High performance lamination adhesive with low free monomer

By using low content of aromatic-based isocyanate and polyol components in the binder, combined with specific solvent systems and additives, the problem of high isocyanate content in the prior art is solved, and under high temperature and chemical corrosion conditions are achieved Excellent bonding performance and safety.

CN119072396APending Publication Date: 2024-12-03ARKEMA FRANCE SA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202380035231.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-16
Filing Date
2023-05-15
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing solvent-based two-component adhesives exhibit high free monomer isocyanate content under high temperature and chemical corrosion conditions, which affects operating safety and food safety.

Method used

Using a low content of aromatic isocyanate and phosphate polyol and polyester polyol adhesive composition, the ratio of isocyanate reactive components and polyol components is controlled to form excellent adhesive properties and rapid curing. The binder and the combination of specific solvent systems and additives reduce the migration of aromatic amines.

Benefits of technology

Excellent bonding performance and rapid curing under high temperature and chemical corrosion conditions are achieved, while significantly reducing the risk of unwanted aromatic amines moving into food, meeting strict regulatory standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005093344750000041
    Figure BDA0005093344750000041
  • Figure BDA0005093344750000051
    Figure BDA0005093344750000051
  • Figure BDA0005093344750000052
    Figure BDA0005093344750000052
Patent Text Reader

Abstract

Disclosed is a solvent-based adhesive composition comprising: at least one isocyanate component comprising an aromatic-based isocyanate wherein the weight of free monomer isocyanate is less than 1% by weight, based on the weight of the isocyanate component, and wherein the weight of free monomer isocyanate is less than 1% by weight, based on the weight of the isocyanate component; and at least one isocyanate reactive component, the at least one isocyanate reactive component comprising at least one phosphate polyol. A process for manufacturing the adhesive and a laminate made in part from the adhesive and a process for manufacturing the laminate are also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to adhesive compositions. More particularly, the present disclosure relates to solvent-based two-component adhesive compositions for use with laminating films that exhibit excellent adhesive properties, heat and chemical resistance, and very low levels of migratory aromatic species. Background Art

[0002] Adhesive compositions can be used for a wide variety of purposes. For example, some adhesives are used to bond two or more film layers of a substrate together to form a composite film, i.e., a laminate comprising two or more film layers. Examples of substrates typically include polyethylene, polypropylene, polyester, polyamide, metal, paper or cellophane, etc. The use of adhesives in different lamination end-use applications is generally known. For example, adhesives are typically applied between laminated films and can be used to make film / film and film / foil laminates, which are used in food, drug and industrial consumer product packaging, especially in the flexible packaging industry for food packaging. Laminating adhesives can generally be divided into three categories: (1) solvent-based laminating adhesives, (2) solvent-free laminating adhesives, and (3) water-based laminating adhesives. The performance of adhesives varies according to the type and application of the adhesive. In the category of solvent-based laminating adhesives, solvent-based polyurethanes are widely used to achieve relatively good heat resistance, moisture resistance and chemical resistance.

[0003] In the category of solvent-based laminating adhesives, there are many types; and a specific type includes polyurethane-based multi-component laminating adhesives; and more specifically two-component adhesives. Typically, polyurethane-based two-component laminating adhesives include: a first component comprising isocyanate and / or polyurethane prepolymer and a second component comprising one or more polyols. The polyurethane prepolymer can be obtained by reacting polyisocyanate with polyether polyol and / or polyester polyol. The second component includes polyether polyol and / or polyester polyol. Each component may optionally include one or more additives. Common solvents for such systems include methyl ethyl ketone, ethyl acetate, toluene, etc., all of which must be anhydrous (moisture-free) to prevent premature reaction of the isocyanate groups of the polyurethane.

[0004] Two components of adhesive composition (i.e. isocyanate and polyol component) are mixed in a predetermined ratio to form adhesive composition. Then the adhesive composition carried by solvent is applied to film / or foil substrate. Evaporate solvent from the adhesive composition applied. Then another film / or foil substrate is contacted with other substrates to form a curable laminated structure. Solidify the laminated structure so that two substrates are bonded together.

[0005] Solvent-based adhesive compositions can be used for high performance lamination applications (e.g. hot fill, boil in bag, freezer conditions, etc.). Known adhesives are usually based on aromatic isocyanates, which exhibit excellent adhesion and fast curing characteristics. However, the free monomeric isocyanate in the isocyanate component is usually high, and its content is usually more than 10% by weight, which may affect handling safety and food safety. Therefore, there is a need for a high performance solvent-based adhesive with excellent adhesion performance, fast curing and meeting strict regulatory standards. DETAILED DESCRIPTION

[0006] Numerical ranges disclosed herein include all values ​​from the lower limit to the upper limit, and include the lower limit and the upper limit. For ranges containing exact values ​​(e.g., ranges from 1 or 2 or 3 to 5 or 6 or 7), any sub-ranges between any two exact values ​​are included (e.g., the above ranges 1 to 7 include sub-ranges of 1 to 2; 2 to 6; 5 to 7; 3 to 7; 5 to 6, etc.).

[0007] The term "composition" refers to a mixture of materials comprising the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0008] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not they are specifically disclosed. For the avoidance of any doubt, unless stated to the contrary, all compositions claimed by using the term "comprising" may include any additional additives, adjuvants or compounds, whether in polymeric form or otherwise. In contrast, the term "consisting essentially of excludes any other components, steps or procedures (except those that are not essential to operability) from the scope of any subsequent statements. The term "consisting of" excludes any components, steps or procedures that are not specifically described or listed. Unless otherwise stated, the term "or" refers to the listed members individually and in any combination. The use of the singular includes the use of the plural, and vice versa.

[0009] An "isocyanate" is a chemical substance that contains at least one isocyanate group in its structure. An isocyanate group is represented by the formula: -N=C=O or abbreviated as "NCO". An isocyanate containing more than one or at least two isocyanate groups is a "polyisocyanate". An isocyanate with two isocyanate groups is a diisocyanate, and an isocyanate with three isocyanate groups is a triisocyanate, etc.

[0010] A "polyisocyanate" is a molecule containing at least two isocyanate groups.

[0011] "Polyethers" are chemical compounds containing two or more ether linkages in the same linear chain of atoms.

[0012] A "polyester" is a chemical compound containing two or more ester bonds in the same linear chain of atoms.

[0013] A "polyol" is an organic compound containing multiple hydroxyl (OH) groups. In other words, a polyol contains at least two OH groups. Non-limiting examples of suitable polyols include diols having two OH groups, triols having three OH groups, and tetraols having four OH groups.

[0014] "Polyester polyol" is a compound containing polyester and polyol in the main chain structure of the compound.

[0015] "Polyether polyol" is a compound containing polyether and polyol in the main chain structure of the compound.

[0016] Unless thickness is expressly specified, "film" (including when referring to a "film layer" in a thicker article) includes any thin, flat extruded or cast thermoplastic article having a generally consistent and uniform thickness in one dimension of about 0.5 millimeters (mm) (20 mils) or less.

[0017] A "polymer film" is a film made of a polymer or a polymer mixture. The composition of a polymer film is usually 80 weight percent (wt%) of one or more polymers.

[0018] "Polymer" is a polymeric compound prepared by polymerizing monomers (whether of the same type or different types). Therefore, the general term "polymer" encompasses the term homopolymer (used to refer to polymers prepared from only one type of monomer, where it should be understood that trace impurities can be incorporated into the polymer structure) and the term "interpolymer", which includes copolymers (used to refer to polymers prepared from two or more different types of monomers), terpolymers (used to refer to polymers prepared from three different types of monomers) and polymers prepared from more than three different types of monomers. Trace impurities (e.g., catalyst residues) can be incorporated into and / or within the polymer. It also encompasses all forms of copolymers, such as random, block, etc. It should be noted that although polymers are often referred to as "made of" one or more specified monomers, "based on" a specified monomer or monomer type, "containing" a specified monomer content, etc., in this context, the term "monomer" should be understood to refer to the polymerized residue of the specified monomer rather than unpolymerized substances. In general, polymers are referred to herein as "units" based on the polymerized form of the corresponding monomer.

[0019] A solvent-based adhesive is disclosed, the adhesive comprising at least one isocyanate component and at least one isocyanate-reactive component. The isocyanate component contains less than 1% by weight of an aromatic-based isocyanate based on the weight of the isocyanate component. The isocyanate-reactive component comprises at least one phosphate polyol and at least one polyester polyol. A method for producing a laminated product using the above-mentioned adhesive is also disclosed.

[0020] The aromatic-based isocyanate in the isocyanate component can be, for example, isocyanate monomers, polyisocyanates (eg, dimers, trimers, etc.), isocyanate prepolymers, and mixtures of two or more of the foregoing."Polyisocyanate" is any compound containing two or more isocyanate groups.

[0021] Aromatic-based isocyanates useful in the present disclosure may include, for example, one or more polyisocyanate compounds, including, but not limited to, for example, 1,3- and 1,4-phenylene diisocyanates; 1,5-naphthylene diisocyanate; 2,4'-diphenylmethane diisocyanate (2,4'-MDI); 4,4'-diphenylmethane diisocyanate (4,4'-MDI); 3,3'-dimethyl-4,4'-biphenyl diisocyanate (TODI) and isomers thereof; polymeric isocyanates; and mixtures of two or more thereof.

[0022] Examples of some of the commercially available aromatic-based components that can be used in the present disclosure may include, for example, ISONATE TM 125M, ADCOTTE TM L76-204, COREACTANT CT TM , available from Dow Chemical; DESMODUR TM E2200 / 76, available from Covestro; and mixtures thereof.

[0023] The phosphate ester in the isocyanate reactive component can be selected, for example, from phosphate ester compounds having the following chemical structure:

[0024]

[0025] Where R 1 is any organic group. In addition to the side groups shown in structure (I), R 1 may or may not have one or more additional -OH side groups, and R 1 It may or may not have one or more additional side groups of structure (I). Any two or more of the -OH group and the group of structure (I) may or may not be connected to R 1Each -OH group and each group of structure (I) may be connected to R 1 on individual atoms.

[0026] Characterization R 1 A convenient way to describe is to describe a compound having the following structure (II):

[0027]

[0028] Where R 1 Same as in structure (I). The compound having structure (II) is referred to herein as a "precursor polyol".

[0029] Suitable precursor polyols may have a number average Mw of 90 g / mol or more, 200 g / mol or more, or 400 g / mol or more. Suitable precursor polyols may have a number average Mw of 4,000 g / mol or less, 2,000 g / mol or less, 1,200 g / mol or less, 900 g / mol or less, or 500 g / mol or less. Suitable precursor polyols may have a number average Mw of 200 g / mol to 4,000 g / mole, 400 g / mol to 2,000 g / mol, 400 g / mol to 1,200 g / mol, or 400 g / mol to 900 g / mol.

[0030] Suitable precursor polyols may be alkyl higher polyols, monosaccharides, disaccharides and compounds having the following structure (III):

[0031]

[0032] Where R 2 , R 3 , R 4 and R 5 Each of n is independently any other organic group; 1 、n 2 and n 3 Each independently represents an integer from 0 to 10. In addition to the side groups shown in structure (III), R 2 It should also be understood that any two or more side groups may or may not be connected to R. 2 In some embodiments, there is a mixture of compounds having structure (III), wherein the compounds of structure (III) have 1 、n 2 and n 3 Such mixtures are described herein by stating the parameter n 1 、n2 or 3 The molecular weight of a mixture is described by a non-integer value, where the non-integer value represents the number average of that parameter. When the molecular weight of such a mixture needs to be estimated, the number average molecular weight is used.

[0033] In the precursor polyol having structure (III), each pendant group may be attached to R 2 In the precursor polyol having structure (III), R 3 , R 4 and R 5 It may be a hydrocarbon group having 1 C to 4 C, 2 C to 3 C or 3 C. In the precursor polyol having structure (III), R 3 , R 4 and R 5 One or more of R may be an alkyl group, which may be linear, cyclic, branched, or a combination thereof; 3 , R 4 or R 5 One or more of may be a straight chain or branched chain alkyl group; and R 3 , R 4 and R 5 One or more of R may be a branched alkyl group. 3 , R 4 or R 5 Can be the same as each other.

[0034] In the precursor polyol having structure (III), n 1 、n 2 and n 3 One or more of may be 0 to 8. In the precursor polyol having structure (III), n 1 、n 2 and n 3 One or more of may be 1 or greater. In the precursor polyol having structure (III), n 1 、n 2 and n 3 One or more of may be 6 or less. In the precursor polyol having structure (III), n 1 、n 2 and n 3 Can be the same.

[0035] The precursor polyol group having structure (III) may be one in which R 2 , R 3 , R 4 and R 5 Each of which is an alkyl group; such precursor polyols are referred to herein as alkoxylated alkyl triols. In the triol, when n 1 、n2 and n 3 At least one of is 1 or greater and R 2 When having the following structure (IV):

[0036]

[0037] The triol is referred to herein as alkoxylated glycerol. In the alkoxylated triol, when R 3 , R 4 and R 5 When each of R is a branched alkyl group having exactly 3 C, the alkoxylated triol is referred to herein as a propoxylated triol. 2 The propoxylated triols having structure (IV) are referred to herein as propoxylated glycerols.

[0038] The precursor polyol as the alkyl higher polyol may be a compound having 10 C or less carbon atoms; a compound having 6 C or less carbon atoms; a compound having 3 C or less carbon atoms; or glycerol.

[0039] The precursor polyol can be an alkyl higher polyol and a compound having structure (III). It should be noted that if n 1 Equal to (=) n 2 =n 3 = 0 and if R 2 is an alkyl group or an alkyl group having a hydroxyl group, then the compound having the structure (IV) is an alkyl higher polyol.

[0040] The precursor polyol group can be alkyl triols and alkoxylated alkyl triols. These compounds are glycerol and alkoxylated glycerol. Alkoxylated glycerol is propoxylated glycerol.

[0041] Another suitable phosphate compound that can be used in the present disclosure includes compounds containing carbamate bonds. The phosphate compound containing carbamate bonds is prepared by reacting one or more suitable phosphate functional polyols with one or more polyisocyanates, and one or more diisocyanates may also be included. The amount of polyisocyanate can be kept low enough so that some or all of the reaction products are phosphate functional polyols. Alternatively, the polyol may first react with the polyisocyanate to prepare an -OH terminated prepolymer, which is then reacted with polyphosphoric acid. Phosphate compounds with carbamate bonds include those compounds with a number average Mw in the range of 1,000 g / mol to 6,000 g / mol, in the range of 1,200 g / mol to 4,000 g / mol, and in the range of 1,400 g / mol to 3,000 g / mol.

[0042] The phosphate ester compound may be a reaction product of reactants including a precursor polyol and a phosphoric acid-type acid, wherein the resulting phosphate ester compound has a chemical structure of structure (I).

[0043] The amounts of phosphoric acid and precursor polyol are selected to determine the following M p ∶M x Ratio: M hy = the number of hydroxyl groups per molecule of the precursor polyol; N x =M hy -2;M x =(number of moles of precursor polyol) x (N x ); and M p =The number of moles of phosphorus atoms contained in phosphoric acid.

[0044] Usually, M p :M x The ratio is 0.1:1 or higher, 0.2:1 or higher, 0.5:1 or higher, or 0.75:1 or higher. p :M x The ratio may be 1.1:1 or lower.

[0045] Typically, the weight ratio of phosphoric acid to precursor polyol is 0.005:1 or higher, 0.01:1 or higher, or 0.02:1 or higher. The weight ratio of phosphoric acid to precursor polyol can be 0.3:1 or lower, or 0.2:1 or lower, or 0.12:1 or lower.

[0046] Phosphoric acid may contain polyphosphoric acid. And typically, the amount of polyphosphoric acid in the phosphoric acid is 75% by weight or more, 80% by weight or more, or 90% by weight or more, by weight, based on the weight of the phosphoric acid. Polyphosphoric acid is available in various grades; each grade is characterized by a percentage. To determine the grade, it is first recognized that pure monomeric orthophosphoric acid, the content of phosphorus pentoxide is considered to be 72.4%. Any grade of polyphosphoric acid can also be analyzed, considering that one mole of polyphosphoric acid (the formula weight is marked as "Fppa") contains the number of moles of phosphorus pentoxide marked as "Nppo", and the percentage of phosphorus pentoxide ("PCppo") is given by PCppo = (Nppo × 142) / Fppa, expressed as a percentage. Then, the grade of the polyphosphoric acid is a ratio, expressed as a percentage: grade = PCppo / 72.4.

[0047] The polyphosphoric acid used may have a grade of 100% or more, or 110% or more.The polyphosphoric acid used may have a grade of 150% or less, or 125% or less.

[0048] Further information regarding suitable phosphate esters and the preparation of such suitable phosphate esters can be found, for example, in PCT Publication No. WO / 2015 / 168670.

[0049] The amount of phosphate polyol used in the isocyanate reactive component can be 0.1 wt % to 1 wt %, 1 wt % to 5 wt %, 5 wt % to 10 wt %, 10 wt % to 15 wt %, or 15 wt % to 20 wt %, based on the dry weight of the isocyanate reactive component.

[0050] In addition to one or more phosphate functional polyols, the disclosed solvent-based adhesive composition also contains one or more phosphorus-free polyols. The isocyanate reactive component may include one or more polyester polyols. The polyester polyol may have a molecular weight of >2000 g / mol.

[0051] Suitable polyester polyols that can be used in the present disclosure include, but are not limited to, for example, aliphatic polyester polyols; aromatic polyester polyols; copolymers of aliphatic and aromatic polyester polyols; polycarbonate polyols; polycaprolactone polyols; and mixtures thereof. These polyester polyols are: the reaction product of a polyacid and a polyol; or the reactant of a phosgene or carbonate monomer and a polyol; or are produced via the ring-opening polymerization of a cyclic ester compound.

[0052] Examples of suitable polyacids that can be used in the present disclosure include succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, maleic anhydride, fumaric acid, 1,3-cyclopentane-dicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid and anhydrides or ester derivatives of these dicarboxylic acids; and p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid and ester derivatives or dimer acids of these dihydroxycarboxylic acids; and mixtures thereof. These polyacids can be used alone or in combination of two or more polyacids.

[0053] According to the present disclosure, any known polyol can be used. Non-limiting examples of suitable polyols that can be used in the present disclosure include: glycols such as ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, methylpentanediol, dimethylbutanediol, butylethylpropylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, bishydroxyethoxybenzene, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, triethylene glycol, polycaprolactone diol, dimer glycol, bisphenol A and hydrogenated bisphenol A; Polyesters produced by ring-opening polymerization of ethylene oxide, propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, tetrahydrofuran and cyclohexene; and polyethers produced by addition polymerization in a usual manner with the aid of one or more compounds containing two active hydrogen atoms as initiators, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol and neopentyl glycol; and mixtures thereof. These polyols may be used alone or in combination of two or more polyols.

[0054] The amount of polyester polyol used in the isocyanate reactive component may be greater than 10 wt %, greater than 20 wt %, greater than 30 wt %, greater than 40 wt %, greater than 50 wt %, greater than 60 wt %, or greater than 70 wt %, based on the dry weight of the polyol component.

[0055] In addition, the polyol component may include a polyether polyol. Suitable polyether polyols include, but are not limited to, polypropylene glycol, polytetramethylene ether glycol, polyoxybutylene polyols, or mixtures and copolymers thereof. Suitable polypropylene glycols include polyols based on propylene oxide, ethylene oxide, or mixtures thereof with an initiator selected from propylene glycol, dipropylene glycol, sorbitol, sucrose, glycerol, and / or mixtures thereof, available from Dow Chemical under the trade name VORANOL TM BASF uses the trade name PLURACOL TM , Lonza under the trade name POLY-G TM POLY-L TM and POLY-Q TM and Covestro under the trade name ACCLAIM TM In particular, preferred are polypropylene glycols having a functionality between 2 and 6 and a molecular weight between 250 and 1500. Suitable polytetramethylene ether glycols include, but are not limited to, POLYTHF TM, TERTHANE from Invista TM , PTMG from Mitsubishi TM and PTG from Dairen TM Suitable polyoxybutylene-based polyols include, but are not limited to, polybutylene oxide homopolymer polyols, polybutylene oxide-polypropylene oxide copolymer polyols, and polybutylene oxide-polyethylene oxide copolymer polyols.

[0056] Additionally, low molecular weight glycols including, but not limited to, ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, trimethylolpropane, triisopropanolamine, and neopentyl glycol may be incorporated into the polyol compound.

[0057] The adhesive composition of the present disclosure generally includes at least one solvent. Suitable solvents may include, but are not limited to, ethyl acetate, propyl acetate, methyl ether ketone, methyl butyl ketone, acetone, toluene, and mixtures thereof.

[0058] The amount of solvent used in the disclosed method may be, for example, 20 to 90 wt %, 30 to 80 wt %, or 40 to 70 wt %, based on the total amount of components in the adhesive composition.

[0059] The adhesive compositions of the present disclosure may include one or more additional optional conventional ingredients or additives, including, but not limited to, catalysts, tackifiers, tackifiers, antioxidants, fillers, colorants, pigments, surfactants, solvents, polymers (including, for example, thermoplastic resins other than those discussed herein above), dehydrating agents (including, for example, silanes), benzoyl chloride, other polyols (including, for example, aliphatic polyols), ultraviolet indicators, and combinations of two or more of these.

[0060] The adhesive composition may include, for example, an adhesion promoter. Non-limiting examples of suitable adhesion promoters include coupling agents such as silane coupling agents, titanate coupling agents, and aluminate coupling agents; epoxy resins, phosphoric acid, polyphosphoric acid, and phosphoric acid esters.

[0061] Examples of silane coupling agents that can be used in the present disclosure include, but are not limited to, aminosilanes such as γ-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethyldimethoxysilane, and N-phenyl-γ-aminopropyltrimethoxysilane; epoxysilanes such as β-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane, γ-glycidoxypropyl-trimethoxysilane, and γ-glycidoxypropyltriethoxysilane; vinylsilanes such as vinyltri(β-methoxyethoxy)silane, vinyltriethoxysilane, vinyltrimethoxysilane, and γ-methacryloxypropyltrimethoxysilane; hexamethyldisilazane; γ-mercaptopropyltrimethoxysilane; and mixtures thereof.

[0062] Examples of titanate coupling agents useful in the present disclosure include, but are not limited to, tetraisopropoxytitanium, tetra-n-butoxytitanium, butyl titanate dimer, tetrastearyl titanate, titanium acetylacetonate, titanium lactate, tetraoctyl titanate, titanium lactate, tetrastearyl titanium; and mixtures thereof.

[0063] Examples of epoxy resins that can be used in the present disclosure include, but are not limited to, various readily available epoxy resins, such as bisphenol a-epichlorohydrin (epi-bis) type epoxy resins, novolac type epoxy resins, β-methyl epichlorohydrin type epoxy resins, cyclic oxirane type epoxy resins, glycidyl ether type epoxy resins, glycidyl ester type epoxy resins, polyethylene glycol ether type epoxy resins, glycol ether type epoxy resins, epoxidized fatty acid ester type epoxy resins, polycarboxylate type epoxy resins, aminoglycidyl type epoxy resins, resorcinol type epoxy resins; and mixtures thereof.

[0064] The adhesion promoter may be a phosphoric acid ester compound or epoxy silane ((3-glycidoxypropyl)-trimethoxysilane). Phosphoric acid may be incorporated into the polyol component, while epoxy silane may be incorporated into the isocyanate component. Both epoxy silane and phosphoric acid may be incorporated into the polyol component.

[0065] The average functionality of the adhesive composition (ie, the isocyanate component and the polyol component), excluding non-reactive components (such as solvents) may be from 2 to 3.

[0066] The amount of the optional components, when used, may be 0 wt % to 15 wt %, 0.01 wt % to 10 wt %, or 0.1 wt % to 5 wt %, based on the total amount of components in the adhesive composition.

[0067] It is contemplated that two components, an isocyanate component and a polyol component, are used in the present disclosure. It is also contemplated that the isocyanate component and the polyol component of the disclosed adhesive composition can be prepared separately and, if necessary, stored until the adhesive composition is desired to be used. The method for producing the adhesive composition includes mixing the above-mentioned isocyanate and polyol components to form an adhesive composition that can be cured. In some embodiments, the isocyanate component and the polyol component are each liquid at 25° C. When the adhesive composition is desired to be used, the isocyanate component and the polyol component are generally contacted with each other and mixed together in a stoichiometric ratio (NCO / OH) of 1 to 2.5. It is expected that when the two components are contacted, a curing reaction begins, wherein the isocyanate groups react with the hydroxyl groups to form urethane segments. The adhesive composition formed by contacting the two components can be referred to as a "curable mixture".

[0068] In order to form the adhesive composition, the mixing of two components can be carried out at any suitable time in the process of forming the adhesive composition and applying the adhesive to the substrate, such as before the application process, during or as the result of the application process.All steps in the step of the present invention can be performed under ambient room temperature.As required, heating or cooling can be adopted.Suitable conventional mixer (such as using electric, pneumatic or other power mechanical mixer) can be used to mix.

[0069] The method for preparing the solvent-based adhesive composition of the present disclosure includes, for example, the following steps:

[0070] (1) providing an isocyanate component; (2) providing a polyol component; (3) mixing the two components to form a resin mixture; (4) diluting the resin mixture in a solvent to form a diluted resin mixture having an applied solids content of 25 wt % to 55 wt %, 30 wt % to 45 wt %, or 35 wt % to 40 wt %, based on the total weight of the diluted resin mixture; and (5) removing the solvent from the composition after applying the composition to a substrate and before curing the composition to form an adhesive composition.

[0071] Some of the advantageous properties exhibited by the solvent-based adhesive compositions of the present disclosure include, for example, (1) good adhesive properties; (2) fast curing; and (3) low levels of unwanted aromatic amines (such as MDA and TDA) that migrate into food products packaged using the adhesive.

[0072] For example, the adhesive may have a bond greater than 2 N / 15 mm after heat testing for 1 hour at 100° C. and above. The bond may depend on the type of film substrate used, and in some embodiments, the film may bond where the substrate failure mode after testing occurs prior to bonding.

[0073] The curing time of the adhesive may be 1 day to 8 days, 1 day to 7 days, or 2 days to 7 days.

[0074] Also disclosed herein is a method of forming a laminate using an adhesive composition of the present disclosure. The adhesive composition (such as the adhesive composition discussed above) can be liquid at 25°C. Even if the composition is solid at 25°C, the composition can be heated as needed to convert the composition to a liquid state. A solvent is added to the mixed adhesive composition until the desired solid content is reached. A solid content of 25% or more can be used.

[0075] Adhesive compositions of the present disclosure can be used to bond substrates together; and the adhesive compositions can be used on various single suitable substrates or multiple suitable substrates. The substrate can be a similar material or a dissimilar material. For example, the substrate can be selected from high, low or medium density plastics (e.g., selected from polystyrene, polyethylene, ABS, polyurethane, polyethylene terephthalate, polybutylene terephthalate, polypropylene, polyphenylene, polycarbonate, polyvinyl chloride, polysulfone and their mixtures), paper, wood and reconstituted wood products, polymer-coated substrates, waxed paperboard, paperboard, particleboard, textiles, leather and metals (e.g., aluminum, iron and other non-ferrous materials), metallized plastics (e.g., metallized plastic films), etc.

[0076] The wet bonding lamination and dry bonding lamination of a plurality of substrate layers are possible.Can use conventional application technology that adhesive composition is applied on the required substrate, this conventional application technology such as rotogravure printing, flexographic printing, conventional or airless spraying, roller coating, brush coating, wire rod coating, scraping coating or coating process, for example curtain coating, overflow, bell coating, disc coating and dip coating process.Can carry out on the whole surface of substrate with adhesive composition coating substrate, perhaps such as along the edge, or be coated on the part of substrate surface in the discontinuous position.In case be applied on the substrate, adhesive composition just such as by applying heat and airflow or some other suitable conventional methods dry, to remove all residual solvents existing in the adhesive composition basically.

[0077] The laminate comprising the solvent-based adhesive composition of the present disclosure can be formed by applying an adhesive to at least one of two different substrates, and combining the substrates together so that the adhesive is disposed between the surfaces of the two substrates; and then curing the adhesive to form a bond between the two substrates. The substrate may include, for example, two separate films; and each of the films may be made of different materials or the same material. Typically, an adhesive composition layer is applied to the surface of the film. The thickness of the adhesive composition mixture layer that can be cured applied to the film surface is 1 micron (μm) to 5 μm. As used herein, a "film" is any structure that is 0.5 mm or less in one dimension of the structure; and is 1 centimeter (cm) or greater in the other two dimensions of the structure.

[0078] The surface of another film is contacted with the layer of the mixture capable of curing to form an uncured laminate. The curable mixture is then cured or solidified. The uncured laminate may be subjected to pressure, such as by passing through a roller, which may or may not be heated. The uncured laminate may be heated to accelerate the curing reaction.

[0079] Suitable substrates for forming laminated structures include films, such as paper, woven fabrics and nonwoven fabrics, polymer films, metal foils, metal coating (metallized) polymer films and their combinations. Substrates are stacked to form laminated structures, wherein one or more substrates in these substrates are adhered together according to the adhesive composition of the present disclosure. Film optionally can have a surface with an ink-printed image. Ink can contact with the adhesive composition. The film can be a polymer film, a metal-coated polymer film or a polymer film. "Polymer film" is a film made of a polymer or a polymer mixture. The composition of the polymer film is typically 80 weight % or more of one or more polymers.

[0080] The adhesive composition is particularly useful for packaging and sealing applications. For example, a plastic film, a metal film, or a metallized plastic film can be laminated with the adhesive composition of the present disclosure (e.g., over its entire surface or at least a portion of its surface, such as along its edge or at intermittent locations) to form a laminate. The laminate can be used to form a pouch made from at least two layers of film, wherein the adhesive is bonded between the two layers of film. Food can be packaged for boil-in-bag preparations, or the resulting laminate can be used to seal or package some other article.

[0081] Example

[0082] The following examples are provided to further illustrate the present disclosure in detail but should not be construed as limiting the scope of the claims. Unless stated to the contrary, implied by the context, or customary in the art, all parts and percentages are by weight, and all test methods are current as of the filing date of this disclosure.

[0083] The various raw materials or raw materials used in the examples of the present invention (Inv.Ex.) and comparative examples (Comp.Ex.) are explained in Table 1 as follows:

[0084] Table 1 - Raw materials

[0085]

[0086]

[0087] Table 2 Adhesive preparation (parts)

[0088]

[0089] Preparation of prepolymer 1 - isocyanate component

[0090] 673g ISONATE TM 125M MDI was melted in a 40°C oven and added to 2 1327 g of VORANOL PUP 2025 polyol was preheated to 50°C and added with ISONATE TM 125M MDI. When all exothermic phenomena are complete, the mixture is stirred continuously and then heated to 80°C to 85°C while continuing to stir. The mixture is then stirred continuously for 1.5 hours while the temperature is maintained at 80°C. The residual NCO% is checked via titration until the measured value is 8.4, close to the theoretical value of 8.5. The solution is then cooled to 40°C to 50°C and transferred to a metal can. The can is filled with nitrogen to prevent reaction with moisture and stored in a refrigerator until distillation.

[0091] The evaporator temperature, condenser temperature, pressure, feed rate and wiper speed of the laboratory scale UIC KDL 5 distillation equipment were set to 175°C, 45°C, 0.04mbar, 0.6kg / hour to 1.2kg / hour and 360U / minute, respectively. In the laboratory, a single pass was used, but when scaled up, two or more passes may be required. The NCO% of the final prepolymer should be 2.82, the viscosity should be 15560mPas, and the residual free MDI monomer should be 0.1%.

[0092] Residual MDI is reported as weight % based on the weight of the prepolymer.Viscosity is measured at 25°C with a Model DVIII Brookfield Viscometer according to ASTM method D2196 using spindle 4 and 20 rpm.

[0093] General preparation of phosphate ester compounds

[0094] A 1 liter (L) multi-necked round-bottom flask was dried in an oven with dry nitrogen (N 2 ) for 30 minutes, then add 150 g of VORANOL TM CP 450 polyether polyol was placed in 70 mL / min N 2 Purge. Load the syringe with 4 g of 115% polyphosphoric acid 20 acid (PPA). Add PPA dropwise to the polyether polyol under vigorous stirring. Minimal temperature rise should be observed. Heat the reactor contents to 100°C for 1 hour and then cool to 45°C. Then, add 40 g of ethyl acetate to the reactor, followed by the slow addition of 50 g of ISONATE TM 125M diisocyanate. The significant exotherm is controlled by the use of an ice bath to maintain the reaction pot below 75°C, and the development of a yellow to amber color should be observed. The reactor is then held at 65°C for 1 hour, at which time the contents are cooled and packaged. The product should have the following properties: 76.0% solids, a hydroxyl number (OHN) of 112 mg KOH / g, an acid value (AV) of 19.0 mg KOH / g, and a viscosity of 1,665 millipascal-seconds (mPa·s) at 25°C.

[0095] General Procedure for Preparing Isocyanate-Reactive Components

[0096] The polyester polyol and the phosphate polyol were charged into a glass reactor. The reactor was heated to about 40° C., and the resulting mixture was stirred at 40° C. for about 30 minutes. The resulting mixture was then packaged and stored.

[0097] General Procedure for Preparing Adhesive Formulations

[0098] The relevant ingredients used to prepare the adhesive formulation containing the isocyanate-reactive component, the isocyanate component and the solvent are described in Table 2.

[0099] Using the adhesive of Example 1 of the present invention as a typical example for the preparation of adhesive formulation samples, about 750 g of an isocyanate reactive component (component A), about 420 g of an isocyanate component (component B) and about 1,725 ​​g of ethyl acetate were loaded into a plastic container. The materials were mixed for 30 minutes using a mechanical mixer at room temperature (about 25° C.) to obtain the formulated adhesive of the present invention example.

[0100] General procedure for preparing laminates

[0101] Via Nordmeccania LABO COMBI TMThe 400 pilot coater produced laminates based on solvent-based adhesives at room temperature (about 25°C) at a nip temperature of 180°F and a two-minute drying temperature of 176°F. The polymer film was corona treated before lamination, and aluminum (Al) foil that was not corona treated was used. The coating weight of each laminate was maintained at about 2.5 pounds per ream. The prepared laminates were then cured in a controlled environment (e.g., at 25°C and 50% relative humidity).

[0102] The examples were prepared using films including "Prelam", which is a 12 μm (48 gauge) polyester ("PET") film at 3.26 g / m 2 (2.00 lbs / ream) laminated to ADCOTE TM / Coreactant F, commercially available from The Dow Chemical, and includes a cast polypropylene ("CPP") film having a thickness of 65 μm. GF-19, a 1.5 mil thick polyethylene sealing film containing a large amount of slip additive, is commercially available from Berry Plastics.

[0103] Bond strength measurement

[0104] The laminated samples were cut into 15 mm wide strips and loaded on a THWING ALBERT equipped with a 50 N load cell. TM The films were pulled at 4 inches / minute on a QC-3A peel tester. When the two films in the laminate separated, the average of the forces during the pull was recorded. If one of the films was strained or broke, the maximum force or breaking force was recorded. These values ​​are the average of three separate sample strips. After the laminate was made, the initial or green bond was tested as soon as possible. Additional T-peel tests were performed at the time intervals indicated below.

[0105] General procedure for preparing sachets

[0106] Performance Testing

[0107] In-bag boiling test procedure

[0108] The laminates were made of Prelam Al and GF-19. One of the 9" x 12" (23 cm x 30.5 cm) sheets of the laminate was folded over to obtain a double layer of approximately 9" x 6" (23 cm x 15.25 cm) so that the PE film of one layer was in contact with the PE film of the other layer. The edges were trimmed on a paper cutter to obtain a folded sheet of approximately 5" x 7" (12.7 cm x 17.8 cm). The two long sides and one short side were heat sealed at the edges to obtain a finished pouch with an inner dimension of 4" x 6" (10.2 cm x 15.2 cm). The heat seal was performed at 177°C (350°F) and a hydraulic pressure of 276 kPa (40 PSI) for 1 second. Two or three pouches were prepared for each test.

[0109] Fill the pouch with 100 ± 5 ml of 1:1:1 sauce (a blend of equal parts by weight of ketchup, vinegar, and vegetable oil) through the edge of the opening. Avoid splashing the filler onto the heat seal area as this will cause the heat seal to fail during the test. After filling, seal the top of the pouch in a manner that minimizes air entrapment within the pouch.

[0110] The seal integrity was tested on all four sides of the pouch to ensure that there were no defects in the seal that could cause the pouch to leak during testing. Any suspect pouches were discarded and replaced. In some cases, defects in the laminate were marked to identify if new additional defects were created during testing.

[0111] Fill a pot 2 / 3 full of water and bring to a boil. The boiling water pot has a lid to reduce the loss of water and steam. Observe the pot during the test to ensure that there is enough water to keep boiling. Place the pouch in boiling water and keep it for 30 minutes. Take out the pouch and compare the degree of tunneling, bubbling, delamination or leakage with any marked pre-existing defects. Record the observations. Cut the pouch open, empty it, and rinse it with soap and water. Cut one or more 15mm strips from the pouch and measure the laminate bond strength at 4 inches / minute according to the standard bond strength test described previously. This process is completed as soon as possible after taking out the pouch contents. Inspect the interior of the bag and record any other visual defects.

[0112] 121℃ Test Procedure

[0113] The laminates were made from Prelam / / CPP as described above. One of the 9 inch by 12 inch (23 cm by 30.5 cm) sheets of the laminate was folded over to obtain a double layer of approximately 9 inches by 6 inches (23 cm by 15.3 cm) so that the CPP film of one layer was in contact with the CPP film of the other layer. The edges of the folded laminate were trimmed on a paper cutter to obtain a folded sheet of approximately 5 inches by 7 inches (12.7 cm by 17.8 cm). The two long sides and one short side of the folded sheet were heat sealed at the edges to obtain a finished pouch having an inside dimension of 4 inches by 6 inches (10.2 cm by 15.2 cm). Heat sealing was performed at 400°F (204°C) for 1 second under a hydraulic pressure of 40 pounds per square inch (psi) (276 kilopascals [kPa]). Two or three pouches were prepared for each test.

[0114] The pouches prepared as described above were filled through the edge of the opening with 100 milliliters (mL) ± 5 mL of distilled water (DI water) or 1:1:1 sauce (a blend of equal weight parts of ketchup, vinegar, and vegetable oil). Splashing the filler into the heat seal area should be avoided because this will cause the heat seal to fail during the test. After filling, the top of the pouch is sealed in a manner that minimizes air entrapment within the pouch. The seal integrity is tested on all four sides of the pouch to ensure that there are no defects in the seal that can cause the pouch to leak during the test. Any defective pouches are discarded and replaced. In some cases, defects in the laminate are marked to identify whether new additional defects are generated during the test.

[0115] The pouches containing the 1:1:1 sauce were then placed in a STERIS autoclave set at 121°C for 1 hour. The pouches were removed after testing and the extent of tunneling, blistering, delamination or leakage was compared to any marked pre-existing defects. Observations were recorded. The pouches were cut open, emptied, and rinsed with soap and water. One or more 15 mm strips were cut from the pouches and the laminate bond strength was measured according to the standard bond strength test described above. This process was completed as soon as possible after the pouch contents were removed. The interior of the pouch was visually inspected and any other visual defects were recorded.

[0116] Migration sample preparation

[0117] 30.8 square inches (in 2 )(198.7 square centimeters (cm 2 Each sample of the pouches composed of the laminate of ) was filled with 100 mL of 3% acetic acid. The pouches were then transferred to a chamber and stored at 121° C. for 2 hours. After testing and cooling to ambient temperature, the acetic acid was transferred to a polyethylene bottle.

[0118] Acetic acid samples were extracted and prepared for analysis within a few days of preparation and analyzed via UV-Vis spectroscopy within 24 hours of preparation.

[0119] Table 4 - Performance of the samples of the present invention and the comparative samples under the test condition of 121°C

[0120]

[0121] DL: Delamination, secondary membrane separates from primary membrane

[0122] AT: Adhesive transfer (adhesive fails to adhere to the primary film and transfers to the secondary film).

[0123] Table 5 - Performance of the samples of the present invention and the comparative samples under the boil-in-bag test conditions

[0124]

[0125] DL: Delamination, secondary membrane separates from primary membrane

[0126] AT: Adhesive transfer (adhesive fails to adhere to the primary film and transfers to the secondary film).

Claims

1. A solvent-based adhesive composition, comprising: a. at least one isocyanate component, the at least one isocyanate component comprising an aromatic-based isocyanate, wherein the weight of free monomeric isocyanate is less than 1% by weight based on the weight of the isocyanate component, and b. at least one isocyanate-reactive component, the at least one isocyanate-reactive component comprising at least one phosphate ester polyol.

2. The adhesive of claim 1, wherein the at least one aromatic-based isocyanate prepolymer comprises a reaction product of at least one isocyanate compound and at least one polyol compound.

3. The adhesive of any one of the preceding claims, wherein the weight percent of the at least one phosphate polyol, based on the weight of the isocyanate-reactive component, is at least 0.

1.

4. The adhesive according to any one of the preceding claims, wherein the NCO-reactive component further comprises a polyester polyol or a blend of a polyester polyol and a polyether polyol.

5. The adhesive according to any one of the preceding claims, wherein the molecular weight of at least one polyester polyol is greater than 2000 g / mol and less than 15,000 g / mol.

6. The adhesive of any one of the preceding claims, wherein the weight percent of the at least one polyester polyol, based on the weight of the isocyanate-reactive component, is at least 10.

7. The adhesive of any one of the preceding claims, wherein the weight percent of the at least one phosphate polyol is less than 20, based on the weight of the isocyanate-reactive component.

8. The composition according to any one of the preceding claims, further comprising a solvent selected from the group consisting of ethyl acetate, methyl ether ketone, acetone, toluene and other suitable solvents, mixtures of two or more thereof.

9. A method of producing a solvent-based polyurethane adhesive composition for use in producing laminates, the method comprising admixing: a. at least one isocyanate component, the at least one isocyanate component comprising an aromatic-based isocyanate, wherein the weight of free monomeric isocyanate is less than 1% by weight based on the weight of the isocyanate component, and b. at least one isocyanate-reactive component, the at least one isocyanate-reactive component comprising at least one phosphate ester polyol.

10. A multi-layer laminated product, comprising: (a) at least the first layer; (b) at least a second layer; and (c) The adhesive according to claim 1, wherein the adhesive is disposed between the first layer and the second layer; The adhesive is cured to bond the first layer to the second layer.

11. A method for producing a laminated product, the method comprising the steps of: a. The adhesive according to claim 1 is applied to at least a portion of the surface of the first layer and / or the second layer; b. contacting the first layer and the second layer so that the adhesive is disposed between the first layer and the second layer; and c. curing the adhesive to form a laminate comprising bonding the first layer to the second layer via the cured adhesive.

12. An article for flexible packaging, comprising the laminate according to claim 11.

Citation Information

Patent Citations

  • Two-component adhesive compositions based on phosphate ester modified isocyanates, and methods for making same

    CN112041364A

  • Bactericidal adhesive composition

    CN114127219A

  • Reactive polyurethanes having a low content of monomeric diisocyanates

    US20040259968A1

  • Ultralow Monomer Polyurethanes

    US20170369632A1

  • Polyurethane-Based Binder System

    US20180044462A1