Thermally conductive silicone composition

By using specific organopolysiloxanes, thermal conductivity fillers, low melting point gallium alloys, and alkoxysilane compounds in the silicone composition, the problem of insufficient thermal conductivity and moisture resistance in the prior art is solved, and efficient Heat dissipation performance and stable thermal resistance performance.

CN119072532APending Publication Date: 2024-12-03SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
CN202380034590.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-22
Filing Date
2023-03-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing thermal conductivity materials cannot obtain sufficient thermal conductivity and moisture resistance in highly integrated and high-speed heat-generating electronic components, which makes it difficult to solve the thermal resistance problem.

Method used

The thermal conductivity and moisture resistance are optimized by mixing appropriate ratios using a thermally conductive silicone composition comprising specific organopolysiloxanes, thermal conductivity fillers, and low melting point gallium or gallium alloys, alkoxysilane compounds.

Benefits of technology

The silicone composition with excellent thermal conductivity and humidity resistance is suitable as a high-performance heat dissipation paste and can maintain low thermal resistance under high temperature and high humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention is a thermally conductive silicone composition comprising the following components (A)-(D): 100 parts by mass of (A) an organopolysiloxane having a kinematic viscosity at 25 DEG C of 10-500,000 mm2 / s; (B) 10-2,000 parts by mass of a thermally conductive filler having an average particle diameter of 0.01-100 [mu] m; 1,000-20,000 parts by mass of (C) gallium or a gallium alloy having a melting point of-20 DEG C to 100 DEG C; and (D) 0.1-100 parts by mass of an alkoxysilane compound represented by general formula (1). As a result, a thermally conductive silicone composition having excellent thermal conductivity and heat resistance is provided. In the formula (1), R1 is an alkyl group with the carbon atom number of 6-20, R2 is an unsubstituted or substituted monovalent alkyl group with the carbon atom number of 1-10, R3 is an alkyl group with the carbon atom number of 1-6, a is an integer of 1-3, b is an integer of 0-2, and the sum of a and b is an integer of 1-3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thermally conductive organic silicon composition. Background Art

[0002] For example, in order to prevent damage or performance degradation caused by temperature rise during use, heat sinks and other heat sinks are widely used in most heat-generating electronic components such as CPUs (Central Processing Units). In order to efficiently conduct the heat generated by the heat-generating electronic components to the heat sink, a thermally conductive material is generally used between the heat-generating electronic components and the heat sink.

[0003] As thermally conductive materials, heat sinks and thermal pastes are generally known. Although heat sinks can be easily installed, gaps may be generated at the interface between the heat generating electronic components or the heat sink, for example, so that the interface thermal resistance becomes larger and the thermal conductivity becomes insufficient. On the other hand, thermal pastes are similar in properties to liquids, so they are not affected by the unevenness of the surfaces of the heat generating electronic components or the heat sink, and can be closely attached to both and reduce the interface thermal resistance, but sufficient heat dissipation performance cannot be obtained.

[0004] Therefore, for example, Patent Documents 1 to 5 propose technologies for blending low melting point metals or metal fillers as components that impart thermal conductivity. However, these thermally conductive materials still cannot achieve sufficient thermal conductivity effects due to the further increase in heat generation caused by the high integration and high speed of heat-generating electronic components in recent years. Patent Document 6 discloses that although the heat dissipation performance is significantly improved, there is still a disadvantage of poor moisture resistance.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2003-176414

[0008] Patent Document 2: Japanese Patent Application Publication No. 2005-112961

[0009] Patent Document 3: Japanese Patent Application Publication No. 2003-218296

[0010] Patent Document 4: Japanese Patent Application Publication No. 2004-039829

[0011] Patent Document 5: Japanese Patent Application Publication No. 2007-106809

[0012] Patent Document 6: Japanese Patent Application Publication No. 2021-169582 Summary of the invention

[0013] 1. Technical issues to be resolved

[0014] An object of the present invention is to provide a thermally conductive silicone composition which is formed to solve the above-mentioned technical problems and has excellent thermal conductivity and moisture resistance.

[0015] (II) Technical solution

[0016] In order to solve the above technical problems, the present invention provides a thermally conductive silicone composition, which comprises the following components (A) to (D):

[0017] 100 parts by mass of (A) having a kinematic viscosity at 25°C of 10 to 500,000 mm 2 / s of organopolysiloxane;

[0018] 10 to 2,000 parts by mass of (B) a thermally conductive filler having an average particle size of 0.01 to 100 μm;

[0019] 1,000 to 20,000 parts by mass of (C) gallium or a gallium alloy having a melting point of -20 to 100°C; and

[0020] 0.1 to 100 parts by mass of (D) an alkoxysilane compound represented by the following general formula (1),

[0021] R 1 a R 2 b Si(OR 3 ) 4-a-b (1)

[0022] In formula (1), R 1 are independently an alkyl group having 6 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, R 3 are independently an alkyl group having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and the sum of a+b is an integer of 1 to 3.

[0023] Such a thermally conductive silicone composition has excellent thermal conductivity and moisture resistance.

[0024] Furthermore, in the present invention, it is preferred that the component (A) does not contain an alkenyl group.

[0025] Such a thermally conductive silicone composition has excellent heat resistance.

[0026] Furthermore, in the present invention, it is preferred that the component (B) is at least one selected from the group consisting of zinc oxide powder, aluminum oxide powder, boron nitride powder, aluminum nitride powder, aluminum hydroxide powder, and magnesium oxide powder.

[0027] Such a thermally conductive silicone composition can further improve thermal conductivity.

[0028] In the present invention, it is preferred that the component (A) is an organopolysiloxane represented by the following average composition formula (2):

[0029] R 4 c SiO (4-c) / 2 (2)

[0030] In formula (2), R 4 It does not contain an alkenyl group and is independently a monovalent hydrocarbon group having 1 to 18 carbon atoms and being unsubstituted or substituted, and 1.8≤c≤2.2.

[0031] Such a thermally conductive silicone composition can have good fluidity.

[0032] In the present invention, it is preferred that the component (A) contains a hydrolyzable group-containing organopolysiloxane represented by the following general formula (3) in an amount of 10 to 100% by mass relative to the total mass of the component (A).

[0033] [Chemical formula 1]

[0034]

[0035] In formula (3), R 5 is an alkyl group having 1 to 6 carbon atoms, R 6 The alkylene radicals do not contain an alkenyl group and are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, and d is an integer of 5 to 120.

[0036] As long as it is such a thermally conductive silicone composition, the powder can be highly filled in the silicone composition.

[0037] Furthermore, in the present invention, it is preferred that the gallium alloy of the component (C) is at least one selected from the group consisting of a Ga-In alloy, a Ga-Sn-Zn alloy, a Ga-In-Sn alloy, and a Ga-In-Bi-Sn alloy.

[0038] Such a thermally conductive silicone composition can be made into a thermally conductive silicone composition with excellent workability in the composition preparation step.

[0039] (III) Beneficial effects

[0040] As described above, the thermally conductive silicone composition of the present invention can be a thermally conductive silicone composition having excellent thermal conductivity and moisture resistance. The silicone composition can be suitably used as a heat dissipation grease. DETAILED DESCRIPTION

[0041] As described above, there is a need to develop a thermally conductive silicone composition having excellent thermal conductivity and moisture resistance.

[0042] The inventors of the present application have conducted intensive studies to achieve the above-mentioned purpose, and as a result, have found that excellent thermal conductivity and moisture resistance can be exhibited by mixing a thermally conductive filler with a low melting point metal having a melting point of -20 to 100°C and a specific alkoxysilane compound in a suitable ratio in a specific organic polysiloxane, thereby completing the present invention.

[0043] That is, the present invention is a thermally conductive silicone composition comprising the following components (A) to (D):

[0044] 100 parts by mass of (A) having a kinematic viscosity at 25°C of 10 to 500,000 mm 2 / s of organopolysiloxane;

[0045] 10 to 2,000 parts by mass of (B) a thermally conductive filler having an average particle size of 0.01 to 100 μm;

[0046] 1,000 to 20,000 parts by mass of (C) gallium or a gallium alloy having a melting point of -20 to 100°C; and

[0047] 0.1 to 100 parts by mass of (D) an alkoxysilane compound represented by the following general formula (1),

[0048] R 1 a R 2 b Si(OR 3 ) 4-a-b (1)

[0049] In formula (1), R 1 are independently an alkyl group having 6 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, R 3 are independently an alkyl group having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and the sum of a+b is an integer of 1 to 3.

[0050] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.

[0051] <Thermal Conductive Silicone Composition>

[0052] The thermally conductive silicone composition of the present invention contains the following components (A) to (D), and can be suitably used as, for example, a heat dissipation paste.

[0053] (A)Ingredients

[0054] (A) The kinematic viscosity of the component at 25°C is 10 to 500,000 mm 2 / s, preferably 30~100,000mm 2 / s, more preferably 50 to 10,000 mm 2 / s of organopolysiloxane. If the kinematic viscosity of the organopolysiloxane is lower than the above lower limit, oil bleeding is likely to occur when the paste is made. In addition, if it is greater than the above upper limit, the organosilicon composition will lack ductility, which is not preferred. In addition, in the present invention, the kinematic viscosity of the organopolysiloxane is a value measured at 25°C using an Ostwald viscometer.

[0055] In the present invention, the organopolysiloxane of component (A) can be any organopolysiloxane known in the past as long as it has the above-mentioned kinematic viscosity. The molecular structure of the organopolysiloxane is not particularly limited, and it can be any of linear, branched, and cyclic structures. In particular, it can have a linear structure in which the main chain is composed of repeated diorganosiloxane units and the molecular chain ends are capped with triorganosiloxy groups. The above-mentioned organopolysiloxane can be a single species or a combination of two or more species. In addition, from the perspective of heat resistance, it is preferred that component (A) does not contain alkenyl groups.

[0056] The organopolysiloxane of the component (A) may be an organopolysiloxane represented by the following average composition formula (2).

[0057] R 4 c SiO (4-c) / 2 (2)

[0058] In formula (2), R 4 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and 1.8≤c≤2.2.

[0059] In the above general formula (2), R 4 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 14 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; or groups in which some or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, bromine, and chlorine, cyano, etc., for example, 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, p-chlorophenyl, etc. Methyl and phenyl are preferred.

[0060] In the general formula (2), c is a number in the range of 1.8 to 2.2, and is particularly preferably a number in the range of 1.9 to 2.1. When c is in the above range, the obtained thermally conductive silicone composition can have good fluidity.

[0061] As the organopolysiloxane represented by the average composition formula (2), a linear organopolysiloxane represented by the following general formula (4) is preferred.

[0062] [Chemical formula 2]

[0063]

[0064] In the above general formula (4), R 7 does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 14 carbon atoms. Examples of the monovalent hydrocarbon group include the above-mentioned R 4 Among them, it is preferred that R 7 are all methyl groups. m is the kinematic viscosity of the organopolysiloxane at 25°C of 10 to 500,000 mm 2 / s, preferably 30~100,000mm 2 / s, more preferably 50~10,000mm 2 / s.

[0065] Specific examples include the following components.

[0066] [Chemical formula 3]

[0067]

[0068] In addition, the component (A) may contain the organopolysiloxane represented by the above average composition formula (4) and the organopolysiloxane having a hydrolyzable group represented by the following general formula (3). The content of the hydrolyzable organopolysiloxane represented by the following general formula (3) in the component (A) is preferably 10 to 100% by mass, more preferably 30 to 95% by mass, and even more preferably 50 to 90% by mass, relative to the total mass of the component (A).

[0069] [Chemical formula 4]

[0070]

[0071] (In general formula (3), R 5 is an alkyl group having 1 to 6 carbon atoms, R 6 does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and d is an integer of 5 to 120).

[0072] The organopolysiloxane represented by the general formula (3) can assist in highly filling the powder in the silicone composition. Furthermore, the silicone composition contains the organopolysiloxane, and the surface of the powder is covered by the organopolysiloxane, which makes it difficult for the powders to aggregate with each other. This effect lasts even at high temperatures, so the heat resistance of the silicone composition is improved. In addition, the surface of the powder can also be hydrophobized using the organopolysiloxane represented by the general formula (3).

[0073] In the above general formula (3), R 5 is an alkyl group having 1 to 6 carbon atoms. Examples thereof include alkyl groups having 1 to 6 carbon atoms such as methyl, ethyl, and propyl, and methyl and ethyl are particularly preferred. 6 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl and octadecyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; or groups in which some or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine, bromine, chlorine, or cyano, such as 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, p-chlorophenyl, etc. Methyl is particularly preferred. In the above general formula (3), d is preferably an integer of 5 to 120, and more preferably an integer of 10 to 90. In addition, d is a compound of the general formula (3) satisfying a kinematic viscosity at 25° C. of 10 to 500,000 mm 2 / s, preferably 30~100,000mm 2 / s value.

[0074] Specific examples of the organopolysiloxane having a hydrolyzable group include the following components.

[0075] [Chemical formula 5]

[0076]

[0077] (B) Ingredients

[0078] (B) component is a thermally conductive filler. The type of thermally conductive filler is not particularly limited, and the powder used for heat dissipation (thermal conductivity) paste in the past can be used. In particular, it can be a component with high thermal conductivity, preferably selected from at least one or more of zinc oxide powder, aluminum oxide powder, boron nitride powder, aluminum nitride powder, aluminum hydroxide powder, and magnesium oxide powder. These thermally conductive fillers (inorganic compound powders) can be used as needed and the surface of which is hydrophobized using organosilane, organosilazane, organopolysiloxane, organic fluorine compound, etc. The thermally conductive filler. Hydrophobization can be carried out using the organopolysiloxane represented by the above-mentioned general formula (3).

[0079] The average particle size of the thermally conductive filler is 0.01 to 100 μm, more preferably 0.1 to 80 μm, and further preferably 0.5 to 50 μm. Whether the average particle size of the thermally conductive filler is less than the above lower limit or greater than the above upper limit, the filling rate of the obtained silicone composition cannot be increased, so it is not preferred. These thermally conductive fillers can be used alone or in combination of two or more with different average particle sizes. The above average particle size is the cumulative average diameter based on volume. The average particle size can be measured using a particle size distribution meter manufactured by NIKKISO CO., LTD, namely Microtrac MT3300EX.

[0080] The amount of the thermally conductive filler added relative to 100 parts by mass of component (A) may be in the range of 10 to 2,000 parts by mass, more preferably in the range of 50 to 1,500 parts by mass, and further preferably in the range of 100 to 1,000 parts by mass. When the amount is less than the above lower limit, the silicone composition cannot be given a sufficient thermal conductivity. In addition, when the amount exceeds the above upper limit, the viscosity of the silicone composition becomes high and difficult to handle. Therefore, whether the amount is less than the above lower limit or greater than the above upper limit, it is difficult to make a grease-like silicone composition.

[0081] (C) Ingredients

[0082] The component (C) of the present invention is gallium or a gallium alloy, and its melting point needs to be in the range of -20 to 100°C. If it is lower than -20°C, it is difficult to manufacture, so it is not preferred in terms of economy. If it is higher than 100°C, it cannot be quickly melted in the preparation process of the composition, resulting in poor operability, and it will precipitate and become uneven during manufacturing. Therefore, gallium or gallium alloys with a melting point in the range of -20 to 100°C are in an appropriate range both in terms of economy and the conditions required for processing. It is particularly preferred to be in the range of -10 to 50°C.

[0083] The melting point of metal gallium is 29.8° C. In addition, representative gallium alloys having a melting point in the above range include, for example, gallium-indium alloys such as Ga-In (mass ratio = 75.4:24.6, melting point = 15.7° C.); gallium-tin-zinc alloys such as Ga-Sn-Zn (mass ratio = 82:12:6, melting point = 17° C.); gallium-indium-tin alloys such as Ga-In-Sn (mass ratio = 21.5:16.0:62.5, melting point = 10.7° C.; or, mass ratio = 62.0:25.0:13.0, melting point = 5° C.; mass ratio = 68.5:21.5:10, melting point = -19° C.); gallium-indium-bismuth-tin alloys such as Ga-In-Bi-Sn (mass ratio = 9.4:47.3:24.7:18.6, melting point = 48.0° C.), etc.

[0084] The component (C) may be used alone or in combination of two or more.

[0085] The shape of the liquid particles or solid particles of gallium and its alloys present in the composition of the present invention is generally roughly spherical, but may also include amorphous shapes. In addition, the average particle size is generally 0.1 to 200 μm, and 10 to 100 μm is particularly preferred. As long as the above average particle size is above the above lower limit, the viscosity of the composition will not become too high, the ductility is excellent, and therefore the coating operability is excellent, and on the contrary, as long as it is below the above upper limit, it will not separate. In addition, since the present composition will retain an appropriate viscosity, the dispersed state of the particles of the above shape and average particle size can be maintained even when stored at room temperature.

[0086] In addition, the particle size of the component (C) is a numerical value of the average particle size that is automatically measured by automatically measuring the area based on the image binarization after the image of the particles to be measured is photographed with a microscope. For example, it can be measured using a microscope VHX-8000 manufactured by KEYENCE CORPORATION. The particles to be measured can be clamped between two slides and then photographed with a microscope, and the average particle size can be automatically measured using the attached image processing function (automatic area measurement based on image binarization).

[0087] Relative to 100 parts by mass of the above-mentioned (A) component, the blending amount of the (C) component is 1,000 to 20,000 parts by mass, preferably 2,000 to 15,000 parts by mass, and more preferably 3,000 to 10,000 parts by mass. If the above-mentioned blending amount is less than 1,000 parts by mass, the thermal conductivity will be lowered, and when the composition is thicker, sufficient heat dissipation function cannot be obtained. If it is more than 20,000 parts by mass, it is difficult to make a uniform composition, the viscosity of the composition will be too high, and there is a problem that a paste composition with ductility cannot be obtained.

[0088] (D) Ingredients

[0089] Component (D) can not only assist in highly filling the silicone composition of the present invention with powder, but also improve the moisture resistance of component (C). Gallium and gallium alloys themselves have the disadvantage of continuously oxidizing if exposed to high humidity for a long time, which results in an increase in the thermal resistance of the silicone composition. However, by including component (D), the increase in thermal resistance is not found even under high humidity, and the performance can be maintained.

[0090] (D) The component is an alkoxysilane compound represented by the following general formula (1).

[0091] R 1 a R 2 b Si(OR 3 ) 4-a-b (1)

[0092] (In formula (1), R 1 are independently an alkyl group having 6 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, R 3 are independently an alkyl group having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and the sum of a+b is an integer of 1 to 3).

[0093] R 1 Each of the groups is independently an alkyl group having 6 to 20 carbon atoms, preferably an alkyl group having 10 to 20 carbon atoms, and more preferably an alkyl group having 16 to 20 carbon atoms.

[0094] As R in the above general formula 1 , for example, hexyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, nonadecyl, eicosyl, etc. Preferably, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, more preferably hexadecyl, octadecyl, eicosyl.

[0095] If the number of carbon atoms is less than 6, the wettability of the above-mentioned components (B) and (C) will not be sufficiently improved. If it is 21 or more, the organosilane will be cured at room temperature, which will not only be inconvenient to handle, but also the low-temperature characteristics of the obtained composition will be reduced. In order to improve moisture resistance, the number of carbon atoms is preferably 10 to 20, and particularly preferably 16 to 20.

[0096] In addition, as the above R 2, independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, preferably 1 to 8 carbon atoms, for example: alkyl groups such as methyl, ethyl, propyl, hexyl, and octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(nonafluorobutyl)ethyl, 2-(heptadecafluorooctyl)ethyl, and p-chlorophenyl. Among them, methyl and ethyl are preferred.

[0097] In addition, as the above R 3 , are independently alkyl groups having 1 to 6 carbon atoms, and examples thereof include methyl, ethyl, propyl, butyl, pentyl, hexyl and the like. Among them, methyl and ethyl are particularly preferred.

[0098] As suitable specific examples of the component (D), the following compounds can be mentioned.

[0099] C6H 13 Si(OCH3)3

[0100] C 12 H 25 Si(OCH3)3

[0101] C 10 H 21 Si(CH3)(OCH3)2

[0102] C 10 H 21 Si(C6H5)(OCH3)2

[0103] C 10 H 21 Si(CH3)(OC2H5)2

[0104] C 10 H 21 Si(CH=CH2)(OCH3)2

[0105] C 10 H 21 Si(CH2CH2CF3)(OCH3)2

[0106] C 10 H 21 Si(OCH3)3

[0107] C 12 H 25 Si(OC2H5)3

[0108] C 16 H 33 Si(OCH3)3

[0109] C 18 H 37 Si(OCH3)3

[0110] C 20 H 41 Si(OCH3)3

[0111] C 18 H 37 Si(OC2H5)3

[0112] In addition, this (D) component can be used alone as one, and can also be used in combination as two or more. In addition, relative to 100 parts by mass of (A) component, its admixture is 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, and further preferably 10 to 50 parts by mass. If the above-mentioned admixture is too much, the moisture resistance improvement effect will not increase and is uneconomical, and it is slightly volatile, so if placed in an open system, there may be a situation where the composition of the present invention gradually hardens. In addition, if the above-mentioned admixture is too little, it is impossible to fully prevent the progress of oxidation, and the numerical value of thermal resistance will deteriorate.

[0113] (Other ingredients)

[0114] Furthermore, the silicone composition of the present invention can be blended with a conventionally known antioxidant, dye, pigment, flame retardant, anti-settling agent, thixotropy enhancer, etc. in an amount that meets the target as needed.

[0115] The method for manufacturing the thermally conductive silicone composition of the present invention can be based on the method for manufacturing the silicone paste composition known in the past, and there is no particular limitation. For example, it can be manufactured by the following method: using a mixer such as TRIMIX, TWINMIX, PLANETARY MIXER (all mixers manufactured by Inoue Manufacturing Co., Ltd., registered trademarks); ULTRAMIXER (mixer manufactured by Mizuho Industrial Co., Ltd., registered trademark); HIVIS DISPER MIX (mixer manufactured by Tokushu Kikai Kogyo Co., Ltd., registered trademark) to mix the above-mentioned (A) to (D) components and other components as needed for 30 minutes to 4 hours. When the (C) component is solid at room temperature, it is ideal to dissolve the (C) component in advance with a heating furnace, etc., and then blend it. In addition, as needed, it can be mixed while heating at a temperature in the range of 50 to 150°C.

[0116] The absolute viscosity of the thermally conductive silicone composition of the present invention measured at 25°C is preferably 10 to 500 Pa·s, more preferably 30 to 450 Pa·s, and further preferably 50 to 400 Pa·s. As long as the absolute viscosity is below the above upper limit, the operability will become good, and as long as the absolute viscosity is above the above lower limit, the composition will not flow out after being applied to various substrates, and a good paste can be provided. The above absolute viscosity can be obtained by preparing each component in the above blending amount. The above absolute viscosity can be measured using model PC-1TL (10 rpm) manufactured by Malcom.

[0117] The thermally conductive silicone composition of the present invention may have a high thermal conductivity of preferably 3.0 W / mK or more, more preferably 4.0 W / mK or more, and further preferably 5.0 W / mK or more at 25°C.

[0118] In addition, the thermally conductive silicone composition of the present invention exhibits the property that the thermal resistance value does not increase even after being placed under high temperature and high humidity. Specifically, the thermal resistance value after exposure to 130°C / 85%RH for 100 hours is no more than twice that of the initial value, so it can be said that the reliability is high under high temperature and high humidity.

[0119] The thermally conductive silicone composition of the present invention can be used as a paste. There is no particular limitation on the method of using the thermally conductive silicone composition of the present invention as a paste, as long as it is used in the same way as the conventional heat dissipation (thermal conductive) silicone paste. For example, it can be suitable for clamping the paste between electrical and electronic components such as LSI (large-scale integration) or other heat-generating components and cooling components or heat-dissipating components, transferring heat from the heat-generating components to the cooling components or heat-dissipating components and dissipating the heat. The thermally conductive silicone composition of the present invention has low viscosity, high thermal conductivity and extremely excellent moisture resistance, and therefore can be suitable for use as a heat dissipation (thermal conductive) paste for semiconductor devices of high-quality models and the like.

[0120] [Example]

[0121] Hereinafter, the present invention will be described in more detail using Examples and Comparative Examples, but the present invention is not limited thereto.

[0122] (A)Ingredients

[0123] (A-1) Both ends are capped with trimethylsilyl groups and the kinematic viscosity at 25°C is 1,000 mm 2 / s of dimethyl polysiloxane.

[0124] (A-2) Both ends are capped with trimethylsilyl groups and the kinematic viscosity at 25°C is 5,000 mm 2 / s of dimethyl polysiloxane.

[0125] (A-3) Kinematic viscosity at 25°C is 35 mm 2 / s and an organopolysiloxane represented by the following formula (7).

[0126] [Chemical formula 6]

[0127]

[0128] (B) Ingredients

[0129] (B-1) Zinc oxide powder: average particle size 1.0 μm

[0130] (B-2) Alumina powder: average particle size 8.9 μm

[0131] (B-3) Boron nitride powder: average particle size 2.0 μm

[0132] (B-4) Aluminum nitride powder: average particle size 6.8 μm

[0133] (B-5) Aluminum hydroxide powder: average particle size 25 μm

[0134] (B-6) Magnesium oxide powder: average particle size 45 μm

[0135] <Particle size measurement>

[0136] The particle size of the thermally conductive filler (component (B)) is measured by using a volume-based cumulative average diameter measured by a particle size distribution analyzer, Microtrac MT3300EX, manufactured by NIKKISO CO., LTD.

[0137] (C) Ingredients

[0138] (C-1) Metal Gallium (melting point = 29.8°C)

[0139] (C-2) Ga-In alloy (mass ratio = 75.4:24.6, melting point = 15.7°C)

[0140] (C-3) Ga-In-Sn alloy (mass ratio = 62.0:25.0:13.0, melting point = 5°C)

[0141] (C-4) Ga-In-Sn alloy (mass ratio = 68.5:21.5:10, melting point = -19°C)

[0142] (C-5) Metal Indium (Melting Point = 156.2°C) <For Comparison>

[0143] (D) Ingredients

[0144] (D-1)C 10H 21 Si(OCH3)3

[0145] (D-2)C 16 H 33 Si(OCH3)3

[0146] (D-3)C 18 H 37 Si(OCH3)3

[0147] (D-4) CH3Si(OCH3)3<for comparison>

[0148] [Examples 1 to 7 and Comparative Examples 1 to 8]

[0149] Preparation of silicone composition

[0150] The above components (A) to (D) were placed in a 5-liter planetary mixer (PLANETARY MIXER) (manufactured by Inoue Manufacturing Co., Ltd., registered trademark) according to the compositions and blending amounts shown in Tables 1 and 2 below, and stirred at room temperature for 1 hour to prepare a silicone composition.

[0151] In addition, (C-1) and (C-5) having a melting point higher than room temperature are melted in a heating furnace before being charged.

[0152] <Measurement of Viscosity>

[0153] The absolute viscosity of the composition at 25° C. was measured using a model PC-1TL (10 rpm) manufactured by Malcom.

[0154] <Measurement of Thermal Conductivity>

[0155] The thermal conductivity was measured at 25° C. using TPS-2500S manufactured by Kyoto Electronics Manufacturing Co., Ltd.

[0156] <Measurement of Particle Size of Gallium or Alloy in Composition>

[0157] The composition was sandwiched between two microscopes and photographed with a microscope VHX-8000 manufactured by KEYENCE CORPORATION, and the average particle size was automatically measured using an attached image processing function (automatic area measurement by image binarization).

[0158] <Thickness of Composition>

[0159] Each composition obtained above (excluding Comparative Examples 1, 2, 4, 6, and 7) was applied to the entire surface of a standard aluminum plate (diameter 1.26 mm, thickness 1.0 mm), and overlapped with another standard aluminum plate from above, and the composition was pressed for 15 minutes with a load of 2 kgf. In addition, the thickness of each composition was calculated by subtracting the thickness of the two standard aluminum plates from the thickness of the entirety (the thickness of the two aluminum plates and the composition).

[0160] The thickness of the aluminum plate and the thickness of the composition were measured using a micrometer (manufactured by Mitutoyo Corporation, model: M820-25VA).

[0161] <Thermal resistance measurement>

[0162] The thermal resistance (mm) of each composition was measured using the thermal resistance sample and a thermal resistance measuring device (Model: LFA447 manufactured by NETZSCH-Geratebau GmbH). 2 ・K / W).

[0163] The thermal resistance was measured immediately after the thermal resistance sample was prepared and after the thermal resistance sample was exposed to 130°C / 85%RH for 100 hours using a highly accelerated life tester (model: EHS-212M) manufactured by ESPEC Corp.

[0164] As a judgment, the sample whose thermal resistance value after exposure to 130°C / 85%RH for 100 hours is more than twice that of the initial value can be said to have low reliability under high temperature and high humidity.

[0165] [Table 1]

[0166]

[0167] [Table 2]

[0168]

[0169] According to the results in Table 1, the thermally conductive silicone composition of the present invention exhibits high thermal conductivity and sufficiently low thermal resistance, and even though the thermal resistance after being placed under high temperature and high humidity changes compared to before being placed under high temperature and high humidity, it is still sufficiently low, about 1.13 times. On the other hand, in Comparative Examples 1, 2, 4, 6, and 7, it was impossible to make a paste. In addition, the thermal conductivity of Comparative Example 3 was not sufficient. Furthermore, in Comparative Examples 5 and 8, although the thermal conductivity itself was sufficient, the thermal resistance after being placed under high temperature and high humidity increased to 20 times and about 16 times, respectively.

[0170] This manual contains the following protocols.

[0171] [1] A thermally conductive silicone composition comprising the following components (A) to (D):

[0172] 100 parts by mass of (A) having a kinematic viscosity at 25°C of 10 to 500,000 mm 2 / s of organopolysiloxane;

[0173] 10 to 2,000 parts by mass of (B) a thermally conductive filler having an average particle size of 0.01 to 100 μm;

[0174] 1,000 to 20,000 parts by mass of (C) gallium or a gallium alloy having a melting point of -20 to 100°C; and

[0175] 0.1 to 100 parts by mass of (D) an alkoxysilane compound represented by the following general formula (1),

[0176] R 1 a R 2 b Si(OR 3 ) 4-a-b (1)

[0177] (In formula (1), R 1 are independently an alkyl group having 6 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, R 3 are independently an alkyl group having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and the sum of a+b is an integer of 1 to 3).

[0178] [2] The thermally conductive silicone composition according to [1] above, wherein the component (A) does not contain an alkenyl group.

[0179] [3] The thermally conductive silicone composition according to [1] or [2], wherein the component (B) is one or more selected from zinc oxide powder, aluminum oxide powder, boron nitride powder, aluminum nitride powder, aluminum hydroxide powder, and magnesium oxide powder.

[0180] [4] The thermally conductive silicone composition according to any one of [1] to [3] above, wherein the component (A) is an organopolysiloxane represented by the following average composition formula (2):

[0181] R 4 c SiO (4-c) / 2 (2)

[0182] (In formula (2), R 4does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and 1.8≤c≤2.2).

[0183] [5] The thermally conductive silicone composition according to any one of [1] to [4] above, wherein the component (A) contains a hydrolyzable group-containing organopolysiloxane represented by the following general formula (3) in an amount of 10 to 100% by mass relative to the total mass of the component (A),

[0184] [Chemical formula 7]

[0185]

[0186] (In formula (3), R 5 is an alkyl group having 1 to 6 carbon atoms, R 6 does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and d is an integer of 5 to 120).

[0187] [6] The thermally conductive silicone composition as described in any one of [1] to [5] above, characterized in that the gallium alloy of the component (C) is one or more selected from the group consisting of Ga-In alloy, Ga-Sn-Zn alloy, Ga-In-Sn alloy, and Ga-In-Bi-Sn alloy.

[0188] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any configuration that is substantially the same as the technical concept described in the claims of the present invention and that can achieve the same effects is included in the technical scope of the present invention.

Claims

1. A thermally conductive silicone composition, characterized in that: Contains the following ingredients (A) to (D): 100 parts by mass of (A) having a kinematic viscosity at 25°C of 10 to 500,000 mm 2 / s of organopolysiloxane; 10 to 2,000 parts by mass of (B) a thermally conductive filler having an average particle size of 0.01 to 100 μm; 1,000 to 20,000 parts by mass of (C) gallium or a gallium alloy having a melting point of -20 to 100°C; and 0.1 to 100 parts by mass of (D) an alkoxysilane compound represented by the following general formula (1), R 1 a R 2 b Si(OR 3 ) 4-a-b (1) In formula (1), R 1 are independently an alkyl group having 6 to 20 carbon atoms, R 2 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, R 3 Each of the groups is independently an alkyl group having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and the sum of a+b is an integer of 1 to 3.

2. The thermally conductive silicone composition according to claim 1, characterized in that: The component (A) does not contain an alkenyl group.

3. The thermally conductive silicone composition according to claim 1, characterized in that: The component (B) is at least one selected from the group consisting of zinc oxide powder, aluminum oxide powder, boron nitride powder, aluminum nitride powder, aluminum hydroxide powder, and magnesium oxide powder.

4. The thermally conductive silicone composition according to claim 2, characterized in that: The component (B) is at least one selected from the group consisting of zinc oxide powder, aluminum oxide powder, boron nitride powder, aluminum nitride powder, aluminum hydroxide powder, and magnesium oxide powder.

5. The thermally conductive silicone composition according to claim 1, characterized in that: The component (A) is an organopolysiloxane represented by the following average composition formula (2), R 4 c SiO (4-c) / 2 (2) In formula (2), R 4 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and 1.8≤c≤2.

2.

6. The thermally conductive silicone composition according to claim 2, characterized in that: The component (A) is an organopolysiloxane represented by the following average composition formula (2), R 4 c SiO (4-c) / 2 (2) In formula (2), R 4 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and 1.8≤c≤2.

2.

7. The thermally conductive silicone composition according to claim 3, characterized in that: The component (A) is an organopolysiloxane represented by the following average composition formula (2), R 4 c SiO (4-c) / 2 (2) In formula (2), R 4 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and 1.8≤c≤2.

2.

8. The thermally conductive silicone composition according to claim 4, characterized in that: The component (A) is an organopolysiloxane represented by the following average composition formula (2), R 4 c SiO (4-c) / 2 (2) In formula (2), R 4 It does not contain an alkenyl group and is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, and 1.8≤c≤2.

2.

9. The thermally conductive silicone composition according to any one of claims 1 to 8, characterized in that: The component (A) contains a hydrolyzable group-containing organopolysiloxane represented by the following general formula (3) in an amount of 10 to 100% by mass relative to the total mass of the component (A). [Chemical formula 1] In formula (3), R 5 is an alkyl group having 1 to 6 carbon atoms, R 6 The alkylene radicals do not contain an alkenyl group and are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, and d is an integer of 5 to 120.

10. The thermally conductive silicone composition according to any one of claims 1 to 8, characterized in that: The gallium alloy of the component (C) is one or more selected from the group consisting of Ga-In alloy, Ga-Sn-Zn alloy, Ga-In-Sn alloy, and Ga-In-Bi-Sn alloy.

11. The thermally conductive silicone composition according to claim 9, characterized in that: The gallium alloy of the component (C) is one or more selected from the group consisting of Ga-In alloy, Ga-Sn-Zn alloy, Ga-In-Sn alloy, and Ga-In-Bi-Sn alloy.

Citation Information

Patent Citations

  • Thermally conductive silicone composition, cured product thereof and method for laying the same, and heat- releasing structure for semiconductor device using the same

    JP2003176414A

  • Heat radiating member and method for manufacturing and for installing the same

    JP2003218296A

  • Heat radiation member, its manufacturing method, and its lay-out method

    JP2004039829A

  • Curable organopolysiloxane composition and semiconductor apparatus

    JP2005112961A

  • Heat-conductive grease composition

    JP2007106809A

Cited By

  • Heat-conducting silicone grease with high reliability and low thermal resistance and preparation method thereof

    CN121293765A