Polyurethane (meth) acrylate and photocurable resin composition containing same
By combining specific polyurethane (meth)acrylate with polyisocyanate compound and dihydroxy compound, a photocurable resin composition is formed, and the problems of conflicting residual film ratio, flexibility and mechanical strength in the prior art are solved, so as to achieve the realization of the problem of Excellent performance and thixotropy after development.
Patent Information
- Application Number
- CN202380035711.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-09
- Filing Date
- 2023-05-02
- Publication Date
- 2024-12-03
AI Technical Summary
The conventional photocurable resin composition is difficult to achieve excellent residual film ratio, flexibility and mechanical strength after development at the same time, and does not cause whitening during winding, and has insufficient thixotropy.
Using specific polyurethane (meth)acrylate, 35-60% is formed by reaction between 75-90% polyoxyalkylene derivatives, 10-25% polyisocyanate compounds and 0-5% dihydroxy compounds. The polyurethane (meth)acrylate, combined with 35 to 60% of the (meth)acrylic polymer with an acid value of 50 to 300 mg KOH/g and 0.1 to 5% of the photopolymerization initiator, constitutes a photocurable resin composition .
The residual film after development is excellent in the rate, flexibility and mechanical strength, and does not whiten during winding, and has excellent thixotropy.
Smart Images

Figure CN119072510A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to urethane (meth) acrylate and a photocurable resin composition containing the urethane (meth) acrylate. Background Art
[0002] Photocurable resins are widely used in various applications such as coating materials such as hard coats, the manufacture of three-dimensional molded products, and photoresists. Among them, polyurethane (meth) acrylate is one of the representative photocurable resins. With the expansion of the use of photocurable resin compositions, the improvement and diversification of the requirements for the physical properties of photocurable resin compositions, polyurethane (meth) acrylates and photocurable resin compositions containing them are required to form films or layers with excellent properties such as mechanical strength and flexibility.
[0003] For example, as a resist material used for etching in the manufacture of printed wiring boards, plating in the field of metal precision processing, etc., a photosensitive element can be used, which is composed of a layer composed of a photosensitive resin composition (hereinafter referred to as a "photosensitive layer"), a support film, and a protective film as needed.
[0004] The pattern formation of the printed wiring board is carried out through the development process. In the development using a negative photoresist, the above-mentioned photosensitive layer is irradiated with active energy rays using a mask, so that the exposed part and the unexposed part show a solubility difference, and the unexposed part is dissolved with a solvent to form a pattern of a predetermined shape. In recent years, with the miniaturization of electronic products, the miniaturization of integrated circuits, and the high-precision of display devices, it is necessary to form fine patterns, so it is required that the residual film rate of the undissolved part based on the developer when forming the pattern is excellent.
[0005] Photosensitive elements are sometimes used in the form of coils, and since the photosensitive layer is bent when being wound into a coil, the photosensitive layer is required to be flexible. Furthermore, since the photosensitive layer is bent, it may sometimes partially whiten, which may lead to poor product quality, so it is also required to have a performance that does not cause whitening. In addition, when the through holes provided on the substrate are covered with a photosensitive layer such as a multi-layer circuit substrate, the photocurable resin composition is required to form a photosensitive layer that will not be broken by the injection pressure of the developer or water washing. However, in general, the flexibility is deteriorated when the mechanical strength is improved, but in order to meet all the above requirements, it is necessary to form a photosensitive layer with excellent flexibility and mechanical strength that are contradictory to each other.
[0006] In addition, the photosensitive layer is usually formed on the support film by coating the solution of the photocurable resin composition on the support film. If the viscosity of the composition is too high, the composition cannot be evenly coated. On the contrary, if the viscosity is too low, the film formed by the composition becomes thinner and the desired properties such as strength cannot be obtained. Therefore, the photocurable resin composition is also required to have thixotropy for controlling rheology.
[0007] In response to these requirements, various photocurable resin compositions have been studied in the past. For example, Patent Document 1 discloses a photosensitive resin composition that can form a pattern with excellent resolution and bendability by combining a binder polymer having a dispersion (weight average molecular weight / number average molecular weight) of less than 1.6 with a specific photopolymerizable compound. However, the residual film rate and thixotropy of the photosensitive resin composition described in Patent Document 1 are insufficient. Patent Document 2 discloses a photosensitive resist liquid with thixotropy, but there is no research on flexibility. Patent Document 3 discloses a film that does not whiten when bent by a specific acrylic resin composition, but there is no research on the residual film rate and thixotropy. [Prior art literature] [Patent Literature]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 2013-109323 [Patent Document 2] Japanese Patent Application Publication No. 2005-152736 [Patent Document 3] Japanese Patent Application Publication No. 2020-147653 Summary of the invention [Problems to be solved by the invention]
[0009] An object of the present invention is to provide a photocurable resin composition which has excellent residual film rate after development, flexibility, and mechanical strength, can form a film which does not whiten when wound up, and has excellent thixotropy.
Methods to solve the problem
[0010] The present inventors have studied to solve the above problems and have found that the above problems can be solved by using a specific urethane (meth)acrylate. The present invention based on this finding is as follows.
[0011] [1] Polyurethane (meth)acrylate, characterized in that it is obtained by reacting 75 to 90% by mass of a polyoxyalkylene derivative (A) represented by formula (1), 10 to 25% by mass of a polyisocyanate compound (B) represented by formula (2), and 0 to 5% by mass of a dihydroxy compound (C) represented by formula (3).
[0012]
Chemical formula 1
[0013] (Where R 1 is a hydrogen atom or a methyl group, l, m and n represent the average degree of polymerization respectively, l is a number from 1 to 20, m is a number from 0 to 15, and n is a number from 1 to 10. )
[0014]
Chemical formula 2
[0015] (In the formula, 3 R 2 are each independently an alkylene group having 1 to 10 carbon atoms.) HO-(R 3 O) p -H(3) (Where R 3 is an alkylene group having 2 to 4 carbon atoms, and p represents an average degree of polymerization, which is a number greater than 1 and less than 5. )
[0016] In the reaction of [1], the amounts of the above components are all values relative to the total amount of the above polyoxyalkylene derivative (A), the above polyisocyanate compound (B) and the above dihydroxy compound (C) (hereinafter, sometimes referred to as "the total amount of reactants").
[0017] [2] A photocurable resin composition comprising 35 to 60% by mass of the polyurethane (meth)acrylate described in [1] above, 35 to 60% by mass of a (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g, and 0.1 to 5% by mass of a photopolymerization initiator.
[0018] Hereinafter, the photocurable resin composition of the above-mentioned [2] may be described as "photocurable resin composition (I)". In addition, the content of the above-mentioned components in the photocurable resin composition (I) is a value relative to the total amount of the above-mentioned urethane (meth)acrylate, the above-mentioned (meth)acrylic polymer and the above-mentioned photopolymerization initiator (hereinafter, sometimes described as "the total amount of components (I)").
[0019] [3] A photocurable resin composition comprising 30 to 50% by mass of the polyurethane (meth)acrylate described in [1] above, 0.01 to 10% by mass of a polyoxyalkylene derivative (A) represented by the formula (1), 40 to 60% by mass of a (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g, and 0.1 to 5% by mass of a photopolymerization initiator.
[0020]
Chemical formula 3
[0021] (Where R 1 is a hydrogen atom or a methyl group, l, m and n represent the average degree of polymerization respectively, l is a number from 1 to 20, m is a number from 0 to 15, and n is a number from 1 to 10. )
[0022] Hereinafter, the photocurable resin composition of the above-mentioned [3] may be described as "photocurable resin composition (II)". In addition, the content of the above-mentioned components in the photocurable resin composition (II) is a value relative to the total amount of the above-mentioned polyurethane (meth)acrylate, the above-mentioned polyoxyalkylene derivative (A), the above-mentioned (meth)acrylic polymer and the above-mentioned photopolymerization initiator (hereinafter, sometimes described as "the total amount of components (II)"). [Effects of the invention]
[0023] By using the polyurethane (meth)acrylate of the present invention, a photocurable resin composition can be obtained which has excellent residual film rate after development, flexibility and mechanical strength, can form a film which does not whiten when wound up, and has excellent thixotropy. DETAILED DESCRIPTION
[0024] The following is a detailed description of this specific embodiment, but the present invention is not limited to the following embodiment.
[0025] In this specification, "(meth)acrylate" means acrylate or methacrylate. Here, only one (meth)acrylate may be used, or two or more (meth)acrylates may be used in combination. Therefore, when there may be two or more (meth)acrylates, "(meth)acrylate" means acrylate and / or methacrylate. The meaning of the term "(meth)acrylic acid" is also the same as that of "(meth)acrylate".
[0026] In the present specification, a “polyethylene glycol chain” means a polyoxyethylene chain, a “polypropylene glycol chain” means a polyoxypropylene chain, a “polybutylene glycol chain” means a polyoxybutylene chain, and a “polytetramethylene glycol chain” means a polyoxytetramethylene chain.
[0027] In the present specification, "propenyl" means a propylene group, and "butenyl" means a butylene group. Therefore, both the propenyl group and the butenyl group may be straight-chain or branched-chain.
[0028] [Polyoxyalkylene derivative (A)] The polyoxyalkylene derivative (A) used in the present invention is represented by formula (1):
[0029]
Chemical formula 4
[0030] (Where R 1 is a hydrogen atom or a methyl group, l, m and n represent the average degree of polymerization respectively, l is a number from 1 to 20, m is a number from 0 to 15, and n is a number from 1 to 10. ) The polyoxyalkylene derivative (A) may be used alone or in combination of two or more.
[0031] From the viewpoint of improving the flexibility of urethane (meth)acrylate, R 1 Preferred is methyl.
[0032] In formula (1), l, m and n are the average polymerization degrees of oxyethylene (C2H4O), oxypropylene (C3H6O) and oxybutylene (C4H8O), respectively. Therefore, l, m and n can all be decimals. In addition, (C3H6O) is an arbitrary constituent unit and m can also be 0.
[0033] l is 1 to 20, preferably 4 to 17, more preferably 6 to 15, and further preferably 8 to 12. m is 0 to 15, preferably 0 to 10, more preferably 0 to 5, further preferably 0 to 2, and particularly preferably 0. n is 1 to 10, preferably 2 to 9, more preferably 3 to 8, and further preferably 4 to 6. By using a polyoxyalkylene derivative (A) in which l, m, and n are within the above ranges, the residual film rate of a film formed from the photocurable resin composition can be improved while maintaining the flexibility thereof.
[0034] The butenyl group may be either linear or branched, but a linear butenyl group is preferred from the viewpoint of flexibility and residual film rate of a film formed from the photocurable resin composition. That is, (C4H8O) in formula (1) is preferably oxytetramethylene.
[0035] In addition, -(C2H4O) l -(C3H6O) m -(C4H8O) n -C2H4O, C3H6O and C4H8O in the formula (1) may exist randomly or in blocks. In addition, their arrangement order is not particularly limited and may be different from the arrangement described in the formula (1).
[0036] As the polyoxyalkylene derivative (A), a commercially available one may be used, or a synthesized one may be used. In order to form a film having excellent flexibility, residual film rate, and mechanical strength, the polyoxyalkylene derivative (A) is preferably: R 1Polyethylene glycol-tetramethylene glycol monomethacrylate wherein C4H8O is methyl, m is 0, and C2H4O and C4H8O in polyethylene glycol-tetramethylene glycol monomethacrylate may exist randomly or in blocks as described above, and their arrangement order is not particularly limited.
[0037] [Polyisocyanate compound (B)] The polyisocyanate compound (B) used in the present invention is represented by formula (2):
[0038]
Chemical formula 5
[0039] (In the formula, 3 R 2 are each independently an alkylene group having 1 to 10 carbon atoms.) The polyisocyanate compound (B) may be used alone or in combination of two or more.
[0040] The three R in formula (2) 2 They can be the same or different, but from the perspective of easy availability, the three R 2 Preferably they are the same substance. 2 The alkylene group may be linear or branched, but is preferably linear.
[0041] R 2 The number of carbon atoms in R is preferably 3 to 9, more preferably 4 to 8, and still more preferably 5 to 7. 2 The polyisocyanate compound (B) having a carbon number within the above range can improve the mechanical strength and residual film rate of a film formed from the photocurable resin composition while maintaining the flexibility thereof.
[0042] The polyisocyanate compound (B) may be a commercially available substance or a synthetic substance. As the polyisocyanate compound (B), for example, isocyanurates of diisocyanates (i.e., trimers of diisocyanates) (e.g., DURANATE TPA-100 and DURANATE TKA-100 manufactured by Asahi Chemicals Corporation) etc. may be cited. From the viewpoint of the residual film rate of the film formed by the photocurable resin composition, isocyanurates of hexamethylene diisocyanate (i.e., trimers of hexamethylene diisocyanate) are particularly preferred as the polyisocyanate compound (B).
[0043] [Dihydroxy compound (C)] The dihydroxy compound (C) used in the present invention is represented by formula (3): HO-(R 3 O)p -H(3) (Where R 3 is an alkylene group having 2 to 4 carbon atoms, and p represents an average degree of polymerization, which is a number greater than 1 and less than 5. ) The dihydroxy compound (C) may be used alone or in combination of two or more. The dihydroxy compound (C) is an optional component, and the polyurethane (meth)acrylate of the present invention can be produced without using the dihydroxy compound (C).
[0044] R 3 The alkylene group may be straight chain or branched chain. 3 The number of carbon atoms in is preferably 2 to 4, more preferably 2 to 3, and still more preferably 2. 3 The dihydroxy compound (C) having a carbon number within the above range can increase the residual film rate of a film formed from the photocurable resin composition.
[0045] p is an average degree of polymerization and may be a decimal. p is preferably 1 to 4, more preferably 1 to 3, and further preferably 2. By using a dihydroxy compound (C) having p within the above range, the residual film rate of a film formed from the photocurable resin composition can be increased.
[0046] As the dihydroxy compound (C), diethylene glycol is particularly preferred from the viewpoint of the residual film ratio of the film.
[0047] [Urethane (meth)acrylate] The urethane (meth)acrylate of the present invention can be obtained by urethanization reaction of 75 to 90% by mass of a polyoxyalkylene derivative (A), 10 to 25% by mass of a polyisocyanate compound (B), and 0 to 5% by mass of a dihydroxy compound (C).
[0048] The amount of the polyoxyalkylene derivative (A) in the urethanization reaction is preferably 78 to 89% by mass, more preferably 79 to 88% by mass, further preferably 81 to 86% by mass, particularly preferably 83 to 85% by mass, based on the total amount of reactants. The amount of the polyisocyanate compound (B) in the polyurethane reaction is preferably 11 to 22% by mass, more preferably 12 to 21% by mass, further preferably 14 to 19% by mass, particularly preferably 15 to 17% by mass, based on the total amount of reactants. The amount of the dihydroxy compound (C) in the urethanization reaction is preferably 0 to 4% by mass, more preferably 0 to 3% by mass, further preferably 0.01 to 2% by mass, particularly preferably 0.1 to 1% by mass, based on the total amount of reactants. By reacting the components in the amounts within the above ranges, the polyurethane (meth)acrylate of the present invention can be produced with good productivity without causing residual raw materials or gelation, and further, the mechanical strength and residual film rate of the film formed from the photocurable resin composition can be improved while maintaining the flexibility thereof.
[0049] The polyurethane reaction is preferably carried out in the presence of a catalyst and a polymerization inhibitor. Examples of polyurethane catalysts include cobalt naphthenate, zinc naphthenate, stannous chloride, tin chloride, tetra-n-butyltin, tri-n-butyltin acetate, n-butyltin trichloride, trimethyltin hydroxide, dimethyltin dichloride, dibutyltin acetate, dibutyltin dilaurate, dibutyltin diethylhexanoate, dibutyltin sulfite, and tin octenate. The catalyst may be used alone or in combination of two or more. When a catalyst is used, its amount is preferably 10 to 1,000 ppm (by mass) relative to the total amount of the reactants.
[0050] Examples of the polymerization inhibitor include phenols such as hydroquinone, hydroquinone monomethyl ether, mono-tert-butylhydroquinone, catechol, p-tert-butylcatechol, 2,6-di-tert-butyl-m-cresol, 2,6-di-tert-butyl-4-methylphenol, pyrogallol, and β-naphthol; quinones such as benzoquinone, 2,5-diphenyl-p-benzoquinone, methyl-p-benzoquinone, and dimethyl-p-benzoquinone; nitro compounds or nitroso compounds such as nitrobenzene, m-dinitrobenzene, 2-methyl-2-nitrosopropane, α-phenyl-tert-butylnitrone, and 5,5-dimethyl-1-pyrroline-1-oxide; amines such as tetrachlorobenzoquinone-amine, diphenylamine, diphenylpicrylhydrazine, phenol-α-naphthylamine, pyridine, and phenothiazine; and sulfides such as dithiobenzoyl sulfide and dibenzyltetrasulfide. The polymerization inhibitor may be used alone or in combination of two or more.
[0051] When a polymerization inhibitor is used, its amount is preferably 10 to 10,000 ppm (mass basis) relative to the total amount of the reactants, and more preferably 100 to 1,000 ppm. When the amount of the polymerization inhibitor is less than 10 ppm, a sufficient polymerization inhibition effect may not be obtained, and when it exceeds 10,000 ppm, various physical properties of the obtained polyurethane (meth)acrylate may be adversely affected.
[0052] The reaction temperature in the polyurethane reaction is preferably 20 to 90° C., and the reaction time is preferably 1 to 30 hours. When the reaction temperature is lower than 20° C. or the reaction time is shorter than 1 hour, the yield of the target polyurethane (meth) acrylate tends to decrease. On the other hand, when the reaction temperature is higher than 90° C. or the reaction time is longer than 30 hours, coloration and side reactions of the polyurethane (meth) acrylate tend to occur easily.
[0053] In the above-mentioned polyurethane reaction, an organic solvent may also be used. Examples of the organic solvent include aromatic hydrocarbon solvents such as toluene and xylene; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; and ester solvents such as ethyl acetate, propyl acetate, isobutyl acetate, and butyl acetate.
[0054] The end point of the polyurethane reaction can be determined by the 2270 cm-1 -1 The infrared absorption spectrum of the reaction mixture disappears, or the isocyanate content is determined by the method described in JIS K 7301. In the latter method, the isocyanate content is calculated and the end point is when the polyurethane (meth)acrylate content becomes 0.5% by mass or less, preferably 0.1% by mass or less.
[0055] [Photocurable resin composition] The present invention provides a photocurable resin composition (I), comprising The polyurethane (meth)acrylate of the present invention, A (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g, and Photopolymerization initiator.
[0056] The present invention also provides a photocurable resin composition (II), which contains The polyurethane (meth)acrylate of the present invention, The polyoxyalkylene derivative (A) represented by the above formula (1), A (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g, and Photopolymerization initiator.
[0057] Hereinafter, each component in the photocurable resin composition (I) and (II) will be described in turn. Each component may be used in one kind only, or in two or more kinds. In addition, below, sometimes "photocurable resin composition (I) and (II)" are collectively referred to as "photocurable resin composition of the present invention".
[0058] The polyurethane (meth)acrylate of the present invention is described above. The content of the polyurethane (meth)acrylate of the present invention in the photocurable resin composition (I) is 35 to 60% by mass, preferably 43 to 57% by mass, and more preferably 47 to 53% by mass relative to the total amount of the components (I). The content of the polyurethane (meth)acrylate of the present invention in the photocurable resin composition (II) is 30 to 50% by mass, preferably 40 to 50% by mass, and more preferably 44 to 50% by mass based on the total amount of the component (II). By adjusting the content of the urethane (meth)acrylate of the present invention to the above range, the mechanical strength and the residual film rate of the film formed from the photocurable resin composition can be improved while maintaining the flexibility thereof.
[0059] The description of the polyoxyalkylene derivative (A) in the photocurable resin composition (II) is the same as that described in [Polyoxyalkylene derivative (A)]. From the viewpoint of not damaging the thixotropy of the above-mentioned composition and the mechanical strength of the obtained film and imparting flexibility to the film, the content of the polyoxyalkylene derivative (A) in the photocurable resin composition (II) is 0.01 to 10% by mass, preferably 0.1 to 8% by mass, and more preferably 1 to 6% by mass relative to the total amount of the component (II). When the content is less than 0.01% by mass, it is not confirmed that the flexibility of the film is improved, and when it is more than 10% by mass, the mechanical strength of the film is reduced.
[0060] The photocurable resin composition of the present invention contains a (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g. By using such a (meth)acrylic acid polymer, the developability during development using an alkaline solution is improved. In this specification, "(meth)acrylic acid polymer" means a polymer having a constituent unit derived from (meth)acrylic acid. From the viewpoint of developability, the acid value of the above-mentioned (meth)acrylic acid polymer is preferably 80 to 180 mgKOH / g, preferably 100 to 150 mgKOH / g.
[0061] The above-mentioned (meth) acrylic acid series polymer is preferably a copolymer of (meth) acrylic acid and (meth) acrylic acid alkyl ester. In addition, the "alkyl" in this specification also includes cycloalkyl. Both (meth) acrylic acid and (meth) acrylic acid alkyl ester can be used in only one kind, or in two or more kinds. As (meth) acrylic acid alkyl ester, for example, methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, butyl (meth) acrylate, pentyl (meth) acrylate, hexyl (meth) acrylate, cyclohexyl (meth) acrylate, heptyl (meth) acrylate, octyl (meth) acrylate, 2-ethylhexyl (meth) acrylate, etc. can be cited. The above-mentioned (meth) acrylic acid series polymer is more preferably a copolymer of (meth) acrylic acid, cyclohexyl (meth) acrylate and methyl (meth) acrylate, and more preferably a copolymer of methacrylic acid, cyclohexyl methacrylate and methyl methacrylate.
[0062] From the viewpoint of mechanical strength and flexibility of a film formed from the photocurable resin composition, the weight average molecular weight of the (meth)acrylic polymer is preferably 10,000 to 100,000, more preferably 15,000 to 80,000, and even more preferably 20,000 to 60,000. The weight average molecular weight is a value measured by gel permeation chromatography (GPC).
[0063] The content of the (meth)acrylic polymer in the photocurable resin composition (I) is 35 to 60% by mass, preferably 39 to 56.5% by mass, and more preferably 44 to 52% by mass, based on the total amount of the components (I). The content of the (meth)acrylic polymer in the photocurable resin composition (II) is 40 to 60% by mass, preferably 43 to 57% by mass, and more preferably 46 to 54% by mass, based on the total amount of the component (II). By adjusting the content of the (meth)acrylic polymer to the above range, the mechanical strength and the residual film ratio of the film formed from the photocurable resin composition can be improved while maintaining the flexibility of the film.
[0064] The photocurable resin composition of the present invention contains a photopolymerization initiator. Examples of the photopolymerization initiator include benzoin isopropyl ether, benzoin isobutyl ether, benzophenone, Michler's ketone, methyl o-benzoylbenzoate, acetophenone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, ethyl anthraquinone, isopentyl p-dimethylaminobenzoate, ethyl p-dimethylaminobenzoate, 1-hydroxycyclohexyl phenyl ketone (e.g., Irgacure 184 manufactured by BASF), 2-hydroxy-2-methyl-1-phenyl-1-propanone (e.g., Darocur 1173 manufactured by BASF), 2,2-dimethoxy-1,2-diphenyl-1-ethanone (e.g., Irgacure 651 manufactured by BASF), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone (e.g., Irgacure 184 manufactured by BASF), and 1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone (e.g., Irgacure 184 manufactured by BASF). 907), 2-benzyl-2-dimethylamino-1(4-morpholinophenyl)-1-butanone, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, methyl benzylformate, etc.
[0065] The content of the photopolymerization initiator in the photocurable resin composition (I) is 0.1 to 5% by mass, preferably 0.5 to 4% by mass, and more preferably 1 to 3% by mass, based on the total amount of the components (I). The content of the photopolymerization initiator in the photocurable resin composition (II) is 0.1 to 5% by mass, preferably 0.5 to 4% by mass, and more preferably 1 to 3% by mass, based on the total amount of the component (II). By adjusting the content of the photopolymerization initiator to the above range, the mechanical strength of the film formed from the photocurable resin composition can be improved while maintaining its flexibility.
[0066] The photocurable resin composition of the present invention may contain a solvent or other components unless the effects of the present invention are impaired.
[0067] As the solvent, any known solvent can be used, for example, methanol, ethanol, ethyl acetate, butyl acetate, acetone, methyl ethyl ketone, N,N-dimethylformamide, tetrahydrofuran, benzene, toluene, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol ethyl methyl ether, propylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate, etc. The solvent may be used alone or in combination of two or more.
[0068] When a solvent is used, the content of the solvent in the photocurable resin composition (I) is preferably 35 to 60% by mass, more preferably 40 to 60% by mass, and even more preferably 45 to 55% by mass based on the entire photocurable resin composition (I). When a solvent is used, the content of the solvent in the photocurable resin composition (II) is preferably 35 to 65% by mass, more preferably 40 to 60% by mass, and even more preferably 45 to 55% by mass based on the entire photocurable resin composition (II). By adjusting the content of the solvent to the above range, the mechanical strength and the residual film ratio of the film formed from the photocurable resin composition can be improved while maintaining the flexibility of the film.
[0069] As other components, for example, heat-resistant enhancers, leveling agents, developing aids, inorganic fine particles, coupling agents, fillers, thermosetting resins such as epoxy resins, phenolic resins, and polyvinylphenol, curing agents, plasticizers, polymerization inhibitors, antioxidants, defoamers, viscosity modifiers, pigments, etc. Other components may be used alone or in combination of two or more.
[0070] The photocurable resin composition of the present invention can be applied to a substrate by a known method, and examples of such methods include dip coating, spray coating, flow coating, curtain coating, roll coating, spin coating, and brush coating.
[0071] The photocurable resin composition of the present invention can be formed into a cured film by irradiating active energy rays such as ultraviolet rays, visible light, radiation, electron beams, etc. For photocuring, a high-pressure mercury lamp, a metal halide lamp, etc. can be used. The atmosphere for irradiating light can be air or an inert gas such as nitrogen or argon. [Example]
[0072] Hereinafter, examples and comparative examples are given to further specifically illustrate the above-mentioned embodiment.
[0073] (Synthesis of polyurethane (meth)acrylate) (Synthesis example 1) 300 g of polyethylene glycol-tetramethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER55PET-800, R in formula (1)) as a polyoxyalkylene derivative (A) was added to a 1000 ml flask equipped with a stirrer, a thermometer, and a condenser. 1 : methyl, l: about 10, m: 0, n: about 5, C2H4O and C4H8O are randomly present), 0.05g of dibutyltin dilaurate as a polyurethane catalyst, and 0.05g of 2,6-di-tert-butyl-4-methylphenol as a polymerization inhibitor. 57.1g of polyisocyanate compound (B) (manufactured by Asahi Kasei Chemicals Co., Ltd., isocyanurate of hexamethylene diisocyanate, trade name: DURANATE TPA-100, isocyanate group content: 23.1% by mass) was added to the above flask so that the mass ratio of polyoxyalkylene derivative (A): polyisocyanate compound (B) was 84:16, and the reaction was maintained at 70°C for 5 hours. Then, the reaction was carried out until the isocyanate group content according to the method in accordance with JIS K 7301 was 0.1 mass % or less, and then 0.1 g of hydroquinone monomethyl ether was added to the flask as a polymerization inhibitor to obtain the target polyurethane (meth)acrylate.
[0074] (Synthesis example 2) The same operation as in Synthesis Example 1 was carried out except that 299 g of polyethylene glycol-tetramethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER55PET-800) as the polyoxyalkylene derivative (A) and 1 g of diethylene glycol as the dihydroxy compound (C) were used instead of 300 g of polyethylene glycol-tetramethylene glycol monomethacrylate to obtain the target polyurethane (meth)acrylate.
[0075] (Comparative Synthesis Example 1) The target polyurethane (meth)acrylate was obtained by the same operation as in Synthesis Example 1 except that 300 g of polyethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER AE-200) as a polyoxyethylene derivative was used instead of 300 g of polyethylene glycol-tetramethylene glycol monomethacrylate.
[0076] (Preparation of Photocurable Resin Composition) (Example 1) 200 g of methyl ethyl ketone as a solvent, 100 g of the polyurethane (meth)acrylate of Synthesis Example 1, 3 g of a photopolymerization initiator ("Irgacure 907" manufactured by BASF), and 100 g of a polymer 1 as a (meth)acrylic polymer (a copolymer of methacrylic acid, cyclohexyl methacrylate and methyl methacrylate, with respect to the monomer components forming the polymer 1 (i.e., the total amount of methacrylic acid, cyclohexyl methacrylate and methyl methacrylate), the amount of methacrylic acid: 20% by mass, the amount of cyclohexyl methacrylate: 50% by mass, the amount of methyl methacrylate: 30% by mass, the acid value of the polymer 1: 130 mgKOH / g, the weight average molecular weight of the polymer 1: 30,000) were mixed to prepare a photocurable resin composition.
[0077] (Example 2) A photocurable resin composition was obtained by performing the same operation as in Example 1 except that 100 g of the urethane (meth)acrylate of Synthesis Example 2 was used instead of 100 g of the urethane (meth)acrylate of Synthesis Example 1.
[0078] (Example 3) The same operation as in Example 1 was carried out, except that 99 g of the polyurethane (meth)acrylate of Synthesis Example 1 and 1 g of polyethylene glycol-tetramethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER 55PET-800) as the polyoxyalkylene derivative (A) were used instead of 100 g of the polyurethane (meth)acrylate of Synthesis Example 1, to obtain a photocurable resin composition.
[0079] (Example 4) The same operation as in Example 1 was carried out, except that 95 g of the polyurethane (meth)acrylate of Synthesis Example 1 and 5 g of polyethylene glycol-tetramethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER 55PET-800) as the polyoxyalkylene derivative (A) were used instead of 100 g of the polyurethane (meth)acrylate of Synthesis Example 1, to obtain a photocurable resin composition.
[0080] (Example 5) The same operation as in Example 1 was carried out except that 97.5 g of the polyurethane (meth) acrylate of Synthesis Example 2 and 2.5 g of polyethylene glycol-tetramethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER 55PET-800) as the polyoxyalkylene derivative (A) were used instead of 100 g of the polyurethane (meth) acrylate of Synthesis Example 1 to obtain a photocurable resin composition.
[0081] (Comparative Example 1) The same operation as in Example 1 was carried out, except that 50 g of the polyurethane (meth) acrylate obtained in Synthesis Example 1 and 50 g of polyethylene glycol-tetramethylene glycol monomethacrylate (manufactured by NOF Corporation, trade name: BLEMMER 55PET-800) as the polyoxyalkylene derivative (A) were used instead of 100 g of the polyurethane (meth) acrylate in Synthesis Example 1, to obtain a photocurable resin composition.
[0082] (Comparative Example 2) A photocurable resin composition was obtained by performing the same operation as in Example 1 except that 100 g of the urethane (meth)acrylate of Comparative Synthesis Example 1 was used instead of 100 g of the urethane (meth)acrylate of Synthesis Example 1.
[0083] (Comparative Example 3) A photocurable resin composition was obtained by carrying out the same operation as in Example 1 except that 100 g of trimethylolpropane triacrylate was used instead of 100 g of the urethane (meth)acrylate of Synthesis Example 1.
[0084] (Evaluation) (Evaluation of thixotropy) Using a rheometer, at a temperature of 25°C and 1s -1 , or temperature 25℃ and 10s -1 The viscosity of the photocurable resin composition is measured by the following formula: TI value = at a temperature of 25°C and a shear rate of 1s -1 Viscosity of the photocurable resin composition at a temperature of 25°C and a shear rate of 10 s -1 The viscosity of the photocurable resin composition under The TI value was calculated and the thixotropy was evaluated according to the following criteria. The results are shown in Tables 1 and 2. ◎: TI value is 1.5 or more ○: TI value is 1.1 or more and less than 1.5 ×: TI value is 1.0 or more and less than 1.1
[0085] (Whitened evaluation) The photocurable resin composition was applied to a polyethylene terephthalate (PET) film ("A4100" manufactured by Toyobo Co., Ltd., film thickness 50 μm), and dried on a hot plate at 120° C. for 5 minutes to obtain a film of the photocurable resin composition. The film was repeated 10 times using a cylindrical mandrel bending tester (manufactured by BEVS Co., Ltd.) and then wound on a After the test, the appearance of the film was visually checked and whitening was evaluated using the following criteria. The results are shown in Tables 1 and 2. ◎: After the test, the film has no change in appearance. ○: After the test, the film was slightly whitened. ×: After the test, the film was whitened.
[0086] (Evaluation of residual film rate) The photocurable resin composition was applied to a glass substrate and dried at 120°C, and the film thickness (initial film thickness) of the obtained coating was measured. Then, the obtained coating was irradiated with ultraviolet rays to prepare a cured film. The obtained cured film was immersed in a 0.4 mass% tetramethylammonium hydroxide aqueous solution for 60 seconds, washed with water and dried, and then the film thickness (film thickness after immersion) of the cured film was measured. The film thickness was measured at 3 points by the stylus method, and their average value was used as the value of the initial film thickness or the film thickness after immersion, according to the following formula: Residual film rate (%) = film thickness after immersion (μm) / initial film thickness (μm) × 100 The residual film ratio was calculated and evaluated using the following criteria. The results are shown in Tables 1 and 2. ◎: Residual film rate is more than 85% ○: Residual film rate is 80% or more and less than 85% ×: Residual film rate is less than 80%
[0087] (Evaluation of film strength) The photocurable resin composition was applied to a glass substrate and dried on a heating plate at 120°C to prepare a coating film. Then, the obtained coating film was irradiated with ultraviolet rays to prepare a cured film. The cured film was peeled off from the glass substrate, and a test piece of 10 mm wide × 50 mm long was cut out. A tensile test was performed using an Autograph (manufactured by Shimadzu Corporation: EZ-SX) at a tensile speed of 10 mm / min to measure the tensile strength, and the film strength was evaluated using the following criteria. The results are shown in Tables 1 and 2. ◎: Tensile strength: 5.0N / mm 2 above ○: Tensile strength: 3.0 N / mm 2 Above, less than 5.0N / mm 2 ×: Tensile strength is less than 3.0 N / mm 2
[0088] (Evaluation of Softness) The test piece was prepared and the tensile test was carried out in the same manner as the evaluation of the film strength described above. The elongation at break (%) was calculated by the following formula: elongation at break (%) = 100 × (L-L0) / L0 (Where L0 is the gauge length, and L is the gauge length at break.) The elongation at break was calculated and the flexibility was evaluated according to the following criteria. The results are shown in Tables 1 and 2. ◎: Elongation at break is 10% or more ○: Elongation at break is 5% or more and less than 10% ×: Elongation at break less than 5%
[0089]
Table 1
[0090]
Table 2
[0091] The evaluation results shown in Tables 1 and 2 show that the photocurable resin compositions of Examples 1 to 5 are excellent in thixotropy, and the cured films obtained therefrom have excellent residual film rate, tensile strength, elongation at break, and no whitening when bent.
[0092] In Comparative Example 1, the tensile strength was insufficient because the amount of the polyoxyalkylene derivative (A) used was large. In Comparative Example 2, the elongation at break was insufficient because the polyurethane (meth) acrylate of Comparative Synthesis Example 1 that did not satisfy the conditions of the present invention was used instead of the polyurethane (meth) acrylate of the present invention. In Comparative Example 3, the elongation at break was insufficient because trimethylolpropane triacrylate was used instead of the polyurethane (meth) acrylate of the present invention.
Industrial Applicability
[0093] The photocurable resin composition containing the urethane (meth)acrylate of the present invention is useful as a coating material, a photoresist, etc., and is also useful for production of a three-dimensional molded article.
[0094] This application is based on Japanese Patent Application No. 2022-077261 filed in Japan, the entire contents of which are incorporated herein by reference.
Claims
1. A urethane (meth) acrylate, characterized in that make 75 to 90% by mass of the polyoxyalkylene derivative (A) represented by the formula (1), 10 to 25% by mass of a polyisocyanate compound (B) represented by formula (2) and 0 to 5% by mass of a dihydroxy compound (C) represented by formula (3) Reaction Formula (1): In formula (1), R 1 is a hydrogen atom or a methyl group, l, m and n respectively represent an average degree of polymerization, l is a number from 1 to 20, m is a number from 0 to 15, and n is a number from 1 to 10; Formula (2): In formula (2), the three R 2 are each independently an alkylene group having 1 to 10 carbon atoms; Formula (3): HO-(R 3 o) p -H(3) In formula (3), R 3 is an alkylene group having 2 to 4 carbon atoms, and p represents an average degree of polymerization, which is a number of 1 or more and less than 5.
2. A photocurable resin composition, characterized in that contain 35 to 60% by mass of the urethane (meth)acrylate according to claim 1, 35 to 60% by mass of a (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g and 0.1 to 5% by mass of a photopolymerization initiator.
3. A photocurable resin composition, characterized in that contain 30 to 50% by mass of the urethane (meth)acrylate according to claim 1, 0.01 to 10% by mass of a polyoxyalkylene derivative (A) represented by the formula (1), 40 to 60% by mass of a (meth)acrylic acid polymer having an acid value of 50 to 300 mgKOH / g and 0.1 to 5% by mass of a photopolymerization initiator; Formula (1): In the formula, R 1 is a hydrogen atom or a methyl group, l, m and n respectively represent an average degree of polymerization, l is a number of 1 to 20, m is a number of 0 to 15, and n is a number of 1 to 10.