Display substrate, preparation method thereof and display equipment
By using microcavity cushions of different materials in OLED display technology, ensuring that their refractive index matches color light, the problem of light efficiency differences caused by inconsistent microcavity structure thickness is solved and the display balance is improved.
Patent Information
- Application Number
- CN202310627137.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing OLED display technology, due to the inconsistent thickness of microcavity structures of sub-pixels of different colors, the light effect of light is different, which affects the display balance.
By using different materials in the microcavity cushion layer of each sub-pixel, the refractive index matches the corresponding color light, thereby adjusting the microcavity structure to meet the constructive interference conditions and reducing the thickness difference of the microcavity cushion layer.
The display balance of each sub-pixel is improved, the difference in light and light effects is reduced, and the display effect is enhanced.
Smart Images

Figure CN119072148A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of display technology, and in particular to a display substrate and a preparation method thereof, and a display device. Background Art
[0002] OLED (Organic Light Emitting Diode) is an organic thin film electroluminescent device, which has the advantages of simple preparation process, low cost, high luminous efficiency, easy to form a flexible structure, etc. Therefore, the display technology using OLED has become an important display technology.
[0003] In order to improve the display effect of OLED products, the current OLED products mostly use the microcavity effect to improve the light output efficiency. Specifically, each sub-pixel in the display substrate of the OLED product adopts a microcavity structure to enhance the light output efficiency. In the prior art, the thickness of the microcavity structure is mainly adjusted by adjusting the thickness of the microcavity cushion layer in each sub-pixel, so that the microcavity structure of each sub-pixel meets the constructive interference condition of the color light corresponding to the sub-pixel.
[0004] However, due to the difference in color light emitted by sub-pixels of different colors, the thickness of the microcavity structure in different sub-pixels is inconsistent. The thickness of the microcavity structure affects the light output efficiency, resulting in differences in the light output efficiency of different sub-pixels, resulting in poor display balance of each sub-pixel. Summary of the invention
[0005] The purpose of the embodiments of the present invention is to provide a display substrate and a manufacturing method thereof, and a display device to improve the display balance of each sub-pixel. The specific technical solution is as follows:
[0006] In a first aspect, an embodiment of the present invention provides a display substrate, wherein the display substrate comprises:
[0007] A display substrate, comprising:
[0008] substrate;
[0009] A plurality of sub-pixels having a microcavity structure are located on the substrate;
[0010] The materials of the microcavity pads in the microcavity structures of the sub-pixels are different, and the refractive index of the microcavity pads in the microcavity structures of the sub-pixels matches the color light corresponding to the sub-pixels; the refractive index of the microcavity pads matching each color light is such that the microcavity structure where the microcavity pads are located satisfies the constructive interference condition of the color light.
[0011] Optionally, the plurality of sub-pixels in the display substrate include: a first sub-pixel and a second sub-pixel;
[0012] The material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride;
[0013] The formation order of the microcavity pad layer in the first sub-pixel is earlier than the formation order of the microcavity pad layer in the second sub-pixel.
[0014] Optionally, the first sub-pixel is a blue sub-pixel, and the second sub-pixel is a green sub-pixel.
[0015] Optionally, each sub-pixel further includes:
[0016] An undercut structure is located on a side of the sub-pixel microcavity pad away from the substrate;
[0017] The undercut structure of each sub-pixel includes a first material layer and a second material layer; the first material layer is located at a layer of the second material layer away from the substrate.
[0018] Optionally, the material of the first material layer in the undercut structure of each sub-pixel is the same as the material of the microcavity pad layer with the slowest etching rate in each sub-pixel;
[0019] The material of the second material layer in the undercut structure of each sub-pixel is different from the material of the microcavity pad layer with the slowest etching rate in each sub-pixel.
[0020] Optionally, the material of the second material layer in the undercut structure of each sub-pixel is different from the material of the microcavity pad layer with the fastest etching rate in each sub-pixel;
[0021] The material of the second material layer in the undercut structure of each sub-pixel is the same as the material of the microcavity pad layer with the fastest etching rate in each sub-pixel.
[0022] Optionally, in each sub-pixel, the first material layer is formed later than the second material layer.
[0023] Optionally, the material of the first material layer is silicon oxide, and the material of the second material layer is silicon nitride.
[0024] Optionally, the display substrate further includes a peripheral area:
[0025] The peripheral region includes a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence;
[0026] Wherein, the first silicon oxide layer is in the same layer as the microcavity pad layer in the first sub-pixel; the second silicon nitride layer is in the same layer as the microcavity pad layer in the second sub-pixel;
[0027] The second silicon nitride layer is in the same layer as the second material layer, and the second silicon oxide layer is in the same layer as the first material layer.
[0028] Optionally, each sub-pixel further includes:
[0029] A reflective electrode layer, located between the substrate and the microcavity pad layer;
[0030] A light-emitting layer and a semi-transparent electrode layer stacked in sequence on a side of the undercut structure away from the substrate;
[0031] Wherein, the reflective electrode layer and the semi-transparent electrode layer form a microcavity structure.
[0032] Optionally, each sub-pixel further includes:
[0033] The reflective electrode protection layer is located between the reflective electrode layer and the microcavity pad layer.
[0034] Optionally, the microcavity pad layer of each sub-pixel includes a via hole; the via hole is used to electrically connect structures on both sides of the microcavity pad layer.
[0035] Optionally, a via taper of a via hole in the microcavity pad layer of each sub-pixel is less than 45°.
[0036] Optionally, the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel and the wavelength of the color light corresponding to the sub-pixel satisfy the following constraints:
[0037]
[0038] Among them, A is the optical path in the microcavity structure of the sub-pixel excluding the pixel pad layer, and is the same in the microcavity structures of each sub-pixel, n is the refractive index of the microcavity pad layer in the microcavity structure of the sub-pixel, d is the thickness of the microcavity pad layer in the microcavity structure of the sub-pixel, k is a positive integer, and λ is the wavelength of the color light corresponding to the sub-pixel.
[0039] In a second aspect, an embodiment of the present invention provides a display device, comprising a display substrate as described in any one of the first aspects.
[0040] In a third aspect, an embodiment of the present invention provides a method for preparing a display substrate, the method comprising:
[0041] providing a substrate;
[0042] forming a plurality of sub-pixels having a microcavity structure on the substrate;
[0043] The materials of the microcavity pads in the microcavity structures of the sub-pixels are different, and the refractive index of the microcavity pads in the microcavity structures of the sub-pixels matches the wavelength of the color light corresponding to the sub-pixels; the refractive index of the microcavity pads matching each color light is such that the microcavity structure where the microcavity pads are located satisfies the constructive interference condition of the color light.
[0044] Optionally, forming a plurality of sub-pixels having a microcavity structure on the substrate includes:
[0045] forming a reflective electrode layer of each sub-pixel on the substrate;
[0046] On the side of the reflective electrode layer of each sub-pixel away from the substrate, using materials corresponding to each sub-pixel, the microcavity cushion layers of each sub-pixel are sequentially formed; the materials corresponding to each sub-pixel are different, and the refractive index of the material corresponding to each sub-pixel matches the color light of the sub-pixel;
[0047] A light-emitting layer and a semi-transparent electrode layer of each sub-pixel are formed on the side of the microcavity pad layer of each sub-pixel away from the substrate; wherein the reflective electrode layer and the semi-transparent electrode layer of each sub-pixel constitute a microcavity structure.
[0048] Optionally, the microcavity pads of the sub-pixels are sequentially formed on the side of the reflective electrode layer of each sub-pixel away from the substrate using materials matching the color light corresponding to each sub-pixel, including:
[0049] According to the order of etching rates of the materials corresponding to the sub-pixels from small to large, the microcavity pads of the sub-pixels are formed in sequence using the materials corresponding to the sub-pixels on the side of the reflective electrode layer of the sub-pixels away from the substrate.
[0050] Optionally, the plurality of sub-pixels in the display substrate include: a first sub-pixel and a second sub-pixel; an etching rate of a material corresponding to the first sub-pixel is lower than an etching rate of a material corresponding to the second sub-pixel;
[0051] The method comprises: forming a microcavity pad layer of each sub-pixel by using the materials corresponding to each sub-pixel in sequence of etching rates from small to large on the side of the reflective electrode layer of each sub-pixel away from the substrate, comprising:
[0052] On a side of the reflective electrode of each sub-pixel away from the substrate, forming a first material film using a material corresponding to the first sub-pixel;
[0053] Etching the first material film to form a microcavity pad layer of the first sub-pixel;
[0054] On a side of the reflective electrode of each sub-pixel away from the substrate, forming a second material film using a material corresponding to the second sub-pixel;
[0055] The second material film is etched to form a microcavity pad layer of the second sub-pixel.
[0056] Optionally, the material corresponding to the first sub-pixel is silicon oxide, and the material corresponding to the second sub-pixel is silicon nitride.
[0057] Optionally, a ratio of an etching rate of a material corresponding to the first sub-pixel to an etching rate of a material corresponding to the second sub-pixel is less than or equal to a preset ratio threshold.
[0058] Optionally, after sequentially forming the microcavity pad layer of each sub-pixel on the side of the reflective electrode layer of each sub-pixel away from the substrate using materials corresponding to each sub-pixel, and before forming the light-emitting layer and the semi-transparent electrode layer of each sub-pixel on the side of the microcavity pad layer of each sub-pixel away from the substrate, the method further includes:
[0059] Using the material of the microcavity pad layer with the slowest etching rate in each sub-pixel, a second material layer is formed on a side of the microcavity pad layer of each sub-pixel away from the substrate;
[0060] Using the material of the microcavity pad layer with the fastest etching rate in each sub-pixel, a first material layer is formed on a side of the second material layer of each sub-pixel away from the substrate;
[0061] The first material layer and the second material layer of each sub-pixel are etched to form an undercut structure of each sub-pixel.
[0062] Beneficial effects of the embodiments of the present invention:
[0063] A display substrate and a preparation method thereof, and a display device provided by an embodiment of the present invention, wherein the display substrate includes a substrate and a plurality of sub-pixels having a microcavity structure, each sub-pixel being located on the substrate; the materials of the microcavity pad in the microcavity structure of each sub-pixel are different, and the refractive index of the microcavity pad in the microcavity structure of each sub-pixel matches the wavelength of the color light corresponding to each sub-pixel; the refractive index of the microcavity pad matched with each color light is such that the microcavity structure where the microcavity pad is located satisfies the constructive interference condition of the color light. Since the materials of the microcavity pad in the microcavity structure of each sub-pixel are different, the refractive index of the microcavity pad in the microcavity structure of different sub-pixels is different, so that the refractive index of the microcavity pad can be adjusted by adjusting the material of the microcavity pad, so that the microcavity structure of the sub-pixel satisfies the constructive interference condition of the corresponding color light, therefore, compared with only adjusting the thickness of the microcavity pad, by adjusting the material of the microcavity pad, the thickness difference of the microcavity pad in the microcavity structure of each sub-pixel of different wavelengths can be reduced, thereby reducing the difference in light output efficiency of different sub-pixels, thereby improving the display balance of each sub-pixel.
[0064] Of course, it is not necessary to achieve all of the advantages described above at the same time to implement any product or method of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can also be obtained based on these drawings.
[0066] Figure 1 is a schematic diagram of a microcavity structure of a sub-pixel;
[0067] Figure 2 It is a schematic diagram of the structure of a display substrate in the prior art;
[0068] Figure 3 A schematic structural diagram of a display substrate provided by an embodiment of the present invention;
[0069] Figure 4 A schematic diagram of the structure of a first sub-pixel provided by an embodiment of the present invention;
[0070] Figure 5 A schematic diagram of the structure of a second sub-pixel provided by an embodiment of the present invention;
[0071] Figure 6 A schematic diagram of the structure of a third sub-pixel provided in an embodiment of the present invention;
[0072] Figure 7 A schematic flow chart of a method for preparing a first display substrate provided by an embodiment of the present invention;
[0073] Figure 8 A schematic flow chart of a second method for preparing a display substrate provided by an embodiment of the present invention;
[0074] Fig. 9 A schematic diagram of forming a first display substrate provided by an embodiment of the present invention;
[0075] Fig.10 A schematic diagram of forming a second display substrate provided by an embodiment of the present invention;
[0076] Fig.11 A schematic diagram of forming a third display substrate provided by an embodiment of the present invention;
[0077] Fig.12 A schematic diagram of forming a fourth display substrate provided by an embodiment of the present invention;
[0078] Fig.13 A schematic diagram of forming a fifth display substrate provided by an embodiment of the present invention;
[0079] Fig.14 A schematic diagram of forming a sixth display substrate provided by an embodiment of the present invention;
[0080] Fig.15 A schematic diagram of forming a seventh display substrate provided by an embodiment of the present invention;
[0081] Fig.16 A schematic diagram of forming an eighth display substrate provided by an embodiment of the present invention;
[0082] Fig.17 A schematic diagram of forming a ninth display substrate provided by an embodiment of the present invention.
[0083] Description of Reference Numerals
[0084] Base 31
[0085] Sub-pixel 32
[0086] Microcavity pad 321
[0087] Undercut structure 322
[0088] First material layer 3221
[0089] Second material layer 3222
[0090] Reflective electrode layer 323
[0091] Luminescent layer 324
[0092] Semi-transparent electrode layer 325
[0093] Reflective electrode protection layer 326
[0094] Via 327 DETAILED DESCRIPTION
[0095] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.
[0096] In order to improve the display effect of OLED products, current OLED products mostly use the microcavity effect to improve the display light efficiency. Specifically, each sub-pixel in the display substrate of the OLED product adopts a microcavity structure to meet the constructive interference condition of the light wave, that is, the optical path of the microcavity structure is an integer multiple of the half wavelength of the light wave. At this time, due to constructive interference, the light output effect of the light wave can be enhanced. Figure 1As shown, a schematic diagram of a microcavity structure of a sub-pixel is shown, the microcavity structure includes a total reflection surface and a semi-transparent surface (also called the light emitting layer of the sub-pixel). After the light wave in the microcavity structure reaches the semi-transparent surface of the sub-pixel, part of it is reflected and part of it is transmitted, so that there are continuously oscillating light waves in the microcavity structure. When the optical path between the total reflection surface and the semi-transparent surface is an integer multiple of half the wavelength of the light wave, due to constructive interference, the light emitting effect of the light wave can be enhanced.
[0097] In the prior art, the thickness of the microcavity structure is adjusted mainly by adjusting the thickness of the microcavity cushion layer in each sub-pixel, so that the microcavity structure of each sub-pixel satisfies the constructive interference condition of the light wave. Figure 2 As shown, a structural schematic diagram of a display substrate in the prior art includes sub-pixel 1 and sub-pixel 2, wherein the light wave of the color light corresponding to sub-pixel 1 is smaller than the light wave of the color light corresponding to sub-pixel 2, the microcavity structure of sub-pixel 1 includes microcavity pad 1, the microcavity structure of sub-pixel 2 includes microcavity pad 2, and the thickness of microcavity pad 1 is smaller than the thickness of microcavity pad 2, so that the thickness D1 of the microcavity structure of sub-pixel 1 is smaller than the thickness D2 of the microcavity structure of sub-pixel 2.
[0098] Due to the difference in wavelengths of light emitted by sub-pixels of different colors, the thickness of the microcavity structure in different sub-pixels is inconsistent. Due to the existence of the light absorption effect, the thickness of the microcavity structure also affects the light output efficiency, resulting in differences in the light output efficiency of different sub-pixels, resulting in poor display balance of each sub-pixel.
[0099] In order to reduce the difference between the light emitting effects of different sub-pixels and improve the display balance of each sub-pixel, an embodiment of the present invention provides a display substrate. Figure 3 As shown, an embodiment of the present invention provides a display substrate, including:
[0100] Base 31;
[0101] A plurality of sub-pixels 32 having a microcavity structure;
[0102] Wherein, each sub-pixel 32 is located on the substrate 31;
[0103] The materials of the microcavity pad 321 in the microcavity structure of each sub-pixel 32 are different, and the refractive index of the microcavity pad 321 in the microcavity structure of each sub-pixel 32 matches the color light corresponding to each sub-pixel 32; the refractive index of the microcavity pad matching each color light is such that the microcavity structure where the microcavity pad is located satisfies the constructive interference condition of the color light.
[0104] The display substrate 100 may be, for example, an organic light emitting diode display substrate (OLED), a micro light emitting diode (Micro Light Emitting Diodes, Micro LED for short) display substrate or a mini light emitting diode (Mini Light Emitting) display substrate, etc., and the present invention does not specifically limit this. In one implementation, the substrate 31 may be a rigid substrate or a flexible substrate, wherein the rigid substrate may be made of glass, quartz or plastic, etc., and the flexible substrate may be made of PET (Polyethylene terephthalate), PEN (Polyethylenenaphthalate two formic acid glycol ester), PI (Polyimide), etc.
[0105] Each sub-pixel included in the display substrate may include multiple types of sub-pixels, and the color of the color light corresponding to the different types of sub-pixels is the color that the sub-pixel needs to display. For example, the display substrate includes red (R) sub-pixels, green (G) sub-pixels, and blue (B) sub-pixels, etc., wherein the color light required to be displayed by the red sub-pixel is red light, with a wavelength range of 622 to 760nm; the color light required to be displayed by the green sub-pixel is green light, with a wavelength range of 492 to 577nm; the color light required to be displayed by the blue sub-pixel is blue light, with a wavelength range of 435 to 450nm. Each sub-pixel 32 is located on the substrate 31, which means that each sub-pixel 32 can be directly on the substrate 31, or there can be an intermediate layer between each sub-pixel 32 and the substrate 31, which is all possible.
[0106] In one implementation, the microcavity structure may include a total reflection surface and a semi-transparent surface, that is, in the embodiment of the present invention, the sub-pixel with the microcavity structure includes a total reflection surface and a semi-transparent surface, and the optical path between the total reflection surface and the semi-transparent surface meets the constructive interference condition of the color light emitted by the sub-pixel. Optionally, the total reflection surface may be a reflective electrode layer, such as an anode composed of materials Al (aluminum), Ti (titanium), and Ag (silver), and the semi-transparent surface may be a semi-transparent electrode layer, which may be composed of a plurality of material layers with different refractive indices, such as a metal / dielectric multilayer film, and the present invention does not specifically limit this.
[0107] The wavelengths of the color lights corresponding to different sub-pixels in the display substrate are inconsistent. In order to make different sub-pixels use the microcavity effect to enhance the luminous effect, it means that the optical paths of the color lights emitted by different sub-pixels are different. In the prior art, the refractive index of each structural layer in the microcavity structure of different sub-pixels in the display substrate is the same. In order to make different sub-pixels use the microcavity effect to enhance the display light effect, when the refractive index of each structural layer is the same, the optical paths of the microcavity structures of different sub-pixels can only be adjusted by adjusting the thickness of the sub-pixel microcavity structure. Specifically, each sub-pixel microcavity structure includes a microcavity cushion layer, and the thickness of the sub-pixel microcavity structure is mainly adjusted by adjusting the thickness of the microcavity cushion layer. Since the thickness of the microcavity structure in different sub-pixels is inconsistent, and the thickness of the microcavity structure affects the light output effect, the light output effect of different sub-pixels is different, resulting in poor display balance of each sub-pixel.
[0108] In order to improve the display balance of each sub-pixel, in the embodiment of the present invention, the materials of the microcavity pad in the microcavity structure of each sub-pixel 32 in the display substrate are different, and the refractive index of the microcavity pad 321 in the microcavity structure of each sub-pixel 32 matches the wavelength of the color light corresponding to each sub-pixel 32; the refractive index of the microcavity pad matching each color light is such that the microcavity structure where the microcavity pad is located satisfies the constructive interference condition of the color light. Since the materials of the microcavity pad in the microcavity structure of each sub-pixel are different, the refractive index of the microcavity pad in the microcavity structure of different sub-pixels is different, so that the refractive index of the microcavity pad is adjusted by adjusting the material of the microcavity pad, so that the microcavity structure of the sub-pixel satisfies the constructive interference condition of the corresponding color light. Since the optical path is the product of the refractive index and thickness of the medium, compared with the case where the refractive index in the microcavity cushion layer of each sub-pixel is the same, by adjusting the microcavity cushion layer material, the difference in the thickness of the microcavity cushion layer in each sub-pixel can be reduced, thereby reducing the difference in the microcavity structure in the sub-pixel, thereby reducing the difference in the light emitting efficiency of the sub-pixel, and improving the display balance of each sub-pixel.
[0109] In one implementation, the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel and the wavelength of the color light corresponding to the sub-pixel satisfy the following constraints:
[0110]
[0111] Among them, A is the optical path in the microcavity structure of the sub-pixel excluding the pixel pad layer, and is the same in the microcavity structure of each sub-pixel, n is the refractive index of the microcavity pad layer in the microcavity structure of the sub-pixel, d is the thickness of the microcavity pad layer in the microcavity structure of the sub-pixel, k is a positive integer, and λ is the wavelength of the color light corresponding to the sub-pixel.
[0112] For example, the display substrate includes sub-pixel 1 and sub-pixel 2, wherein:
[0113] The wavelength of the color light emitted by sub-pixel 1 is λ1, the refractive index of the microcavity cushion layer in its microcavity structure is n1, and the thickness of the microcavity cushion layer in the microcavity structure is d1, then:
[0114]
[0115] The wavelength of the color light emitted by sub-pixel 2 is λ2, the refractive index of the microcavity cushion layer in its microcavity structure is n2, and the thickness of the microcavity cushion layer in the microcavity structure is d2, then:
[0116]
[0117] For sub-pixel 1 and sub-pixel 2, the optical paths in their microcavity structures except for the pixel pad layer are the same, that is, they have the same A. Therefore, the refractive index and / or thickness of the microcavity pad layer can be adjusted to make sub-pixel 1 and sub-pixel 2 meet the above constraints.
[0118] In one implementation, when the k value of each sub-pixel in the display substrate is the same, the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel is positively correlated with the wavelength of the color light corresponding to each sub-pixel. When the k value is the same, the longer the wavelength of the corresponding color light, the greater the refractive index of the microcavity cushion layer. For example, when the k value is the same, the display substrate contains red sub-pixels, green sub-pixels, and blue sub-pixels. Since the wavelength of red light is greater than the wavelength of green light and the wavelength of blue light, the refractive index of the microcavity cushion layer in the red sub-pixel is greater than the refractive index of the microcavity cushion layer in the green sub-pixel and the refractive index of the microcavity cushion layer in the blue sub-pixel. Since the optical path is the product of the refractive index and thickness of the medium, compared with the case where the refractive index in the microcavity cushion layer of each sub-pixel is the same, the difference in the thickness of the microcavity cushion layer in each sub-pixel can be reduced by adjusting the refractive index.
[0119] In the prior art, the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel is the same, so the optical path is adjusted only by thickness to match the wavelength of the sub-pixel with the corresponding color light, which results in different thicknesses of different sub-pixels. Based on this, in the embodiment of the present invention, a refractive index adjustment method is adopted to match the wavelength of the sub-pixel with the corresponding color light, so as to reduce the thickness difference between each sub-pixel, thereby improving the display balance of each sub-pixel.
[0120] In one approach, the optical path and wavelength can be matched only by adjusting the refractive index. In this case, the thickness of the microcavity cushion layer in the microcavity structure of each sub-pixel is the same, and the difference in light output effects of different sub-pixels can be minimized.
[0121] In another way, the thickness and refractive index of the microcavity cushion layer can be adjusted at the same time, thereby enriching the means of adjusting the optical path to better match different business needs. It should be noted that for the embodiment of the present invention, since the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel is positively correlated with the wavelength of the color light corresponding to each sub-pixel, even if there is a difference in the thickness of the microcavity cushion layer in the microcavity structure of each sub-pixel, the degree of difference between the microcavity cushion layers is less than the degree of difference in thickness between the microcavity cushion layers under the same refractive index in the related art.
[0122] In order to match the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel with the wavelength of the color light corresponding to each sub-pixel, in the embodiment of the present invention, the material of the microcavity cushion layer in the microcavity structure of each sub-pixel is a material with adjustable refractive index. Optionally, the material with adjustable refractive index includes at least one of SiO (silicon oxide), SiN (silicon nitride), and Al2O3 (aluminum oxide. The refractive index of each of the above materials can be adjusted by adjusting the film forming parameters. For example, in the process of generating SiO, different particles can be doped in the process of preparing SiO to adjust the refractive index of SiO.
[0123] In one implementation, the material of the microcavity pad in the microcavity structure of each sub-pixel in the display substrate is the same, for example, the material of the microcavity pad in multiple sub-pixel microcavity structures can all be SiO, but the refractive index of the material SiO of the microcavity pad in different sub-pixel microcavity structures is different. In another implementation, the material of the microcavity pad in the microcavity structure of each sub-pixel in the display substrate can be different, for example, the material of the microcavity pad in the microcavity structure of the green sub-pixel is SiN, and the material of the microcavity pad in the microcavity structure of the blue sub-pixel is SiO.
[0124] Optionally, since different materials have different etching rates, and the materials of the microcavity pads of different sub-pixels in the present application are different, in order to reduce etching losses, in the present application, the formation order of the microcavity pads in the microcavity structure of each sub-pixel is inversely proportional to the etching rate of the material of the microcavity pads. In simple terms, the slower the etching rate of the material, the earlier the formation order of the microcavity pads formed by the material.
[0125] In one implementation, the plurality of sub-pixels in the display substrate include: a first sub-pixel and a second sub-pixel, and the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Since the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the formation order of the microcavity pad layer in the first sub-pixel is earlier than the formation order of the microcavity pad layer in the second sub-pixel, that is, the microcavity pad layer of the first sub-pixel is first formed by using silicon oxide, and then the microcavity pad layer of the second sub-pixel is formed by using silicon nitride.
[0126] Optionally, the first sub-pixel may be a blue sub-pixel, and the second sub-pixel may be a green sub-pixel.
[0127] In one implementation, in order to improve the stability of the sub-pixel structure, each sub-pixel 32 further includes: an undercut structure located on a side of the sub-pixel microcavity pad away from the substrate;
[0128] like Figure 4 As shown, an embodiment of the present invention provides a schematic structural diagram of a sub-pixel, each sub-pixel includes a microcavity pad 321 and an undercut structure 322, wherein the undercut structure 322 includes a first material layer 3221 and a second material layer 3222, and the first material layer 3221 is located in a layer of the second material layer 3222 away from the substrate. Due to the existence of the undercut structure 322, when it is necessary to form other structural layers on the undercut structure 322, the structural layer fills the recessed portion of the undercut structure 322, thereby improving the stability of the combination.
[0129] In one implementation, the material of the first material layer 3221 in the undercut structure 322 of each sub-pixel 32 is the same as the material of the microcavity pad layer 321 with the slowest etching rate in each sub-pixel 32; the material of the second material layer 3222 in the undercut structure 322 of each sub-pixel 32 is different from the material of the microcavity pad layer 321 with the slowest etching rate in each sub-pixel 32.
[0130] Exemplarily, in the case where each sub-pixel includes the first sub-pixel and the second sub-pixel, the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Since the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the material of the microcavity pad layer with the slowest etching rate in each sub-pixel is silicon nitride. In this case, the material of the first material layer is silicon nitride, and the material of the first material layer is not silicon nitride.
[0131] In one implementation, the material of the second material layer 3222 in the undercut structure 322 of each sub-pixel 32 is different from the material of the microcavity pad 321 with the fastest etching rate in each sub-pixel 32; the material of the second material layer 3222 in the undercut structure 322 of each sub-pixel 32 is the same as the material of the microcavity pad 321 with the fastest etching rate in each sub-pixel 32.
[0132] Exemplarily, in the case where each sub-pixel includes the first sub-pixel and the second sub-pixel, the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Since the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the material of the microcavity pad layer with the fastest etching rate in each sub-pixel is silicon oxide. In this case, the material of the second material layer is silicon oxide, and the material of the first material layer is not silicon oxide.
[0133] Based on the above example, in one implementation, the material of the first material layer 3221 in the undercut structure 322 of each sub-pixel 32 is the same as the material of the microcavity pad 321 with the slowest etching rate in each sub-pixel 32; the material of the second material layer 3222 in the undercut structure 322 of each sub-pixel 32 is the same as the material of the microcavity pad 321 with the fastest etching rate in each sub-pixel 32.
[0134] Exemplarily, in the case where each sub-pixel includes the first sub-pixel and the second sub-pixel, the material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride. Since the etching rate of silicon oxide is lower than the etching rate of silicon nitride, the material of the microcavity pad layer with the slowest etching rate in each sub-pixel is silicon nitride, and the material of the microcavity pad layer with the fastest etching rate in each sub-pixel is silicon oxide. In this case, the material of the first material layer is silicon nitride, and the material of the second material layer is silicon oxide.
[0135] On this basis, in one implementation, in addition to the sub-pixels, the display panel also includes a peripheral area, and the peripheral area is open to retain all or part of the material layers involved in the sub-pixel manufacturing process. In one implementation, the peripheral area includes a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence; wherein the first silicon oxide layer is in the same layer as the microcavity pad layer in the first sub-pixel; the second silicon nitride layer is in the same layer as the microcavity pad layer in the second sub-pixel; the second silicon nitride layer is in the same layer as the second material layer, and the second silicon oxide layer is in the same layer as the first material layer.
[0136] Since the material of the first material layer in the bottom cut structure of each sub-pixel is the same as the material of the microcavity pad layer with the slowest etching rate in each sub-pixel, and the material of the second material layer in the bottom cut structure of each sub-pixel is the same as the material of the microcavity pad layer with the fastest etching rate in each sub-pixel, therefore, in order to form a small upper and large lower recessed portion in the bottom cut structure, the formation order of the first material layer in each sub-pixel is later than the formation order of the second material layer, so that the first material layer is located on the side of the second material layer away from the backplane, and at the same time, when etching the recessed portion, since the etching rate of the first material layer is slower and the etching rate of the second material layer is faster, a small upper and large lower recessed portion is formed.
[0137] Based on the above examples, Figure 4 As shown, each sub-pixel 32 further includes:
[0138] The reflective electrode layer 323 is located between the substrate 31 and the microcavity pad layer 321;
[0139] Located on the side of the undercut structure 322 away from the substrate 31, a light emitting layer 324 and a semi-transparent electrode layer 325 are stacked in sequence;
[0140] The reflective electrode layer 323 and the semi-transparent electrode layer 325 form a microcavity structure.
[0141] The thickness and refractive index of the reflective electrode layer, the light-emitting layer and the semi-transparent electrode layer in each sub-pixel are the same, that is, the total optical path of the reflective electrode layer, the light-emitting layer and the semi-transparent electrode layer in each sub-pixel is the same. Therefore, the total optical path of the sub-pixel can be adjusted by adjusting the thickness and / or refractive index of the microcavity pad layer to match the optical path of the color light emitted by the sub-pixel.
[0142] In one implementation, when the reflective electrode layer is made of a material that is easily corroded (such as Al), Figure 4 Based on the sub-pixel structure shown, Figure 5 As shown, an embodiment of the present invention provides a structural schematic diagram of a sub-pixel. In order to protect the reflective electrode layer, each sub-pixel also includes a reflective electrode protection layer 326 located between the reflective electrode layer 323 and the microcavity pad layer 321. The material of the reflective electrode protection layer 326 can be a corrosion-resistant conductive material such as ITO (indium tin oxide).
[0143] Generally speaking, the microcavity pad of each sub-pixel is not conductive. Therefore, in order to ensure that the structures on both sides of the microcavity pad can be electrically connected, a via (Via) can be set in the microcavity pad of each sub-pixel, wherein the via can be made of conductive material, so that the via can be conductive to electrically connect the structures on both sides of the microcavity pad.
[0144] In one implementation, when the structures on both sides of the microcavity pad layer include a reflective electrode layer and a light-emitting layer, the via holes in each microcavity pad layer can realize electrical connection between the reflective electrode layer and the light-emitting layer. Figure 4 Based on the sub-pixel structure shown, Figure 6 As shown, an embodiment of the present invention provides a schematic diagram of the structure of a sub-pixel, wherein the microcavity pad layer 321 includes a via 327. For another example, when the structures on both sides of the microcavity pad layer include a reflective electrode protection layer and a light-emitting layer, the vias in each microcavity pad layer can realize electrical connection between the reflective electrode protection layer and the light-emitting layer. For another example, when the structures on both sides of the microcavity pad layer include a reflective electrode layer and an ITO layer, the vias in each microcavity pad layer can realize electrical connection between the reflective electrode layer and the ITO layer.
[0145] In one implementation, in the case of a structure in which vias are used to connect two sides of a microcavity pad layer, a via taper of a via in the microcavity pad layer of each sub-pixel is less than a specified angle threshold, and the via taper is as follows: Figure 6 The θ shown in . The above-mentioned specified angle threshold can be controlled according to demand and experience. Optionally, in order to ensure that the structures on both sides of the microcavity cushion layer overlap without abnormality, the above-mentioned specified angle threshold can be 45°.
[0146] In one embodiment, the present invention further provides a display device, comprising the display substrate provided by the above embodiment of the present invention. Optionally, the above display device includes but is not limited to a mobile phone, a computer, a television, a game console, a car display, etc.
[0147] In order to reduce the difference between the light emitting effects of different sub-pixels and improve the display balance of each sub-pixel, the display substrate provided in the embodiment of the present application is as follows: Figure 7 As shown, an embodiment of the present invention provides a method for preparing a display substrate, comprising steps S701-S702, wherein:
[0148] S701, providing a substrate;
[0149] Before generating the display substrate, a substrate may be provided, which may be a rigid substrate or a flexible substrate, which is not specifically limited in the present invention. In one implementation, the substrate may include a CMOS (Complementary Metal-Oxide-Semiconductor) substrate.
[0150] S702, forming a plurality of sub-pixels having a microcavity structure on a substrate; wherein the materials of the microcavity cushion layers in the microcavity structures of the sub-pixels are different, and the refractive index of the microcavity cushion layers in the microcavity structures of the sub-pixels matches the wavelength of the color light corresponding to the sub-pixels; and the refractive index of the microcavity cushion layers matching each color light is such that the microcavity structure where the microcavity cushion layers are located satisfies the constructive interference condition of the color light.
[0151] In this step, a plurality of sub-pixels having a microcavity structure can be formed on the provided substrate, wherein the material of the microcavity cushion layer in the microcavity structure of each sub-pixel is different, and the refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel matches the wavelength of the color light corresponding to each sub-pixel.
[0152] In the embodiment of the present invention, since the refractive index of the microcavity pad layer matched with each color light is such that the microcavity structure where the microcavity pad layer is located satisfies the constructive interference condition of the color light, it means that the microcavity structure of the sub-pixel can be made to satisfy the constructive interference condition of the corresponding color light by adjusting the refractive index of the microcavity pad layer. Therefore, compared with the method of only adjusting the thickness of the microcavity pad layer, the method of adjusting the refractive index of the microcavity pad layer can reduce the thickness difference of the microcavity pad layer in the microcavity structure of each sub-pixel of different wavelengths, thereby reducing the difference in light emitting efficiency of different sub-pixels, thereby improving the display balance of each sub-pixel.
[0153] In one embodiment, in order to form a plurality of sub-pixels having a microcavity structure on a substrate, Figure 7 Based on the scheme shown, Figure 8As shown, an embodiment of the present invention provides a method for preparing a display substrate, and the above step S702 may include steps S801-S803, wherein:
[0154] S801, forming a reflective electrode layer of each sub-pixel on a substrate;
[0155] The reflective electrode layer may be an anode layer or a cathode layer of a sub-pixel, which is acceptable.
[0156] Optional, such as Fig. 9 As shown in the schematic diagram of forming a display substrate, metal coating can be first performed on the substrate to obtain a metal film. Optionally, metals such as Al (aluminum), Ti (titanium), and Ag (silver) can be used for coating, and the obtained metal film has a total reflection characteristic for light. After the metal film is formed, photoresist can be evenly applied on the formed metal film. After the formed metal film is formed, photolithography can be performed first, that is, light of a specific wavelength can be used to irradiate the photoresist on the preset reflective electrode mask. For the non-light-shielding area on the reflective electrode mask, the photoresist on the metal film below will receive light, and then the photosensitizer in the photoresist will undergo a photochemical reaction.
[0157] If the photoresist is a positive photoresist, the chemical composition of the irradiated area of the positive photoresist (corresponding to the non-light-shielding area in the reflective electrode mask) changes, so that it can be dissolved in the developer, while the chemical composition of the non-irradiated area (corresponding to the light-shielding area in the reflective electrode mask) remains unchanged and is insoluble in the developer. If the photoresist is a negative photoresist, the chemical composition of the non-irradiated area of the negative photoresist (corresponding to the light-shielding area in the reflective electrode mask) changes, so that it can be dissolved in the developer, while the chemical composition of the irradiated area (corresponding to the non-light-shielding area in the reflective electrode mask) remains unchanged and is insoluble in the developer.
[0158] After the irradiation is finished, the photoresist on the metal layer is cleaned with a developer, so that the photoresist on the metal layer that is soluble in the developer is dissolved, while the photoresist that is insoluble in the developer is retained. Fig.10 As shown in a schematic diagram of forming a display substrate, the photoresist remains on the metal layer after being cleaned with a developer.
[0159] After cleaning with a developer, the metal layer can be further etched. Different etching methods can be used according to different usage scenarios and requirements. In one implementation, the area on the metal layer not covered by the photoresist can be dry-etched. There are many dry etching methods, such as sputtering and ion beam milling, plasma etching (Plasma Etching), high-pressure plasma etching, high-density plasma etching, reactive ion etching, etc. In one implementation, the area on the metal layer not covered by the photoresist can be wet-etched. Wet etching is a purely chemical reaction process, which refers to the use of the chemical reaction between the solution and the material to be etched to remove the area not covered by the photoresist to achieve the etching purpose. Such as Fig.11 As shown in a schematic diagram of forming a display substrate, after etching the metal layer, reflective electrode layers of different sub-pixels are obtained.
[0160] In one implementation, when the reflective electrode layer is made of a material that is easily corroded, such as aluminum, a reflective electrode protection layer may be formed on the reflective electrode layer using a corrosion-resistant conductive material in order to protect the reflective electrode layer. Optionally, the reflective electrode layer may be coated with a corrosion-resistant conductive material, and the reflective electrode protection layer may be formed on the reflective electrode layer by coating, exposing, developing, and etching. Fig.12 As shown in the schematic diagram of forming a display substrate, a reflective electrode protection layer is formed on the reflective electrode layer. Optionally, the corrosion-resistant conductive material may be ITO.
[0161] S802, on the side of the reflective electrode layer of each sub-pixel away from the substrate, using materials corresponding to each sub-pixel, sequentially forming a microcavity cushion layer of each sub-pixel; the materials corresponding to each sub-pixel are different, and the refractive index of the material corresponding to each sub-pixel matches the color light of the sub-pixel;
[0162] After the reflective electrode layer of each pixel is obtained, the microcavity pad layer of each sub-pixel can be formed in sequence on the side of the reflective electrode layer of each sub-pixel away from the substrate using the material corresponding to each sub-pixel.
[0163] Optionally, due to the formation of Fig.11 He Ru Fig.12 Therefore, before forming a microcavity cushion layer whose refractive index is positively correlated with the wavelength of the color light corresponding to each sub-pixel, the trench can be filled. Fig.12 Based on this, the trench is filled to obtain Fig.13 Schematic diagram of formation of display substrate shown. Optionally, SiO can be used to fill the trench, specifically, SiO coating can be performed, and then glue coating and dry etching can be performed to fill the trench, thereby reducing the transfer of the step of the reflective electrode layer onto the semi-transparent electrode layer.
[0164] After the trench is filled, a microcavity pad of each subpixel can be formed using a material corresponding to each subpixel on the side of the reflective electrode layer of each subpixel away from the substrate; wherein the refractive index of the material corresponding to each subpixel matches the wavelength of the color light corresponding to each subpixel.
[0165] In one implementation, the microcavity pad layer of each sub-pixel can be formed in sequence using the materials corresponding to each sub-pixel on the side of the reflective electrode layer of each sub-pixel away from the substrate in the order of the etching rates of the materials corresponding to each sub-pixel from small to large. The microcavity pad layers of different sub-pixels are generated in sequence in the order of the etching rates of different pad layers from slow to fast, thereby avoiding etching losses.
[0166] Optionally, the multiple sub-pixels in the above-mentioned display substrate include: a first sub-pixel and a second sub-pixel; and an etching rate of a material corresponding to the first sub-pixel is smaller than an etching rate of a material corresponding to the second sub-pixel.
[0167] Optionally, the ratio of the etching rate of the material corresponding to the first sub-pixel to the etching rate of the material corresponding to the second sub-pixel is less than or equal to a preset ratio threshold. In one implementation, the preset ratio threshold may be 1:20.
[0168] On this basis, the above-mentioned method of forming the microcavity pad layer of each sub-pixel in sequence using the materials corresponding to each sub-pixel in the order of etching rates from small to large on the side of the reflective electrode layer of each sub-pixel away from the substrate may include steps A1-A2:
[0169] Step A1, forming a first material film using a material corresponding to the first sub-pixel on a side of the reflective electrode of each sub-pixel away from the substrate; etching the first material film to form a microcavity pad layer of the first sub-pixel;
[0170] Optionally, a first material film may be formed using a material corresponding to the first sub-pixel, and then the first material film may be subjected to coating, exposure, development and etching to obtain a microcavity pad layer of the first sub-pixel. Fig.14 As shown, an embodiment of the present invention provides a schematic diagram of a display substrate formation process, wherein a first material film is formed using a material corresponding to a first sub-pixel, and then glue coating, exposure, development and etching are performed to form a microcavity pad layer of the first sub-pixel. In one implementation method, a via structure can be formed at the same time to facilitate the subsequent formation of vias.
[0171] Step A2, forming a second material film using a material corresponding to the second sub-pixel on a side of the reflective electrode of each sub-pixel away from the substrate; etching the second material film to form a microcavity pad layer of the second sub-pixel;
[0172] Since the etching rate of the material corresponding to the first sub-pixel is lower than that of the material corresponding to the second sub-pixel, the microcavity pad layer of the second sub-pixel needs to be formed after the microcavity pad layer of the first sub-pixel is formed, thereby reducing etching loss.
[0173] Optionally, a second material film may be formed using the material corresponding to the second sub-pixel, and then the second material film may be etched to form a microcavity pad layer of the second sub-pixel. Fig.15 As shown, an embodiment of the present invention provides a schematic diagram of a display substrate formation process, wherein a second material film is formed using a material corresponding to a second sub-pixel, and then glue coating, exposure, development and etching are performed to form a microcavity pad layer of the second sub-pixel. In one implementation method, a via structure can be formed at the same time to facilitate the subsequent formation of vias.
[0174] In one implementation, the material corresponding to the first sub-pixel is silicon oxide, and the material corresponding to the second sub-pixel is silicon nitride. In this case, a silicon oxide film can be formed first, and then a microcavity pad layer of the first sub-pixel can be etched, and then a silicon nitride film can be formed, and then a microcavity pad layer of the second sub-pixel can be further etched.
[0175] S803, forming a light-emitting layer and a semi-transparent electrode layer of each sub-pixel on a side of the microcavity cushion layer of each sub-pixel away from the substrate; wherein the reflective electrode layer and the semi-transparent electrode layer of each sub-pixel constitute a microcavity structure.
[0176] Optional, in getting Fig.15 After the structure shown in the figure, ITO film formation, coating, exposure and development can be performed, and dry etching can be performed to open the sub-pixel space, and at the same time, the ITO layer vias on the microcavity pad layer of each sub-pixel can be electrically connected to the structure under the pad layer. Fig.16 , which is a schematic diagram of a display substrate forming process provided by an embodiment of the present invention, wherein an ITO layer is formed on a microcavity pad layer.
[0177] In order to improve the stability of the sub-pixel structure, after the microcavity pad layer of each sub-pixel is formed in sequence using the material corresponding to each sub-pixel on the side of the reflective electrode layer of each sub-pixel away from the substrate, and before the light-emitting layer and the semi-transparent electrode layer of each sub-pixel are formed on the side of the microcavity pad layer of each sub-pixel away from the substrate, the undercut structure of each sub-pixel is formed. Optionally, the material of the microcavity pad layer with the fastest etching rate in each sub-pixel can be used to form a second material layer on the side of the microcavity pad layer of each sub-pixel away from the substrate, and then the material of the microcavity pad layer with the slowest etching rate in each sub-pixel can be used to form a first material layer on the side of the second material layer of each sub-pixel away from the substrate, and finally the first material layer and the second material layer of each sub-pixel are etched to form the undercut structure of each sub-pixel.
[0178] Exemplarily, if the material of the microcavity pad layer with the fastest etching rate in each of the above sub-pixels is SiNx, and the material of the microcavity pad layer with the slowest etching rate in each of the above sub-pixels is SiOx, then SiNx can be used to form a SiNx material layer on the side of the microcavity pad layer of each sub-pixel away from the substrate as the second material layer, and then SiOx can be used to form a SiOx material layer on the side of the second material layer of each sub-pixel away from the substrate as the first material layer. Then, the first material layer of each sub-pixel is opened by etching liquid, and the second material layer is further laterally hollowed out by etching liquid, thereby forming an undercut structure with a small top and a large bottom.
[0179] In one implementation, SiOx / SiNx / SiOx composite film coating can be performed, the glue is applied, exposed and developed, and the pixel definition layer in the middle of the pixel is opened by dry etching. Here, PDL etching can be performed in four steps. The first step is to open the PDL above the pixel. The second step is to enlarge the etched CD in the middle of the sub-pixel by lateral debonding. The third step is to use CF4 (carbon tetrafluoride) to open the uppermost SiOx layer according to the time mode. The fourth step is to use SF6 (sulfur hexafluoride) to perform lateral indentation. Because SF6 can open the SiOx / SiNx selection ratio>7, the undercut structure can be dug out. This step forms the LLC indentation structure to be footed. At this point, the pixel definition layer is formed. Fig.17 As shown, an embodiment of the present invention provides a schematic diagram of a display substrate forming process, which can form a pixel definition layer on a microcavity pad layer.
[0180] After forming the pixel definition layer, a light-emitting layer and a semi-transparent electrode layer of each sub-pixel can be formed on the side of the microcavity pad layer of each sub-pixel away from the substrate; wherein the reflective electrode layer and the semi-transparent electrode layer of each sub-pixel constitute a microcavity structure.
[0181] In the embodiment of the present invention, since the refractive index of the microcavity pad layer matched with each color light is such that the microcavity structure where the microcavity pad layer is located satisfies the constructive interference condition of the color light, it means that the microcavity structure of the sub-pixel can be made to satisfy the constructive interference condition of the corresponding color light by adjusting the refractive index of the microcavity pad layer. Therefore, compared with the method of only adjusting the thickness of the microcavity pad layer, the method of adjusting the refractive index of the microcavity pad layer can reduce the thickness difference of the microcavity pad layer in the microcavity structure of each sub-pixel of different wavelengths, thereby reducing the difference in light emitting efficiency of different sub-pixels, thereby improving the display balance of each sub-pixel.
[0182] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0183] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the method embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0184] The above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are included in the protection scope of the present invention.
Claims
1. A display substrate, It is characterized in that The display substrate comprises: substrate; A plurality of sub-pixels having a microcavity structure are located on the substrate; The materials of the microcavity pads in the microcavity structures of the sub-pixels are different, and the refractive index of the microcavity pads in the microcavity structures of the sub-pixels matches the color light corresponding to the sub-pixels; the refractive index of the microcavity pads matching each color light is such that the microcavity structure where the microcavity pads are located satisfies the constructive interference condition of the color light.
2. The display substrate according to claim 1, It is characterized in that The plurality of sub-pixels in the display substrate include: a first sub-pixel and a second sub-pixel; The material of the microcavity pad layer in the first sub-pixel is silicon oxide, and the material of the microcavity pad layer in the second sub-pixel is silicon nitride.
3. The display substrate according to claim 2, It is characterized in that The first sub-pixel is a blue sub-pixel, and the second sub-pixel is a green sub-pixel.
4. The display substrate according to claim 2, It is characterized in that Each sub-pixel also includes: An undercut structure is located on a side of the sub-pixel microcavity pad away from the substrate; The undercut structure of each sub-pixel includes a first material layer and a second material layer; the first material layer is located at a layer of the second material layer away from the substrate.
5. The display substrate according to claim 4, It is characterized in that The material of the first material layer in the undercut structure of each sub-pixel is the same as the material of the microcavity pad layer with the slowest etching rate in each sub-pixel; The material of the second material layer in the undercut structure of each sub-pixel is different from the material of the microcavity pad layer with the slowest etching rate in each sub-pixel.
6. The display substrate according to claim 4, It is characterized in that The material of the second material layer in the undercut structure of each sub-pixel is different from the material of the microcavity pad layer with the fastest etching rate in each sub-pixel; The material of the second material layer in the undercut structure of each sub-pixel is the same as the material of the microcavity pad layer with the fastest etching rate in each sub-pixel.
7. The display substrate according to claim 5 or 6, It is characterized in that The first material layer in each sub-pixel is formed later than the second material layer.
8. The display substrate according to claim 5, It is characterized in that The material of the first material layer is silicon oxide, and the material of the second material layer is silicon nitride.
9. The display substrate according to claim 8, It is characterized in that The display substrate further includes a peripheral area: The peripheral region includes a first silicon oxide layer, a first silicon nitride layer, a second silicon nitride layer, and a second silicon oxide layer stacked in sequence; Among them, the first silicon oxide layer is in the same layer as the microcavity pad layer in the first sub-pixel; the second silicon nitride layer is in the same layer as the microcavity pad layer in the second sub-pixel; the second silicon nitride layer is in the same layer as the second material layer, and the second silicon oxide layer is in the same layer as the first material layer.
10. The display substrate according to claim 4, It is characterized in that Each sub-pixel also includes: A reflective electrode layer, located between the substrate and the microcavity pad layer; A light-emitting layer and a semi-transparent electrode layer stacked in sequence on a side of the undercut structure away from the substrate; Wherein, the reflective electrode layer and the semi-transparent electrode layer form a microcavity structure.
11. The display substrate according to claim 10, It is characterized in that Each sub-pixel also includes: The reflective electrode protection layer is located between the reflective electrode layer and the microcavity pad layer.
12. The display substrate according to claim 1, It is characterized in that The microcavity pad layer of each sub-pixel includes a via hole; the via hole is used to electrically connect the structures on both sides of the microcavity pad layer.
13. The display substrate according to claim 12, It is characterized in that The via taper of the via hole in the microcavity pad layer of each sub-pixel is less than 45°.
14. The display substrate according to claim 1, It is characterized in that The refractive index of the microcavity cushion layer in the microcavity structure of each sub-pixel and the wavelength of the color light corresponding to the sub-pixel satisfy the following constraints: Among them, A is the optical path in the microcavity structure of the sub-pixel excluding the pixel pad layer, and is the same in the microcavity structures of each sub-pixel, n is the refractive index of the microcavity pad layer in the microcavity structure of the sub-pixel, d is the thickness of the microcavity pad layer in the microcavity structure of the sub-pixel, k is a positive integer, and λ is the wavelength of the color light corresponding to the sub-pixel.
15. The display substrate according to claim 10, It is characterized in that The thickness of the microcavity cushion layer in the microcavity structure of each sub-pixel is the same.
16. A display device, It is characterized in that Comprising a display substrate as described in any one of claims 1-15.
17. A method for preparing a display substrate, It is characterized in that The method comprises: providing a substrate; forming a plurality of sub-pixels having a microcavity structure on the substrate; The materials of the microcavity pads in the microcavity structures of the sub-pixels are different, and the refractive index of the microcavity pads in the microcavity structures of the sub-pixels matches the wavelength of the color light corresponding to the sub-pixels; the refractive index of the microcavity pads matching each color light is such that the microcavity structure where the microcavity pads are located satisfies the constructive interference condition of the color light.
18. The method according to claim 17, It is characterized in that The method of forming a plurality of sub-pixels having a microcavity structure on the substrate comprises: forming a reflective electrode layer of each sub-pixel on the substrate; On the side of the reflective electrode layer of each sub-pixel away from the substrate, using materials corresponding to each sub-pixel, the microcavity cushion layers of each sub-pixel are sequentially formed; the materials corresponding to each sub-pixel are different, and the refractive index of the material corresponding to each sub-pixel matches the color light of the sub-pixel; A light-emitting layer and a semi-transparent electrode layer of each sub-pixel are formed on the side of the microcavity pad layer of each sub-pixel away from the substrate; wherein the reflective electrode layer and the semi-transparent electrode layer of each sub-pixel constitute a microcavity structure.
19. The method according to claim 18, It is characterized in that The microcavity pads of each sub-pixel are sequentially formed by using materials matching the color light corresponding to each sub-pixel on the side of the reflective electrode layer of each sub-pixel away from the substrate, including: According to the order of etching rates of the materials corresponding to the sub-pixels from small to large, the microcavity pads of the sub-pixels are formed in sequence using the materials corresponding to the sub-pixels on the side of the reflective electrode layer of the sub-pixels away from the substrate.
20. The method according to claim 19, It is characterized in that The plurality of sub-pixels in the display substrate include: a first sub-pixel and a second sub-pixel; an etching rate of a material corresponding to the first sub-pixel is lower than an etching rate of a material corresponding to the second sub-pixel; The method comprises: forming a microcavity pad layer of each sub-pixel by using the materials corresponding to each sub-pixel in sequence of etching rates from small to large on the side of the reflective electrode layer of each sub-pixel away from the substrate, comprising: On a side of the reflective electrode of each sub-pixel away from the substrate, forming a first material film using a material corresponding to the first sub-pixel; Etching the first material film to form a microcavity pad layer of the first sub-pixel; On a side of the reflective electrode of each sub-pixel away from the substrate, forming a second material film using a material corresponding to the second sub-pixel; The second material film is etched to form a microcavity pad layer of the second sub-pixel.
21. The method according to claim 20, It is characterized in that The material corresponding to the first sub-pixel is silicon oxide, and the material corresponding to the second sub-pixel is silicon nitride.
22. The method according to claim 20, It is characterized in that A ratio of an etching rate of a material corresponding to the first sub-pixel to an etching rate of a material corresponding to the second sub-pixel is less than or equal to a preset ratio threshold.
23. The method according to claim 18, It is characterized in that After sequentially forming the microcavity pad layers of the subpixels on the side of the reflective electrode layer of each subpixel away from the substrate using materials corresponding to each subpixel, and before forming the light-emitting layer and the semi-transparent electrode layer of each subpixel on the side of the microcavity pad layer of each subpixel away from the substrate, the method further includes: Using the material of the microcavity pad layer with the fastest etching rate in each sub-pixel, a second material layer is formed on a side of the microcavity pad layer of each sub-pixel away from the base; Using the material of the microcavity pad layer with the slowest etching rate in each sub-pixel, a first material layer is formed on a side of the second material layer of each sub-pixel away from the base; The first material layer and the second material layer of each sub-pixel are etched to form an undercut structure of each sub-pixel.