Process and method for separating rare earth elements from leaching solution

By controlling the pH value of the leaching solution and introducing ozone precipitation technology, the separation process of rare earth elements is simplified, the problems of complex steps and high cost in the existing technology are solved, and efficient separation and simplified process of high-purity rare earth elements are achieved.

CN119072549APending Publication Date: 2024-12-03RARE EARTH SALTS SEPARATION & REFINING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035675.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-05
Filing Date
2023-03-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art has complex steps, high cost and difficult to expand to the industrial level in the process of separation of rare earth elements, especially the method of separating individual rare earth elements from medium and heavy rare earth elements from leaching solutions is not simple enough.

Method used

By neutralizing the leaching solution, controlling the pH between 2 and 6, ozone precipitates cerium oxide, and precipitates medium-heavy rare earths and lanthanum elements in different pH ranges, followed by treatment with precipitant to produce high-purity rare earth precipitates, simplifying the Process and improve purity.

Benefits of technology

It has achieved efficient separation of high-purity rare earth elements, especially medium and heavy rare earth elements, from the leaching solution, simplified the process flow, reduced costs, and increased global rare earth production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072549A_ABST
    Figure CN119072549A_ABST
Patent Text Reader

Abstract

An improved process for separating individual rare earths and / or sets of rare earth elements from a rare earth-containing leach solution to produce a high purity material for further refining. According to a first preferred embodiment, the invention comprises a method comprising the steps of: neutralizing a leach solution; introducing ozone into the solution while controlling the pH, and precipitating cerium oxide; removing precipitated cerium oxide from the solution; in the presence of ozone, adjusting the pH of the solution to precipitate medium / heavy rare earth; removing the precipitated rare earth concentrate from the solution; treating the remaining solution with a precipitating agent to produce a high purity lanthanum precipitate; and removing solids from the solution.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims priority to U.S. Provisional Application No. 63 / 327,477, filed on April 5, 2022. Technical Field

[0003] The present invention relates to the separation of rare earth elements (REEs). More particularly, the present invention relates to a method for separating rare earth elements from rare earth deposits, leaching solutions and concentrates containing the rare earth elements. Background Art

[0004] Rare earth elements mainly include the lanthanides of the periodic table, but also include scandium and yttrium. Exemplary rare earth elements include: lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (ET), thulium (Tm), ytterbium (Mb), lutetium (Lu), scandium (Sc) and yttrium (Y). Rare earth elements can be divided into light rare earth elements, medium rare earth elements and / or heavy rare earth elements. Exemplary light rare earth elements include La, Ce, PC and Nd. Exemplary medium rare earth elements include Sm, Eu and Gd, also known as SEG. Exemplary heavy rare earth elements include Sc, Tb, Dy, Ho, Er, Tm, Yb, Lu and Y.

[0005] Many of the world's known rare earth mineral resources are composed of light rare earth elements, which account for between 90% and 95% of the total rare earth weight, and medium rare earth elements, which account for about 5% of the total rare earth weight. Many deposits contain less than 1% of the total rare earth content in terms of heavy rare earths.

[0006] The related art discloses a number of different rare earth element extraction methods and apparatus. Some of the methods currently used can be very complex because they require a large number of steps to separate the raw materials into individual elements at high purity. This results in very costly and difficult to deploy processes. Other methods have proven difficult to scale up to an industrial level. If the complexity of the overall process or the amount of material to be processed could be significantly reduced, it might be possible to deploy some of these methods more easily.

[0007] Bauer et al., in "Recovery of Cerium and Lanthanum by Ozonation of Lanthanide Solutions", disclose a process comprising oxidizing a mixed lanthanide solution with ozone at pH 45 and ambient temperature to precipitate 98% of the original cerium present. The corresponding cerium purity is increased from 50% to 98%. A second ozone oxidation precipitation step yields a high yield of 99.9% pure cerium from the 98% pure material.

[0008] Alternatively, ozone treatment at pH 6.5 and 850°C allows cerium and rare earth elements heavier than cerium to be precipitated differently, leaving 89% of the original lanthanum in solution at 95% purity. The precipitate is then dissolved in dilute mineral acid and reoxidized with ozone at pH 4.5 and ambient temperature to recover cerium from the heavier rare earth elements in the precipitate. The filtrate contains an enriched praseodymium-neodymium-samarium-europium mixture that can be separated by ion exchange or solvent extraction.

[0009] W02016 / 058007 discloses a method for selectively separating rare earth elements, which includes the following steps: digesting rare earth oxide powder in nitric acid to form a first rare earth solution including dissolved rare earth elements; contacting the first rare earth solution with ammonium hydroxide to precipitate a first precipitation product and form a second rare earth solution; separating the first precipitation product from the second rare earth solution; increasing the pH of the second rare earth solution to precipitate additional rare earth elements from the second rare earth solution as a first intermediate particle feed; digesting the first intermediate particle feed in nitric acid to form a third rare earth solution; and contacting the third rare earth solution with ammonium hydroxide to precipitate a second precipitation product and form a fourth rare earth solution.

[0010] WO2016 / 011540 discloses treating a REE water leachate through a series of purification and precipitation steps to produce high purity mixed rare earth oxides for refining using solvent extraction techniques. An exemplary purification process uses a pH adjustment step, such as using MgO, MgCO3 or Na2CO3, to remove thorium and iron and other minor impurity elements from the solution. In an alternative embodiment, uranium can be removed from the water leach solution by ion exchange. The purified solution can be treated with soda ash to precipitate impure rare earth carbonates. The rare earth carbonates can then be dissolved in hydrochloric acid (or other acids) and the pH adjusted again to precipitate small amounts of remaining iron and thorium. The purified hydrochloric acid leach solution can then be treated with oxalic acid to precipitate all rare earths as mixed rare earth oxalate products. In an alternative embodiment, a two-stage precipitation is provided from a chloride re-leach solution. Two-stage precipitation can be performed to facilitate recovery: (a) a high purity initial precipitate containing, for example, at least 90% rare earths; and (b) a low purity second precipitate for recycling. For example, the second precipitate may be, for example, a carbonate precipitate, which may be returned directly to the re-leaching process together with the mineral acid.

[0011] WO2016 / 025928 discloses a method for extracting and separating rare earth elements, comprising: providing a rare earth-containing ore or tailings; grinding the rare earth-containing ore to form a powdered ore; leaching the powdered ore with at least one mineral acid; forming a leaching solution comprising at least one metal ion, a rare earth element and a solid material; separating the solid material from the leaching solution to form a water metal concentrate; precipitating the water metal concentrate to selectively remove metal ions from the leaching solution and obtain a rare earth element precipitate; heating the rare earth element precipitate in air to form a rare earth element oxide; mixing the rare earth element oxide with an ammonium salt and heating in dry air / nitrogen; forming an anhydrous rare earth salt mixture in an aqueous solution, and separating the rare earth element from the aqueous solution by an electrodeposition process.

[0012] Prior art methods, while useful in certain situations, are cumbersome and require numerous steps and reagents.Therefore, there is a need for an improved method for separating rare earth elements from a leach solution. Summary of the invention

[0013] Based on the above, it should be apparent that there is a great need for an improved method of separating individual rare earth elements and / or groups of rare earth elements from rare earth-containing leach solutions to produce a simple, easily scalable, low-cost process for producing high-purity materials that can be more easily refined. In addition, there is a need for a method specifically adapted to separate light rare earth elements from medium and heavy rare earth elements to increase global rare earth production.

[0014] In a first aspect, the present invention relates to a method for separating rare earth elements, comprising the following steps:

[0015] a. neutralizing a leaching solution, wherein the leaching solution (i) comprises at least two rare earth metal salts and (ii) has a pH preferably between 2 and 6;

[0016] b. introducing ozone into the solution while controlling the pH between 2 and 6, and precipitating cerium oxide having a purity greater than 97% from the solution;

[0017] c. removing the precipitated cerium oxide from the solution;

[0018] d. In the presence of ozone, the pH of the solution is adjusted to between 6.0 and 8.0 to precipitate oxyhydroxides / hydroxides of medium / heavy rare earths, Nd and Pr;

[0019] e. removing the precipitated rare earth concentrate from the solution;

[0020] f. treating the remaining solution with a precipitating agent to produce a high purity lanthanum precipitate; and

[0021] g. Removal of solids from solution.

[0022] In a second aspect, the present invention relates to a method for separating cerium from a leaching solution comprising at least two rare earth metal salts and having a pH of less than 3.

[0023] According to a preferred embodiment, the method may preferably comprise the following steps:

[0024] a. treating the solution with anhydrous ammonia to raise the pH to between 3 and 5;

[0025] b. introducing ozone into the solution while controlling the pH between 3 and 5 by adding anhydrous ammonia and precipitating greater than 90% of cerium oxide from the solution; and

[0026] c. removing the precipitated cerium oxide from the solution;

[0027] In a third aspect, the present invention relates to a method for separating rare earth elements, comprising the following steps:

[0028] a. slurrying a rare earth concentrate (such as a rare earth carbonate or a rare earth oxide) with water and mixing it with an ammonium salt (such as a nitrate, a halide or a sulfate);

[0029] b. treating the slurry with ozone to produce a high purity Ce concentrate (eg, preferably >90% or >95%) and a solution containing other dissolved rare earths;

[0030] c. removing the solid cerium precipitate from a solution containing other dissolved rare earth elements (including La, Nd, Pr, etc.); and

[0031] d. Treating the solution containing other dissolved rare earths by pH adjustment to in turn produce a separated rare earth concentrate that can be processed into high purity rare earth elements.

[0032] BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A block diagram illustrating a first method according to a first preferred embodiment of the present invention is shown.

[0034] Figure 2 A block diagram illustrating a second method according to an alternative preferred embodiment of the present invention is shown. DETAILED DESCRIPTION

[0035] To promote an understanding of the principles of the invention, reference will now be made to the embodiments illustrated in the drawings and specific language will be used to describe these embodiments. However, it should be understood that the scope of the invention is not limited thereto and that changes and further modifications to the illustrated devices will typically occur to those skilled in the art.

[0036] Where the specification describes advantages of an embodiment or other limitations of the prior art, the applicant does not intend to disclaim or deny any potential embodiments covered by the appended claims unless the applicant specifically states that the potential claim scope is "hereby disclaimed or denied." In addition, the terms "embodiments of the invention," "embodiments," or "invention" do not require that all embodiments of the invention include the discussed features, advantages, or modes of operation, nor that it does not include aspects that are suboptimal or disadvantageous in the prior art.

[0037] As used herein, the word "exemplary" means "serving as an example, instance, or illustration." The embodiments described herein are not limiting, but merely exemplary. It should be understood that the described embodiments are not necessarily to be construed as being superior or advantageous over other embodiments. Furthermore, any examples or illustrations given herein should not in any way be considered as restrictions, limitations, or express definitions of any term using such examples or illustrations. Instead, these examples or illustrations should be considered as merely illustrative.

[0038] As used herein, the singular forms "a", "an", and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. In addition, the word "may" is used in a permissive sense (i.e., meaning "possibly"), rather than in a mandatory sense (i.e., meaning "must"). In addition, it should be understood that throughout this disclosure, where a process or method is shown or described, the steps of the method may be performed in any order (i.e., repeatedly, iteratively or simultaneously), and selected steps may be omitted, unless logically required otherwise. It should be further understood that the terms "comprise" and / or "include", when used herein, specify the presence of the features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.

[0039] In addition, any examples or descriptions given herein shall not be considered in any way as a restriction, limitation or explicit definition of any term using these examples or descriptions. On the contrary, these examples or descriptions should be considered as merely illustrative. It will be understood by those of ordinary skill in the art that any term used in these examples or descriptions will include other embodiments that may or may not be attached or given elsewhere in this specification, all of which are included within the scope of the term.

[0040] To minimize limitations found in the prior art, and to minimize other limitations that will become apparent upon reading the specification, preferred embodiments of the present invention may preferably provide a method for separating rare earth elements from rare earth leach solutions and carbonate concentrates.

[0041] Now refer to Figure 1 According to a first preferred embodiment, the process / method of the present invention may start with a rare earth-containing leaching solution. Typically, the source of such a rare earth leaching solution may be an acid digestion of a rare earth-containing concentrate or ore. Preferably, the rare earth leaching solution of the present invention may be formed from an aqueous rare earth salt, the anion of which is a nitrate (NO3 - ), halides (F - , Cl - Br - ,I - ) or sulfate (SO4 - ). Preferably, the mineral acid of the present invention may be in any concentration, and preferably has a pH of less than 4. According to a further preferred embodiment, the pH of the mineral acid may preferably be less than 1.

[0042] According to a further preferred embodiment, the leaching mixture may preferably comprise a leaching solution comprising at least rare earth ions and a solid material. The leaching solution may also comprise at least one metal ion. For example, the at least one metal ion may comprise at least one aluminum ion, at least one zinc ion, at least one copper ion, at least one nickel ion, at least one titanium ion and / or at least one iron ion. Preferably, the leaching solution may be heated to enhance the extraction of rare earths from the rare earth-containing material.

[0043] The rare earth concentrate preferably consists of about 0.1% REO to 100% REO and is digested with a mineral acid, preferably, the mineral acid can be nitric acid, hydrochloric acid, sulfuric acid or acetic acid. The final pH of the digestion is preferably below 4. According to a further preferred embodiment, the final pH of the digestion may preferably be less than 2 or more preferably less than 1. In the first step 102, the pH of the solution may preferably be adjusted. According to a preferred embodiment, the pH may be adjusted to a range between 3 and 5 or between 3 and 6. According to a further preferred embodiment, the adjusted pH of the solution may preferably be less than 5 or more preferably less than 3.

[0044] After the solution is within the target pH range, ozone may be introduced in the next step 104 while controlling the pH to remain between 3 and 6. Preferably, the treatment of the solution precipitates high purity cerium oxide. According to a preferred embodiment, the precipitated high purity cerium oxide is preferably within the range of 90% purity or above. According to a further preferred embodiment, the purity is preferably greater than 95%, and most preferably greater than 97%.

[0045] In the next step 106, the treatment is continued until the cerium is removed from the solution as precipitated cerium. According to alternative preferred embodiments, the removal of cerium can be carried out by any solid-liquid separation method. According to a preferred embodiment, the pH of the solution is then adjusted to between 6.0 and 7.0. At a desired pH, preferably greater than 6, the medium / heavy rare earths are precipitated with Nd and Pr.

[0046] According to a further preferred embodiment, the treatment of the present invention preferably continues until the desired amount of target rare earth (such as medium / heavy rare earth and Nd and Pr) is removed from the solution as a precipitate. In the next step 108, the precipitate / solid can be removed from the solution by a desired solid-liquid separation method.

[0047] In a next step 110, the remaining solution is then preferably treated with a precipitant (such as carbon dioxide, hydroxide or oxalate) or evaporated to produce a high purity lanthanum concentrate. This can preferably produce a concentrate with a lanthanum purity of greater than 95% and more preferably greater than 98%. According to a preferred next step 112, the solid containing La is then preferably removed from the solution by further solid-liquid separation techniques.

[0048] According to a preferred embodiment, the solids produced in the above treatment may be preferably re-digested with mineral acid and reprocessed as described above to produce higher purity rare earth elements in the next step 114. For example, the La concentrate produced may be digested with mineral acid and the resulting solution may be further reprocessed / treated according to the conditions disclosed for the medium / heavy / Nd-Pr stages to further upgrade and purify La.

[0049] Reference now Figure 2 , now discussing the second embodiment. In the first step 202, a rare earth concentrate (such as a rare earth carbonate) can be slurried preferably with water and mixed with an ammonium salt (such as a nitrate, halide or sulfate). The rare earth concentrate can be a mixture of two or more rare earth elements, one of which is Ce. According to a preferred embodiment, in the first step 202, 1 part of carbonate is mixed with 1 to 20 parts of water and 0.5 to 4 parts of ammonium salt with 1 part of rare earth concentrate to form a slurry. In the next step 204, the slurry can then be treated with ozone to produce a high purity cerium concentrate while dissolving other rare earths. In the next step 206, the cerium solids can then be removed by solid-liquid separation techniques. According to a preferred embodiment, in the next step 208, the resulting solution can then be treated preferably in stages with a pH neutralization technique (as described above) to produce a separated rare earth precipitate, which is reprocessed into high purity rare earth elements. Preferably, the pH of the solution is neutralized to between 6.0 and 8.0, most preferably between 6.0 and 7.0.

[0050] In the desired pH range, medium / heavy rare earths (as well as Nd and Pr) are preferably precipitated out while maintaining pH to continue precipitation. According to a preferred embodiment, this treatment is continued until the desired amount of Nd and Pr is consumed from the solution. Subsequently, in the next step 210, the participants / solids are then preferably removed from the solution by solid-liquid separation techniques.

[0051] In a next step 212, the remaining solution is then treated with a precipitant (such as an alkali, carbonate or chelating agent) to produce a high purity lanthanum concentrate. Such a concentrate may contain greater than 95% lanthanum, preferably greater than 98% lanthanum. In a next step 214, the solids are then preferably removed from the solution. In a next step 216, the resulting solids may be re-digested with a mineral acid and reprocessed as described above to produce a higher purity rare earth element.

[0052] The following examples are given for illustration only and should not be construed as limiting the scope of the present invention.

[0053] Embodiment:

[0054] A rare earth concentrate in carbonate form containing 50% Ce, 30% La and 19% Nd-Pr and 1% Sm-Lu is digested in hydrochloric acid to produce a rare earth chloride solution with a final pH of 1. The pH of the solution is adjusted to 3 and ozone is introduced. The pH can then be maintained between 2.5 and 6 until the desired amount of Ce is removed from the solution at the desired purity (preferably 95%-98%). Solids including cerium are then preferably removed from the solution. The remaining dissolved rare earths can preferably be further processed by adjusting the pH to a value between 6-8, so that the medium and heavy rare earths are preferentially precipitated with NdPr. This medium / heavy / Nd-Pr concentrate can preferably be removed from the solution by solid-liquid separation. According to a preferred embodiment, the remaining leaching solution should preferably contain only high-purity La (preferably greater than 97%). This material can then be further precipitated to produce high-purity La compounds.

[0055] Subsequently, if the desired Nd-Pr, La or Ce purity is not achieved, the purified material can be digested with hydrochloric acid and the pH treatment repeated as described above to target the specific impurity element. By this method, purities as high as 99.9% can be achieved.

[0056] Although the above description of the present invention contains many features, it should not be understood as a limitation on the scope, but rather as an example. Many other variations are possible. Therefore, the scope of the present invention should not be determined by the illustrated embodiments, but by the appended claims and their legal equivalents.

Claims

1. A method for separating rare earth elements, The following steps are involved: a. Treating the leachate solution; wherein the leaching solution comprises at least two rare earth metal salts; wherein the leachate solution is treated by a neutralization process to bring the pH to between 2 and 6; b. introducing ozone into the solution while controlling the pH between 2 and 6, and precipitating cerium oxide from the solution; c. removing the precipitated cerium oxide from the solution; d. removing solids from the solution containing the remaining rare earth elements; e. adjusting the pH of the solution to between 6.0 and 8.0 to precipitate medium / heavy rare earths and hydroxides of Nd and Pr; f. removing the precipitated Nd-Pr and medium / heavy rare earth from the solution; g. treating the remaining solution with a precipitant or evaporating it to produce a high purity lanthanum concentrate; and h. removing the precipitated solid from the solution.

2. The method according to claim 1, further comprising: include: The solid produced in step (h) is re-digested with a mineral acid and reprocessed according to steps (a) to (h).

3. The method of claim 1, wherein the rare earth leaching solution comprises an aqueous rare earth salt.

4. The method according to claim 3, wherein the aqueous rare earth salt is a nitrate (NO 3 - ), halides or sulfates (SO 4 2- ).

5. The method according to claim 1, further comprising: The following steps are involved: The rare earth-containing material is digested with at least one mineral acid to form the leach solution of step (a).

6. The method of claim 5, wherein the pH of the at least one mineral acid is less than 1.

7. The method according to claim 1, wherein the rare earth leaching solution of step (a) further comprises solid materials.

8. The method of claim 1, wherein the rare earth leaching solution of step (a) further comprises at least one non-rare earth metal ion.

9. The method of claim 8, wherein the non-rare earth metal ions comprise non-rare earth metal ions selected from the group consisting of non-rare earth metal ions including aluminum, zinc, copper, nickel, titanium, and iron.

10. The method according to claim 5, further comprising: The following steps are involved: The leaching solution is heated to enhance extraction of the rare earths from the rare earth-containing material.

11. The method of claim 1, wherein the purity of the cerium oxide is greater than 90%.

12. A method for separating cerium from a leaching solution comprising at least two rare earth metal salts and having a pH of less than 3, wherein the method include: a. adjusting the pH of the solution to increase the pH to between 3 and 5; b. introducing ozone into the solution while controlling the pH between 3 and 5; c. precipitating cerium oxide from the solution; as well as d. removing the precipitated cerium oxide from the solution.

13. A method for separating rare earth elements, The following steps are involved: a. The rare earth concentrate is slurried; wherein 1 part of carbonate is mixed with 1 to 20 parts of water and 0.5 to 4 parts of ammonium salt and 1 part of rare earth concentrate to form a slurry; b. treating the slurry with ozone to produce a high purity cerium concentrate and a solution containing other dissolved rare earths; c. removing cerium solids from the solution containing other dissolved rare earth elements; as well as d. The solution containing other dissolved rare earths is sequentially subjected to pH adjustment to produce a separated rare earth concentrate that can be processed into high purity rare earth elements.

14. The method of claim 13, wherein the rare earth concentrate comprises rare earth carbonates or rare earth oxides.

15. The method of claim 14, wherein the ammonium salt is a nitrate, a halide or a sulfate.

16. The method of claim 15, wherein the ammonium salt comprises an aqueous solution of ammonium chloride.

17. The method of claim 16, wherein the step of treating the solution comprises adjusting the pH to between 6.0 and 7.

0.

18. The method according to claim 17, wherein the method further comprises The following steps are involved: In the pH range of 6 to 8, medium / heavy rare earths, neodymium and praseodymium are precipitated from the solution.

19. The method according to claim 18, wherein the method further comprises The following steps are involved: The process is continued until the desired amount of Nd:Pr is consumed from the solution as a precipitate.

20. The method according to claim 19, wherein the method further comprises The following steps are involved: The remaining solution from which the solids have been removed is treated with a precipitating agent to produce a solution comprising a high purity lanthanum concentrate.

21. The method according to claim 20, wherein the method further comprises The following steps are involved: The solids were removed from the solution.

22. The method according to claim 21, wherein the method further comprises The following steps are involved: Any solids produced are re-digested with mineral acid and the solution is reprocessed to produce higher purity rare earth elements.