermal stability, are prone to short circuits and fires, and are poorly compatible with high-polar electrolytes, which cannot meet the needs of high-end fields.

Method used

The membrane is prepared by pulverizing, powder mixing, melt blending, extrusion, cooling and shaping and stretching processes, and the nanometers are improved by modification treatment. The properties of silicon nitride and chitosan form a heat-resistant, flame-retardant and highly breathable diaphragm.

Benefits of technology

The prepared lithium battery separator has excellent heat resistance, flame retardant properties and mechanical strength, which significantly improves the safety of the separator and the long cycle performance of the battery, and is suitable for high-end lithium-ion battery equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994140550000031
    Figure BDA0004994140550000031
  • Figure BDA0004994140550000041
    Figure BDA0004994140550000041
  • Figure BDA0004994140550000091
    Figure BDA0004994140550000091
Patent Text Reader

Abstract

The invention discloses a lithium battery diaphragm and a preparation method thereof, and belongs to the technical field of lithium battery diaphragms. Comprising the following raw materials in parts by weight: 40-60 parts of ultra-high molecular weight polyethylene, 20-32 parts of a pore forming agent, 6-10 parts of modified nano silicon nitride, 5-15 parts of modified chitosan, 0.1-0.2 part of an initiator and 1-3 parts of an antioxidant. Wherein the pore-forming agent is prepared by compounding polyvinyl alcohol and glycerol, and the prepared diaphragm is good in pore diameter consistency, high in air permeability and free of closed pores; the modified nano silicon nitride has good compatibility with a matrix, and can enhance the mechanical strength and heat resistance of the diaphragm; the prepared modified chitosan can obviously enhance the surface wettability, heat resistance and flame retardance of the lithium battery diaphragm, and the performance is long and stable; therefore, the prepared diaphragm is good in aperture consistency, high in air permeability and excellent in mechanical strength, has stable and efficient surface wettability, heat resistance and flame retardance, and has important application value in the technical field of lithium battery diaphragms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium battery separators, and in particular, relates to a lithium battery separator and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of the electric vehicle industry, the development of high-energy power equipment, especially the lithium battery industry, has been promoted worldwide. Lithium batteries, due to their high operating voltage and specific energy, fast charging and discharging, and high safety performance, are regarded as a common energy storage device with broad market prospects and rapid development.

[0003] Lithium batteries are mainly composed of four functional components: positive electrode, electrolyte, diaphragm, and negative electrode. In the structure of lithium batteries, the diaphragm is one of the key components of the inner layer. Although the diaphragm does not participate in the chemical reaction in lithium-ion batteries, it plays a vital role in the performance and safety of lithium batteries. Its main function is to separate the positive and negative electrodes of the battery, avoid short circuits caused by contact between the positive and negative electrodes, prevent byproducts (such as lithium dendrites) from diffusing from the redox reaction of the positive and negative electrode materials, and provide channels for lithium ion migration.

[0004] As lithium batteries become more and more complex, the performance requirements for separators are also getting higher and higher. At present, the most commonly used lithium battery separator materials on the market are polyolefin separators such as polyethylene and polypropylene. However, these materials have low thermal stability and will deform and shrink in size when heated at high temperatures, resulting in poor safety and easy to cause safety accidents such as short circuits. Polyolefin materials lack polar functional groups and have low compatibility with high-polarity electrolytes, resulting in poor wettability and large impedance during ion migration. In addition, polyethylene and polypropylene have low oxygen index and poor flame retardant properties. Once a fire accident occurs, this type of separator is very easy to ignite, and there is a risk of dripping and expanding the fire. It cannot meet the needs of high-end lithium-ion battery equipment. Therefore, it is urgent to invent a separator with excellent heat resistance, wettability and flame retardant properties to meet the higher requirements in the field of lithium battery separator technology. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a lithium battery separator and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a lithium battery separator comprises the following steps:

[0008] The ultra-high molecular weight polyethylene is crushed in a pulverizer, mixed with a pore-forming agent at high speed, and then added into a twin-screw extruder with modified nano silicon nitride, modified chitosan, an initiator and an antioxidant, melt-blended and extruded, cooled and shaped, and then longitudinally and transversely stretched to obtain a membrane. The membrane is immersed in ultrapure water for 1-2 hours, taken out, heat-shaped at high temperature, and rolled up to obtain a lithium battery separator.

[0009] Furthermore, the raw materials are calculated in parts by weight as follows: 40-60 parts of ultra-high molecular weight polyethylene, 20-32 parts of pore formers, 6-10 parts of modified nano silicon nitride, 5-15 parts of modified chitosan, 0.1-0.2 parts of initiators, and 1-3 parts of antioxidants.

[0010] Furthermore, the pore-forming agent is prepared by compounding polyvinyl alcohol and glycerol in a mass ratio of 1:3.

[0011] Furthermore, the high-speed mixing and stirring time is 10-20 minutes, and the mixing speed of the mixer is 2000-3000 r / min.

[0012] Furthermore, the heat setting temperature is 120-150°C.

[0013] Furthermore, the initiator is one of benzoyl peroxide and lauroyl peroxide.

[0014] Furthermore, the antioxidant is a hindered phenol antioxidant.

[0015] The pore-forming agent is a compound of polyvinyl alcohol and glycerol. It is highly water-soluble and can form a microporous structure when dissolved in water. It has the advantages of low cost and high environmental protection, and has good pore size consistency, high air permeability, and no closed pores.

[0016] Furthermore, the modified nano silicon nitride is prepared by the following steps:

[0017] At room temperature, add nano silicon nitride and ethanol aqueous solution into a flask, stir at high speed for 15 minutes under a high shear mixing emulsifier, add vinyl trimethoxysilane (silane coupling agent KH-171), continue to stir at high speed for 45 minutes under a high shear mixing emulsifier, and after the reaction is completed, filter, vacuum dry, and grind to obtain modified nano silicon nitride.

[0018] Furthermore, the usage ratio of the nano silicon nitride, the ethanol aqueous solution and the vinyltrimethoxysilane is 2g:100mL:4.5g.

[0019] Nano silicon nitride is a ceramic powder with excellent performance, good high temperature resistance and mechanical properties. By modifying nano silicon nitride, the surface hydrophobicity of nano silicon nitride is improved, the compatibility of nano silicon nitride with polyethylene matrix is ​​enhanced, the agglomeration of nano silicon nitride is reduced, the performance of nano silicon nitride can be fully exerted, and the heat resistance and mechanical properties of the matrix are greatly enhanced. The modified nano silicon nitride also contains carbon-carbon double bonds and can cross-link with the matrix to further enhance the mechanical strength of the matrix.

[0020] Furthermore, the modified chitosan is prepared by the following steps:

[0021] S1. Mix 4-hydroxystyrene and toluene, add them to a three-necked round-bottom flask equipped with a thermometer, a magnetic stirring system and a spherical condenser, add formaldehyde solution (mass fraction 24%) dropwise under ice-water bath conditions, and continue stirring for 30 minutes, then add 4,4'-diaminodiphenyl sulfone, control the reaction temperature to 65°C, keep the reaction warm for 6 hours, and after the reaction is completed, cool to room temperature, remove the solvent by rotary evaporation, and then purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 3:1), remove the eluent by rotary evaporation to obtain intermediate 1; the ratio of the amount of 4-hydroxystyrene, toluene, formaldehyde solution, and 4,4'-diaminodiphenyl sulfone is 11.9g:100mL:30mL:25.1g;

[0022] 4-Hydroxystyrene reacts with 4,4'-diaminodiphenyl sulfone to obtain intermediate 1; the specific reaction process is as follows:

[0023]

[0024] S2, in a three-necked flask equipped with a stirring device, glutaraldehyde, 4,4'-diaminodiphenyl sulfone, piperidine (condensing agent) and toluene were mixed and stirred uniformly, the reaction temperature was controlled to 60°C, and the reaction was kept warm for 6 hours. After the reaction was completed, it was naturally cooled, and the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 2; the ratio of glutaraldehyde, 4,4'-diaminodiphenyl sulfone, piperidine and toluene was 12.2g:39.2g:15mL:120mL;

[0025] Under the action of the condensing agent, the amino group on 4,4'-diaminodiphenyl sulfone condenses with the aldehyde group on glutaraldehyde to form an imine group (C=N Schiff base structure), and by controlling the molar ratio of the two to be close to 1:1 and a slight excess of glutaraldehyde, only one aldehyde group on glutaraldehyde participates in the reaction to obtain intermediate 2; the specific reaction process is as follows:

[0026]

[0027] S3, chitosan was added to a mixed solution of acetic acid and toluene (the mass fraction of acetic acid was 28%), stirred until completely dissolved, and then intermediate 2 and piperidine were added. After stirring at room temperature for 1 hour, sodium hydroxide solution (mass fraction 35%) was added to adjust the pH to 9, and the reaction was continued for 3 hours. After the reaction was completed, the mixture was allowed to stand for precipitation, filtered, washed with ethanol and water in turn, and dried in an oven to obtain modified chitosan; the ratio of the mixed solution of acetic acid and toluene, chitosan, intermediate 2, and piperidine was 100mL:5g:8.5g:20mL;

[0028] Under the action of the condensation agent, the aldehyde group on the intermediate 2 condenses with the amino group on the chitosan to form an imine group (C=N Schiff base structure) to obtain modified chitosan;

[0029] Chitosan is a polysaccharide. The large number of hydroxyl groups in the molecule can promote the dehydration of the polyethylene matrix into carbon, converting the matrix into a high-concentration carbon layer, and improving the flame retardant properties of the matrix. In addition, the main chain of chitosan contains a large number of ether groups, which enables chitosan to adsorb polysulfides, improve the conductivity of the battery, and improve the utilization rate and rate performance of the active substance sulfur. In addition, by modifying chitosan, the interfacial compatibility between chitosan and polyethylene can be improved. The performance of the modified chitosan is fully exerted; in addition, the modified chitosan molecule also contains diphenyl sulfone, benzoxazine, Schiff base and carbon-carbon double bond structure, among which diphenyl sulfone has good high temperature resistance and thermal oxidation resistance, and desulfurizes under heat to generate SO2, sulfurous acid and water, which can promote the Fries rearrangement reaction of the silicone rubber matrix, accelerate the carbonization of the matrix, and effectively enhance the flame retardant properties of the matrix; the introduced benzoxazine can further enhance the heat resistance of the matrix; the C=N double bond in the Schiff base structure can generate a carbon-nitrogen six-membered ring at high temperature. This type of six-membered ring structure enables the matrix to form a stable cross-linked network, which can synergize with diphenyl sulfone and greatly enhance the flame retardant properties of the matrix; finally, the introduction of carbon-carbon double bonds in the modified chitosan can produce cross-linking with the matrix, because the modified chitosan molecule contains a large number of hydroxyl groups, which can enhance the hydrophilicity of the matrix, so that the diaphragm has good adsorption affinity with the electrolyte, reduce the impedance of ion migration, and improve the long cycle performance of the battery.

[0030] It should be noted that grafting organic molecular chains onto chitosan can improve the resistance to migration and exudation of small organic molecules and improve the stability of the performance of modified chitosan.

[0031] Beneficial effects of the present invention:

[0032] 1. The lithium battery diaphragm pore-forming agent prepared by the present invention is prepared by compounding polyvinyl alcohol and glycerol, has strong water solubility, and the prepared diaphragm has good pore consistency, high air permeability, and no closed pores;

[0033] 2. Modification of nano silicon nitride has better compatibility with the substrate than ordinary nano silicon nitride, reduces agglomeration, and can greatly enhance the mechanical strength and heat resistance of the diaphragm;

[0034] 3. The prepared modified chitosan can significantly enhance the surface wettability, heat resistance and flame retardancy of lithium battery separators, and the performance is long-lasting and stable, not easy to fall off, and can also enhance the long cycle performance of the battery;

[0035] Therefore, the diaphragm prepared by the present invention has good pore size consistency, high air permeability, excellent mechanical strength, and stable and efficient surface wettability, heat resistance and flame retardancy, and has important application value in the field of lithium battery diaphragm technology. DETAILED DESCRIPTION

[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] Preparation of modified chitosan:

[0039] S1. Mix 11.9 g of 4-hydroxystyrene with 100 mL of toluene, add the mixture into a three-necked round-bottom flask equipped with a thermometer, a magnetic stirring system and a spherical condenser, add 30 mL of formaldehyde solution (mass fraction 24%) dropwise in an ice-water bath, and continue stirring for 30 min, then add 25.1 g of 4,4'-diaminodiphenyl sulfone, control the reaction temperature to 65 ° C, keep the reaction warm for 6 h, and after the reaction is completed, cool to room temperature, remove the solvent by rotary evaporation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 3:1), and remove the eluent by rotary evaporation to obtain intermediate 1;

[0040] S2, in a three-necked flask equipped with a stirring device, 12.2g of glutaraldehyde, 39.2g of 4,4'-diaminodiphenyl sulfone, 15mL of piperidine and 120mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 60°C, and the reaction was kept warm for 6h. After the reaction was completed, it was naturally cooled, and the solvent was distilled off under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0041] S3. Add 5 g of chitosan to 100 mL of a mixed solution of acetic acid and toluene (the mass fraction of acetic acid is 28%), stir until completely dissolved, then add 8.5 g of intermediate 2 and 20 mL of piperidine, stir and react at room temperature for 1 h, then add sodium hydroxide solution (mass fraction 35%) to adjust the pH to 9, continue the reaction for 3 h, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan.

[0042] Example 2

[0043] Preparation of modified chitosan:

[0044] S1. Mix 23.8 g of 4-hydroxystyrene with 200 mL of toluene, add the mixture into a three-necked round-bottom flask equipped with a thermometer, a magnetic stirring system and a spherical condenser, add 30 mL of formaldehyde solution (mass fraction 24%) dropwise in an ice-water bath, and continue stirring for 30 min, then add 50.2 g of 4,4'-diaminodiphenyl sulfone, control the reaction temperature to 65 ° C, keep the reaction warm for 6 h, and after the reaction is completed, cool to room temperature, remove the solvent by rotary evaporation, and purify by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 3:1), and remove the eluent by rotary evaporation to obtain intermediate 1;

[0045] S2, in a three-necked flask equipped with a stirring device, 24.4g of glutaraldehyde, 78.4g of 4,4'-diaminodiphenyl sulfone, 30mL of piperidine and 240mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 60°C, and the reaction was kept warm for 6h. After the reaction was completed, it was naturally cooled, and the solvent was distilled off under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 3:2), and the eluent was removed by rotary evaporation to obtain intermediate 2;

[0046] S3. Add 10 g of chitosan to a mixed solution of 200 mL of acetic acid and toluene (the mass fraction of acetic acid is 28%), stir until completely dissolved, then add 17 g of intermediate 2 and 40 mL of piperidine, stir and react at room temperature for 1 h, add sodium hydroxide solution (mass fraction 35%) to adjust the pH to 9, continue the reaction for 3 h, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan.

[0047] Example 3

[0048] Preparation of modified nano silicon nitride:

[0049] At room temperature, add 2 g of nano silicon nitride and 100 mL of ethanol aqueous solution into a flask, stir at high speed for 15 min under a high shear mixer emulsifier, add 4.5 g of vinyltrimethoxysilane, continue to stir at high speed for 45 min under a high shear mixer emulsifier, and after the reaction is completed, filter, vacuum dry, and grind to obtain modified nano silicon nitride.

[0050] Example 4

[0051] Preparation of modified nano silicon nitride:

[0052] At room temperature, 4 g of nano silicon nitride and 200 mL of ethanol aqueous solution were added to a flask, and the mixture was stirred at high speed for 15 min under a high shear mixer emulsifier. 9 g of vinyl trimethoxysilane was added, and the mixture was stirred at high speed for 45 min under a high shear mixer emulsifier. After the reaction was completed, the mixture was filtered, vacuum dried, and ground to obtain modified nano silicon nitride.

[0053] Example 5

[0054] 40g of ultra-high molecular weight polyethylene was put into a pulverizer for pulverization, and then mixed and stirred at high speed with 20g of a pore-forming agent (prepared from 5g of polyvinyl alcohol and 15g of glycerol) for 10min at a stirring speed of 2000r / min. Then, 6g of the modified nano silicon nitride prepared in Example 3, 5g of the modified chitosan prepared in Example 1, 0.1g of benzoyl peroxide and 1g of antioxidant 1010 were added to a twin-screw extruder, melt-blended and extruded, cooled and shaped, and then longitudinally and transversely stretched to obtain a membrane. The membrane was immersed in ultrapure water for 1h, taken out, heat-shaped at a high temperature of 120°C, and rolled up to obtain a lithium battery separator with a thickness of.

[0055] Example 6

[0056] 50g of ultra-high molecular weight polyethylene was put into a pulverizer for pulverization, and then mixed and stirred at high speed with 28g of a pore-forming agent (prepared from 7g of polyvinyl alcohol and 21g of glycerol) for 15min at a stirring speed of 2500r / min. Then, 8g of the modified nano-silicon nitride prepared in Example 4, 10g of the modified chitosan prepared in Example 2, 0.2g of benzoyl peroxide and 2g of antioxidant 1010 were added to a twin-screw extruder, melt-blended and extruded, cooled and shaped, and then longitudinally and transversely stretched to obtain a membrane. The membrane was immersed in ultrapure water for 2h, taken out, heat-set at a high temperature of 130°C, and rolled up to obtain a lithium battery separator.

[0057] Example 7

[0058] 60g of ultra-high molecular weight polyethylene was put into a pulverizer for pulverization, and then mixed and stirred at high speed with 32g of a pore-forming agent (prepared from 8g of polyvinyl alcohol and 24g of glycerol) for 20min at a stirring speed of 3000r / min. Then, 10g of the modified nano-silicon nitride prepared in Example 4, 15g of the modified chitosan prepared in Example 2, 0.2g of benzoyl peroxide and 3g of antioxidant 1010 were added to a twin-screw extruder, melt-blended and extruded, cooled and shaped, and then longitudinally and transversely stretched to obtain a membrane. The membrane was immersed in ultrapure water for 2h, taken out, heat-set at a high temperature of 150°C, and rolled up to obtain a lithium battery separator.

[0059] Comparative Example 1

[0060] Ordinary chitosan of the same mass was used to replace the modified chitosan in Example 7, and the remaining steps were the same as in Example 7 to prepare a diaphragm.

[0061] Comparative Example 2

[0062] A commercially available polyethylene separator for lithium batteries was used.

[0063] The following performance tests were performed on Examples 5-7 and Comparative Examples 1-2:

[0064] The national standard GB / T 2406-2008 "Test method for combustion performance of plastics" is used to measure the limiting oxygen index of the sample before and after being placed at room temperature for 180 days;

[0065] The tensile strength was determined using the national standard GB / T 1040.3-2006 "Determination of tensile properties of plastics Part 3: Test conditions for films and sheets";

[0066] The thermal shrinkage of the sample was determined using the national standard GB / T 36363-2018 "Polyolefin separators for lithium-ion batteries";

[0067] The mass of the dry battery diaphragm is recorded as M0, and then the diaphragm is completely immersed in the electrolyte, the residual electrolyte on the surface is carefully wiped off with filter paper, and it is weighed again. The weight at this time is recorded as M1. The calculation formula for the liquid absorption rate is as follows: (M1-M0) / M0×100%.

[0068] The measured results are shown in Table 1:

[0069] Table 1

[0070]

[0071] The lithium battery separators of Examples 5-7 and Comparative Examples 1-2 were assembled into half-cells with lithium iron phosphate as the positive electrode and graphite as the negative electrode. The specific test method was as follows: the charging current was 2 mA, the charging cut-off voltage was ≥4.3 V, and the discharge cut-off voltage was ≤2.5 V. The capacity retention rate was tested after 1500 cycles.

[0072] The measured results are shown in Table 2:

[0073] Table 2

[0074]

[0075] It can be seen from the above table that the diaphragm prepared in the embodiment of the present invention has excellent mechanical strength, stable and efficient surface wettability, heat resistance and flame retardancy, and can also enhance the long cycle performance of the battery, and has important application value in the field of lithium battery diaphragm technology.

[0076] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0077] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A lithium battery separator, characterized in that: The invention comprises the following raw materials in parts by weight: 40-60 parts of ultra-high molecular weight polyethylene, 20-32 parts of pore-forming agent, 6-10 parts of modified nano silicon nitride, 5-15 parts of modified chitosan, 0.1-0.2 parts of initiator, and 1-3 parts of antioxidant; Wherein, the modified chitosan is prepared by the following steps: S1. Mix 4-hydroxystyrene and toluene, add formaldehyde solution dropwise under ice-water bath, and continue stirring for 30 min, then add 4,4'-diaminodiphenyl sulfone, react at 65°C for 6 h. After the reaction is complete, cool to room temperature, perform rotary evaporation, purify by column chromatography, and perform rotary evaporation to obtain intermediate 1. S2, glutaraldehyde, 4,4'-diaminodiphenyl sulfone, piperidine and toluene were mixed and stirred evenly, and reacted at 60°C for 6 hours. After the reaction was completed, the mixture was naturally cooled, distilled under reduced pressure, purified by column chromatography, and rotary evaporated to obtain intermediate 2; S3. Add chitosan to the mixed solution of acetic acid and toluene, stir until completely dissolved, then add intermediate 2 and piperidine, stir and react at room temperature for 1 hour, adjust the pH to 9, continue the reaction for 3 hours, and after the reaction is completed, let it stand and precipitate, filter, wash and dry to obtain modified chitosan.

2. A lithium battery separator according to claim 1, characterized in that: In step S1, the ratio of the amount of 4-hydroxystyrene, toluene, formaldehyde solution, and 4,4'-diaminodiphenyl sulfone is 11.9 g: 100 mL: 30 mL: 25.1 g.

3. A lithium battery separator according to claim 1, characterized in that: In step S2, the ratio of glutaraldehyde, 4,4'-diaminodiphenyl sulfone, piperidine and toluene is 12.2 g:39.2 g:15 mL:120 mL.

4. A lithium battery separator according to claim 1, characterized in that: In step S3, the ratio of the mixed solution of acetic acid and toluene, chitosan, intermediate 2, and piperidine is 100 mL: 5 g: 8.5 g: 20 mL.

5. A lithium battery separator according to claim 1, characterized in that: The pore-forming agent is prepared by compounding polyvinyl alcohol and glycerol in a mass ratio of 1:

3.

6. A lithium battery separator according to claim 1, characterized in that: The initiator is one of benzoyl peroxide and lauroyl peroxide.

7. A lithium battery separator according to claim 1, characterized in that: The antioxidant is a hindered phenol antioxidant.

8. A lithium battery separator according to claim 1, characterized in that: The modified nano silicon nitride is prepared by the following steps: At room temperature, add nano silicon nitride and ethanol aqueous solution into a flask, stir, add vinyltrimethoxysilane, continue stirring, and when the reaction is complete, filter, vacuum dry, and grind to obtain modified nano silicon nitride.

9. The method for preparing a lithium battery separator according to claim 1, characterized in that: The following steps are involved: The ultra-high molecular weight polyethylene is crushed in a pulverizer, mixed with a pore-forming agent at high speed, and then added into a twin-screw extruder with modified nano silicon nitride, modified chitosan, an initiator and an antioxidant, melt-blended and extruded, cooled and shaped, and then longitudinally and transversely stretched to obtain a membrane. The membrane is immersed in ultrapure water, taken out, heat-shaped at high temperature, and rolled up to obtain a lithium battery separator.

Citation Information

Patent Citations

  • Coating film composition for battery electrodes or separators, battery electrode or separator provided with coating film obtained by using same, and battery provided with battery electrode or separator

    CN105027328A

  • Slurry composition and lithium ion battery diaphragm containing same

    CN105273444A

  • Preparation method and application of multifunctional lithium-sulfur battery separator

    CN109346647A

  • A multipurpose emergency hood

    KR102097761B1

  • Binder for secondary battery, composite separator and secondary battery prepared by using the same

    KR102368234B1