Photosensitive resin composition, photosensitive element, printed wiring board, and method for producing printed wiring board

By using acid-modified vinyl-containing resin, photopolymerization initiator and thermosetting resin in the photosensitive resin composition, the problem of bottom residue of the guide hole is solved, the density and reliability of the printed circuit board are improved, and it is suitable as an interlayer insulating layer. permanent resist.

CN119072658APending Publication Date: 2024-12-03RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202480002247.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-02-06
Filing Date
2024-01-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

As the diameter of the guide holes for interlayer connection is further reduced, it is difficult for the conventional photosensitive resin composition to effectively reduce the bottom residue when the guide hole is formed, which affects the density and reliability of the printed circuit board.

Method used

The photosensitive resin composition containing an acid-modified vinyl-containing resin, a photopolymerization initiator, a photopolymerizable compound and a thermosetting resin is used to reduce the bottom residue when the lead is formed by adjusting the resin composition and process parameters.

Benefits of technology

The bottom residue during the formation of guide holes is significantly reduced, the density and reliability of the printed circuit board are improved, and it is suitable as a permanent resist for the interlayer insulating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072658A_ABST
    Figure CN119072658A_ABST
Patent Text Reader

Abstract

Provided is a photosensitive resin composition containing (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound, and (D) a thermosetting resin, the acid-modified vinyl-containing resin (A) containing a first resin having a weight-average molecular weight of less than 4000 and a second resin having a weight-average molecular weight of 4000 or more; the content of the first resin is more than 60% by mass based on the total amount of the (A) acid-modified vinyl-containing resin, and the content of the (A) acid-modified vinyl-containing resin is 33% by mass or less based on the total solid content of the photosensitive resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive resin composition, a photosensitive element, a printed circuit board and a method for manufacturing the printed circuit board. Background Art

[0002] In recent years, printed circuit boards have been moving towards higher density as the number of circuit layers increases and the wiring becomes finer. In particular, the high density of semiconductor package substrates such as BGA (ball grid array) and CSP (chip size package) equipped with semiconductor chips is remarkable. In addition to the fineness of the wiring, the diameter of the guide holes (also called "through holes") used for interlayer connection is also required to be further reduced.

[0003] As photosensitive resin compositions for forming interlayer insulating layers, there are known, for example, a photosensitive resin composition containing an alkali-soluble resin having a carboxyl group and an ethylenically unsaturated group in the molecule, a photopolymerization initiator and a cyanate compound (see Patent Document 1), and a photosensitive resin composition containing an acid-modified vinyl-containing epoxy resin, a photopolymerizable compound, a photopolymerization initiator, an inorganic filler and a silane compound, wherein the content of the inorganic filler is 20 to 60% by mass based on the total solid content in the photosensitive resin composition (see Patent Document 2).

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2019-66793

[0007] Patent Document 2: Japanese Patent Application Publication No. 2017-116652 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] As the diameter of the via holes for interlayer connection is further reduced, the photosensitive resin composition for forming an interlayer insulating layer is required to reduce the residue at the bottom when the via holes are formed.

[0010] Therefore, an object of the present invention is to provide a photosensitive resin composition capable of reducing the residue at the bottom of a guide hole when forming the guide hole, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board.

[0011] Means for solving technical problems

[0012] In order to solve the above-mentioned problems, the present invention provides the following photosensitive resin composition, photosensitive element, printed wiring board, and method for producing the printed wiring board.

[0013] [1] A photosensitive resin composition comprising (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound, and (D) a thermosetting resin, wherein the acid-modified vinyl-containing resin (A) comprises a first resin having a weight average molecular weight of less than 4,000 and a second resin having a weight average molecular weight of not less than 4,000, the content of the first resin being more than 60% by weight based on the total amount of the acid-modified vinyl-containing resin (A), and the content of the acid-modified vinyl-containing resin (A) being not more than 33% by weight based on the total solid content of the photosensitive resin composition.

[0014] [2] The photosensitive resin composition according to [1], wherein

[0015] The first resin includes an acid-modified epoxy (meth)acrylate having an alicyclic skeleton.

[0016] [3] The photosensitive resin composition according to [1] or [2], wherein

[0017] The second resin includes an acid-modified epoxy (meth)acrylate having no alicyclic skeleton.

[0018] [4] The photosensitive resin composition according to any one of [1] to [3], wherein

[0019] The content of the second resin is 5% by mass or more based on the total amount of the (A) acid-modified vinyl-containing resin.

[0020] [5] The photosensitive resin composition according to any one of [1] to [4], further comprising (E) an inorganic filler.

[0021] [6] The photosensitive resin composition according to any one of [1] to [5], further comprising (F) a pigment.

[0022] [7] A photosensitive element comprising a support film and a photosensitive layer formed on the support film, wherein the photosensitive layer comprises the photosensitive resin composition according to any one of [1] to [6] above.

[0023] [8] A printed wiring board comprising an interlayer insulating layer comprising a cured product of the photosensitive resin composition according to any one of [1] to [6] above.

[0024] [9] A method for manufacturing a printed circuit board, comprising:

[0025] The process of forming a photosensitive layer on a substrate using the photosensitive resin composition described in any one of [1] to [6] above; exposing and developing the photosensitive layer to form a resist pattern; and curing the resist pattern to form an interlayer insulating layer.

[0026]

[10] A method for manufacturing a printed circuit board, comprising:

[0027] The process of forming a photosensitive layer on a substrate using the photosensitive element described in [7] above; the process of exposing and developing the photosensitive layer to form a resist pattern; and the process of curing the resist pattern to form an interlayer insulating layer.

[0028] Effects of the Invention

[0029] According to the present invention, it is possible to provide a photosensitive resin composition capable of reducing residue at the bottom of a guide hole when forming the guide hole, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing the printed wiring board. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a cross-sectional view schematically showing a photosensitive element according to this embodiment.

[0031] Figure 2 This is a schematic diagram showing one aspect of the method for manufacturing a printed wiring board according to the present embodiment. DETAILED DESCRIPTION

[0032] The present invention is described in detail below. In this specification, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved. Regarding the term "layer", when viewed in a plan view, in addition to structures of shapes formed on the entire surface, structures of shapes formed on a portion are also included.

[0033] In this specification, the numerical range represented by "~" indicates a range that includes the numerical values ​​recorded before and after "~" as the minimum value and the maximum value, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of any stage can also be replaced by the upper limit or lower limit of the numerical range of other stages, and can also be replaced by the value shown in the embodiment. In this specification, for example, a record such as "10 or more" refers to a numerical value of 10 and more than 10, and this is used as a reference even if the numerical values ​​are different. In addition, a record such as "10 or less" refers to a numerical value of 10 and less than 10, and this is used as a reference even if the numerical values ​​are different.

[0034] In this specification, about the content of each component in the composition, when there are multiple substances equivalent to each component in the composition, unless otherwise specified, it refers to the total content of the multiple substances present in the composition. In this specification, "ring member number" refers to the number of carbon atoms required to form a ring, excluding the number of carbon atoms of the substituents possessed by the ring. In this specification, "(meth)acrylate" refers to at least one of "acrylate" and its corresponding "methacrylate", and other similar expressions such as (meth)acrylic acid are the same. In this specification, "solid content" refers to non-volatile components other than the volatile substances contained in the photosensitive resin composition, and is also included in liquid, syrupy or waxy components at room temperature (about 25°C).

[0035] [Photosensitive resin composition]

[0036] The photosensitive resin composition involved in the present embodiment contains (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound and (D) a thermosetting resin. The above-mentioned (A) acid-modified vinyl-containing resin contains a first resin with a weight average molecular weight of less than 4000 and a second resin with a weight average molecular weight of more than 4000. The content of the above-mentioned first resin is more than 60% by weight based on the total amount of the above-mentioned (A) acid-modified vinyl-containing resin. The content of the above-mentioned (A) acid-modified vinyl-containing resin is less than 33% by weight based on the total amount of the photosensitive resin composition. The photosensitive resin composition having the above-mentioned structure can reduce the residue at the bottom when the guide hole is formed. The photosensitive resin composition involved in the present embodiment is a negative photosensitive resin composition, and the cured product of the photosensitive resin composition can be suitable for use as a permanent resist such as an interlayer insulating layer. Below, each component used in the photosensitive resin composition of the present embodiment is described in more detail.

[0037] (Component (A): acid-modified vinyl-containing resin)

[0038] The photosensitive resin composition involved in the present embodiment contains an acid-modified vinyl-containing resin as component (A). The acid-modified vinyl-containing resin is not particularly limited as long as it has a vinyl group as a photopolymerizable ethylenically unsaturated bond and an alkali-soluble acidic group. As the acidic group possessed by component (A), for example, a carboxyl group, a sulfonic group, and a phenolic hydroxyl group can be cited. Among these, a carboxyl group is preferably used from the viewpoint of having a better resolution.

[0039] Examples of acid-modified vinyl-containing resins include acid-modified epoxy (meth) acrylates. Acid-modified epoxy (meth) acrylates are resins obtained by acid-modifying epoxy (meth) acrylates, which are the reaction products of epoxy resins and organic acids having vinyl groups. Examples of acid-modified epoxy (meth) acrylates include addition reaction products obtained by adding saturated or unsaturated polybasic acid anhydrides (c) to an esterified product obtained by reacting epoxy resins (a) with monocarboxylic acids (b) containing vinyl groups.

[0040] Examples of the epoxy resin (a) include bisphenol novolac epoxy resins, phenol novolac epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, trisphenol methane epoxy resins, biphenyl epoxy resins, naphthalene epoxy resins, and dicyclopentadiene epoxy resins.

[0041] Examples of the vinyl group-containing monocarboxylic acid (b) include (meth)acrylic acid or derivatives thereof such as acrylic acid, a dimer of acrylic acid, methacrylic acid, β-furfuryl acrylic acid, β-styryl acrylic acid, cinnamic acid, crotonic acid, and α-cyanocinnamic acid, a reaction product of a hydroxyl group-containing (meth)acrylic acid ester with a dibasic acid anhydride, i.e., a half ester compound, and a vinyl group-containing monoglycidyl ether or a reaction product of a vinyl group-containing monoglycidyl ester with a dibasic acid anhydride, i.e., a half ester compound.

[0042] Examples of the hydroxyl group-containing (meth)acrylate, vinyl group-containing monoglycidyl ether and vinyl group-containing monoglycidyl ester include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, pentaerythritol pentamethacrylate, glycidyl acrylate and glycidyl methacrylate.

[0043] Examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.

[0044] As saturated or unsaturated polyacid anhydride (c), for example, succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride and itaconic anhydride can be mentioned. Among these, tetrahydrophthalic anhydride can be used from the viewpoint of better resolution.

[0045] Examples of the acid-modified epoxy (meth)acrylate include (A1) an acid-modified epoxy (meth)acrylate having an alicyclic skeleton and (A2) an acid-modified epoxy (meth)acrylate not having an alicyclic skeleton. The component (A) preferably includes the component (A1) from the viewpoint of achieving better resolution, adhesion of the cured product, and electrical insulation reliability and further reducing the residue at the bottom when forming the guide hole.

[0046] From the viewpoint of better resolution, adhesion of the cured product and electrical insulation reliability and further reducing the residue at the bottom when the guide hole is formed, the number of ring members of the alicyclic skeleton possessed by the component (A1) is preferably 5 to 20, more preferably 5 to 18, further preferably 6 to 18, particularly preferably 8 to 14, and particularly preferably 8 to 12. From the same viewpoint, the number of rings of the alicyclic skeleton possessed by the component (A1) is preferably 2 or more, more preferably 2 to 4, and further preferably 3. As the alicyclic skeleton having 1 ring, for example, a cyclohexane skeleton and a cyclohexene skeleton can be cited, and as the alicyclic skeleton having 2 or more rings, for example, a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton and a saturated dicyclopentadiene skeleton can be cited.

[0047] From the viewpoint of achieving better resolution, adhesion of the cured product, and electrical insulation reliability and further reducing the residue at the bottom of the via when formed, the component (A1) preferably has a saturated dicyclopentadiene skeleton as the alicyclic skeleton, and more preferably has a saturated dicyclopentadiene skeleton represented by the following formula (a).

[0048]

[0049] In formula (a), R A1 represents an alkyl group having 1 to 12 carbon atoms, m 1 is an integer of 0 to 6, and * is a bonding site with other structures.

[0050] As R A1 The alkyl group having 1 to 12 carbon atoms represented by the alkyl group includes, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl and n-pentyl. From the viewpoint of better resolution, adhesion of the cured product and electrical insulation reliability and further reduction of the residue at the bottom when the guide hole is formed, the alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably a methyl group.

[0051] m 1 It is preferably an integer of 0 to 2, and more preferably 0. 1 When it is an integer from 2 to 6, multiple R A1 They can be the same or different.A1 Substitution may be on the same carbon atom or on different carbon atoms to the extent possible.

[0052] As the component (A1), for example, an addition reaction product obtained by adding a saturated or unsaturated polybasic acid anhydride (c) to an esterified product obtained by reacting an epoxy resin (a1) having an alicyclic skeleton with a vinyl group-containing monocarboxylic acid (b) can be used.

[0053] Examples of the epoxy resin (a1) include glycidyl ether type, glycidyl amine type, and glycidyl ester type. Among these, glycidyl ether type is preferred.

[0054] As the epoxy resin (a1), an epoxy resin represented by the following formula (a1-1) or an epoxy resin having a structural unit represented by the following formula (a1-2) is preferred.

[0055]

[0056] In formula (a1-1), R A1 and m 1 With R in formula (a) A1 and m 1 Same, R A2 represents an alkyl group having 1 to 12 carbon atoms, m 2 is an integer of 0 to 3, and n represents the number of structural units in parentheses, which is 0 to 10.

[0057] R A2 The alkyl group having 1 to 12 carbon atoms represented by A1 The alkyl groups listed. 2 It is preferably 0 or 1, and more preferably 0. When the epoxy resin is a mixture of different numbers of structural units in parentheses, n represents the average value of the mixture.

[0058]

[0059] In formula (a1-2), R A1 and m 1 With R in formula (a) A1 and m 1 same.

[0060] Examples of commercially available products of the epoxy resin (a1) include dicyclopentadiene-type epoxy resins such as XD-1000 (manufactured by Nippon Kayaku Co., Ltd., product name), EPICLON HP-7200L, EPICLON HP-7200, EPICLON HP-7200HH, and EPICLON HP-7200HHH (manufactured by DIC Corporation, product name, “EPICLON” is a registered trademark).

[0061] As the component (A2), for example, an addition reaction product obtained by adding a saturated or unsaturated polybasic acid anhydride (c) to an esterified product obtained by reacting an epoxy resin (a2) having no alicyclic skeleton with a monocarboxylic acid (b) containing a vinyl group can be used.

[0062] Examples of the epoxy resin (a2) include bisphenol-based epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin; bisphenol-based novolac epoxy resins such as bisphenol A novolac epoxy resin and bisphenol F novolac epoxy resin; phenol aralkyl epoxy resins; stilbene epoxy resins; naphthalene-based epoxy resins, naphthol novolac epoxy resins, naphthol-based epoxy resins, naphthol aralkyl epoxy resins, naphthylene ether epoxy resins, and other naphthalene skeleton-containing epoxy resins; biphenyl-based epoxy resins; biphenyl aralkyl epoxy resins; xylylene-based epoxy resins; dihydroanthracene-based epoxy resins; and aliphatic chain epoxy resins. Among these, bisphenol-based novolac epoxy resins are preferred, and bisphenol F novolac epoxy resins are more preferred.

[0063] The acid value of component (A) is not particularly limited. From the viewpoint of improving the solubility of the unexposed portion in an alkaline aqueous solution, the acid value of component (A) may be 30 mgKOH / g or more, 40 mgKOH / g or more, or 50 mgKOH / g or more. From the viewpoint of improving the electrical properties of the cured product, the acid value of component (A) may be 150 mgKOH / g or less, 120 mgKOH / g or less, or 100 mgKOH / g or less.

[0064] The component (A) contains a first resin having a weight average molecular weight (Mw) of less than 4000 and a second resin having a weight average molecular weight (Mw) of 4000 or more. The first resin and the second resin are selected from the resins whose Mw satisfies the above conditions in the component (A). The first resin may be the component (A1). The second resin may be the component (A2).

[0065] From the viewpoint of further reducing the residue at the bottom when forming the guide hole, the Mw of the first resin may be 3500 or less, 3000 or less, 2500 or less, or 2000 or less, and from the viewpoint of ensuring the resolution during development, it may be 500 or more or 1000 or more. From the viewpoint of better adhesion of the cured product, the Mw of the second resin may be 4500 or more, 5000 or more, 5500 or more, or 6000 or more, and from the viewpoint of adjusting the viscosity of the varnish during coating, it may be 100000 or less, 50000 or less, or 10000 or less.

[0066] From the viewpoint of further reducing the residue at the bottom when the guide hole is formed and achieving better adhesion of the cured product, the difference between the Mw of the first resin and the Mw of the second resin may be 1000 or more, 1500 or more, 2000 or more, 2500 or more, 3000 or more, 3500 or more, or 4000 or more, and from the viewpoint of compatibility, may be 10000 or less, 9000 or less, 8000 or less, 7000 or less, or 6000 or less.

[0067] (A) The Mw of component can be measured by gel permeation chromatography (GPC). Mw is measured, for example, under the following GPC conditions, and the value converted using the calibration curve of standard polystyrene can be set to Mw. The preparation of the calibration curve can use 5 sample groups ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) as standard polystyrene.

[0068] (GPC conditions)

[0069] GPC apparatus: High-speed GPC apparatus "HCL-8320GPC" (manufactured by Tosoh Corporation)

[0070] Detector: Differential refractometer or UV detector (manufactured by Tosoh Corporation)

[0071] Column: TSKgel SuperMultipore HZH (column length: 15 cm, column inner diameter:

[0072] 4.6mm)(Tosoh Corporation)

[0073] Eluent: Tetrahydrofuran (THF)

[0074] Measurement temperature: 40℃

[0075] Flow rate: 0.35mL / min

[0076] Sample concentration: 10mg / THF5mL

[0077] Injection volume: 20 μL

[0078] In the component (A), the content of the first resin is more than 60% by mass based on the total amount of the component (A). From the viewpoint of further reducing the residue at the bottom when the guide hole is formed, the content of the first resin can be 65% by mass or more, 68% by mass or more, or 70% by mass or more based on the total amount of the component (A), and from the viewpoint of constituting the viscosity of the entire composition, the content of the first resin can be 95% by mass or less, 90% by mass or less, 85% by mass or less, or 80% by mass or less based on the total amount of the component (A).

[0079] In the component (A), the content of the second resin is less than 40% by mass based on the total amount of the component (A). From the viewpoint of increasing the molecular weight during patterning, the content of the second resin can be 5% by mass or more, 10% by mass or more, 15% by mass or more, or 20% by mass or more based on the total amount of the component (A), and from the viewpoint of further reducing the residue at the bottom when the guide hole is formed, the content of the second resin can be 35% by mass or less, 32% by mass or less, or 30% by mass or less based on the total amount of the component (A).

[0080] The content of the component (A) in the photosensitive resin composition is 33% by mass or less based on the total solid content of the photosensitive resin composition. From the viewpoint of further reducing the residue at the bottom when forming the guide hole, the content of the component (A) can be 32% by mass or less, 31% by mass or less, 30% by mass or less, or 29% by mass or less based on the total solid content of the photosensitive resin composition. From the viewpoint of ensuring the resolution during development, the content of the component (A) can be 20% by mass or more, 22% by mass or more, or 25% by mass or more based on the total solid content of the photosensitive resin composition.

[0081] (Component (B): photopolymerization initiator)

[0082] The photosensitive resin composition according to the present embodiment contains a photopolymerization initiator as the component (B). The component (B) is not particularly limited as long as it can polymerize the component (A) and the like.

[0083] Examples of the component (B) include benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-1-butanone, 2-methyl-[4-(methylthio)phenyl]-2-morpholinyl-1-propane, and N,N-dimethylaminoacetophenone. anthraquinone compounds such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; thioxanthone compounds such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; acetophenone dimethyl ketal, benzyl dimethyl ketal, and other ketal compounds; benzophenone, methyl benzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, Michler's ketone Benzophenone compounds such as 4-benzoyl-4'-methyl diphenyl sulfide; imidazole compounds such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5-diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4-di(p-methoxyphenyl)-5-phenylimidazole dimer, 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer; 9-phenylacridine, 1,7 -Acridinium compounds such as bis(9,9'-acridinyl)heptane; acylphosphine oxide compounds such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide; oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyl oxime), 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime]; and tertiary amine compounds such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isopentyl ester, 4-dimethylaminobenzoic acid pentyl ester, triethylamine, and triethanolamine.

[0084] Component (B) may be used alone or in combination of two or more. When two or more are used in combination, it is preferred that an acetophenone compound and a thioxanthone compound be used in combination, and more preferably 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone and 2,4-diethylthioxanthone be used in combination.

[0085] The content of the component (B) in the photosensitive resin composition is not particularly limited, and can be 0.1 to 15 mass %, 0.15 to 5 mass %, 0.15 to 1.5 mass % or 0.18 to 1.2 mass % based on the total solid content of the photosensitive resin composition. When the content of the component (B) is 0.1 mass % or more, it tends to suppress the dissolution of the exposed part during development when forming the resist pattern, and when the content of the component (B) is 15 mass % or less, it tends to improve the heat resistance of the cured product.

[0086] (Component (C): photopolymerizable compound)

[0087] From the viewpoint of improving chemical resistance after exposure and increasing the difference in developer resistance between the exposed portion and the unexposed portion, the photosensitive resin composition of the present embodiment contains a photopolymerizable compound as component (C). Component (C) is not particularly limited as long as it is a photopolymerizable compound having an ethylenically unsaturated group and no acidic group.

[0088] (C) As a component, the photopolymerizable compound which has one ethylenically unsaturated group, the photopolymerizable compound which has two ethylenically unsaturated groups, and the photopolymerizable compound which has three or more ethylenically unsaturated groups are mentioned, for example.

[0089] Examples of the photopolymerizable compound having one ethylenically unsaturated group include (meth)acrylic acid and alkyl (meth)acrylates. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hydroxyethyl (meth)acrylate.

[0090] Examples of the photopolymerizable compound having two ethylenically unsaturated groups include polyethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2-bis(4-(meth)acryloyloxypolyethoxypolypropoxyphenyl)propane, and bisphenol A diglycidyl ether di(meth)acrylate.

[0091] Examples of the photopolymerizable compound having three or more ethylenically unsaturated groups include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from ditrimethylolpropane, such as ditrimethylolpropane tetra(meth)acrylate; and (meth)acrylate compounds having a skeleton derived from diglycerol.

[0092] Among these, from the viewpoint of improving chemical resistance after exposure and increasing the difference in developer resistance between the exposed portion and the unexposed portion, a (meth)acrylate compound having a skeleton derived from dipentaerythritol is preferred, and dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate are more preferred.

[0093] When the photosensitive resin composition of the present embodiment contains the component (C), the content thereof may be 1 to 20 mass %, 2 to 15 mass %, or 4 to 12 mass % based on the total solid content of the photosensitive resin composition.

[0094] ((D) component: thermosetting resin)

[0095] The photosensitive resin composition according to the present embodiment contains a thermosetting resin as the component (D). By containing the component (D), a cured product having excellent adhesiveness can be formed. The component (D) can be used alone or in combination of two or more.

[0096] As component (D), for example, epoxy resin, phenolic resin, unsaturated imide resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin, silicone resin, triazine resin and melamine resin can be mentioned. Among these, epoxy resin is preferred from the viewpoint of better adhesion of the cured product.

[0097] Examples of the epoxy resin include bisphenol-A epoxy resin, bisphenol-F epoxy resin, bisphenol-S epoxy resin and other bisphenol-novolac epoxy resins; phenol-novolac epoxy resins, cresol-novolac epoxy resins, biphenyl-novolac epoxy resins and other novolac epoxy resins; phenol-aralkyl epoxy resins; stilbene-type epoxy resins; naphthalene-type epoxy resins, naphthol-novolac epoxy resins, naphthol-novolac epoxy resins; Epoxy resins containing naphthalene skeletons, such as epoxy resins containing terephthalate, naphthol aralkyl type epoxy resins, and naphthylene ether type epoxy resins; biphenyl type epoxy resins; biphenyl aralkyl type epoxy resins; xylene type epoxy resins; dihydroanthracene type epoxy resins; alicyclic epoxy resins such as dicyclopentadiene type epoxy resins; heterocyclic epoxy resins; epoxy resins containing spiro rings; cyclohexanedimethanol type epoxy resins; trimethylol type epoxy resins; aliphatic chain epoxy resins; and rubber modified epoxy resins.

[0098] Among these, from the viewpoint that the heat resistance, adhesion and electrical insulation reliability of the cured product are better and the residue at the bottom when the guide hole is formed can be further reduced, as the epoxy resin, it is preferred to use at least one selected from bisphenol type epoxy resin, phenol novolac type epoxy resin, naphthol type epoxy resin, naphthalene type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin and cresol novolac type epoxy resin.

[0099] The content of the component (D) in the photosensitive resin composition can be 2 to 30 mass %, 5 to 25 mass % or 8 to 20 mass % based on the total solid content of the photosensitive resin composition. When the content of the component (D) is within the above range, the heat resistance of the formed cured film can be further improved while maintaining good developability.

[0100] ((E) ingredient: inorganic filler)

[0101] The photosensitive resin composition according to the present embodiment may further contain an inorganic filler as the component (E). By containing the component (E), the adhesion and reliability of the cured product can be improved. The component (E) may be used alone or in combination of two or more.

[0102] Examples of the inorganic filler include silica, alumina, titanium dioxide, tantalum oxide, zirconium oxide, silicon nitride, barium titanate, barium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, lead titanate, lead zirconate titanate, lead lanthanum zirconate titanate, gallium oxide, spinel, mullite, cordierite, talc, aluminum titanate, zirconium oxide containing yttrium oxide, barium silicate, boron nitride, calcium carbonate, barium sulfate, calcium sulfate, zinc oxide, magnesium titanate, hydrotalcite, mica, calcined kaolin and carbon.

[0103] From the viewpoint of improving the heat resistance of the cured product, component (E) may contain silicon dioxide, and from the viewpoint of improving the heat resistance and adhesion of the cured product, may contain barium sulfate. From the viewpoint of improving the dispersibility of the inorganic filler, an inorganic filler that has been surface-treated in advance with aluminum oxide or an organic silane compound may be used.

[0104] From the viewpoint of resolution, the average particle size of the inorganic filler is preferably 0.01 to 5.0 μm, more preferably 0.1 to 3.0 μm, further preferably 0.3 to 2.0 μm, and particularly preferably 0.5 to 1.5 μm.

[0105] When the photosensitive resin composition of the present embodiment contains component (E), its content can be 5 to 80 mass %, 10 to 60 mass %, 15 to 50 mass %, 20 to 45 mass %, 25 to 40 mass % or 30 to 40 mass % based on the total solid content of the photosensitive resin composition. When the content of component (E) is within the above range, the resolution, mechanical strength and heat resistance of the cured product can be improved.

[0106] ((F) ingredient: pigment)

[0107] From the viewpoint of improving the recognition or appearance of the manufacturing device, the photosensitive resin composition of the present embodiment may further contain a pigment as the (F) component. As the (F) component, a colorant that develops a desired color when concealing wiring, etc. can be used. As the (F) component, for example, phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black can be cited.

[0108] From the viewpoint of further concealing the wiring, the content of the component (F) may be 0.1 to 10% by mass, 0.5 to 8% by mass, or 1 to 5% by mass based on the total solid content in the photosensitive resin composition.

[0109] ((G) component: elastomer)

[0110] The photosensitive resin composition of the present embodiment may further contain an elastomer as the component (G). By containing the component (G), the reduction in flexibility and bonding strength caused by the deformation (internal stress) inside the resin caused by the curing shrinkage of the component (A) can be suppressed. In addition, by containing the component (G), the resolution of the photosensitive resin composition, the adhesion of the cured product, and the electrical insulation reliability tend to be easily improved. The component (G) may be used alone or in combination of two or more.

[0111] As the component (G), for example, styrene elastomers, olefin elastomers, urethane elastomers, polyester elastomers, polyamide elastomers, acrylic elastomers and silicone elastomers can be mentioned. These elastomers are composed of a hard segment component that contributes to heat resistance and strength and a soft segment component that contributes to flexibility and toughness.

[0112] Examples of the styrene-based elastomer include styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-ethylene-butylene-styrene block copolymers, and styrene-ethylene-propylene-styrene block copolymers. As a component constituting the styrene-based elastomer, in addition to styrene, styrene derivatives such as α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene can be used.

[0113] The number average molecular weight of the styrene-based elastomer may be 1000 to 50000 or 3000 to 20000. In the present specification, the number average molecular weight is a value determined by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent in terms of standard polystyrene.

[0114] Examples of olefin-based elastomers include polymers or copolymers of α-olefins having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-hexene, and 4-methyl-pentene; copolymers of α-olefins having 2 to 20 carbon atoms and non-conjugated dienes having 2 to 20 carbon atoms, such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylene norbornene, ethylidene norbornene, butadiene, and isoprene; and carboxylic acid-modified butadiene-acrylonitrile copolymers. Specifically, examples include polyethylene, polybutadiene, hydroxyl-containing polybutadiene, hydroxyl-containing polyisopropylene, ethylene-propylene copolymers (EPR), and ethylene-propylene-diene copolymers (EPDM).

[0115] The number average molecular weight of the olefin-based elastomer may be 1,000 to 8,000 or 1,500 to 6,500.

[0116] As the polyester-based elastomer, a compound obtained by polycondensation of a dicarboxylic acid or a derivative thereof and a diol compound or a derivative thereof can be used.

[0117] Examples of the dicarboxylic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalene dicarboxylic acid; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid.

[0118] Examples of the diol compound include aliphatic diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis(4-hydroxyphenyl)methane, bis(4-hydroxy-3-methylphenyl)propane, and resorcinol.

[0119] As the polyester elastomer, a multi-block copolymer having an aromatic polyester (e.g., polybutylene terephthalate) as a hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) as a soft segment component can be used. There are different grades of polyester elastomers depending on the type, ratio, and molecular weight of the hard segment and the soft segment. As commercial products of such multi-block copolymers, for example, "Hytrel (registered trademark)" (manufactured by DU PONT-TORAY CO., LTD.), "PELPRENE (registered trademark)" (manufactured by TOYOBO CO., LTD.), "Espel (registered trademark)" and "Teslac (registered trademark)" (manufactured by Resonac Holdings Corporation) can be cited.

[0120] The number average molecular weight of the polyester elastomer may be 900 to 30,000, 1,000 to 25,000, or 5,000 to 20,000.

[0121] As the urethane elastomer, a compound composed of a hard segment including a low molecular weight (short chain) diol and a diisocyanate and a soft segment including a high molecular weight (long chain) diol and a diisocyanate can be used.

[0122] Examples of the short-chain diol include ethylene glycol, propylene glycol, 1,4-butanediol, and bisphenol A. The number average molecular weight of the short-chain diol is preferably 48 to 500.

[0123] Examples of the long-chain diol include polypropylene glycol, polyoxytetramethylene glycol, poly(1,4-butene adipate), poly(ethylene-1,4-butene adipate), polycaprolactone, poly(1,6-hexene carbonate), and poly(1,6-hexene-neopentyl adipate). The number average molecular weight of the long-chain diol is preferably 500 to 10,000.

[0124] The number average molecular weight of the urethane elastomer may be 1,000 to 25,000, 1,500 to 20,000, or 2,000 to 15,000.

[0125] Polyamide-based elastomers are roughly divided into two types: polyether block amide type and polyether ester block amide type, which use polyamide in the hard segment and polyether or polyester in the soft segment. Examples of polyamide include polyamide-6, polyamide-11, and polyamide-12. Examples of polyether include polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene glycol.

[0126] The number average molecular weight of the polyamide-based elastomer may be 1,000 to 50,000 or 2,000 to 30,000.

[0127] Acrylic elastomers can use compounds containing structural units based on (meth)acrylate as main components. Examples of (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, methoxyethyl (meth)acrylate, and ethoxyethyl (meth)acrylate. Acrylic elastomers can be compounds obtained by copolymerizing (meth)acrylate and acrylonitrile, or compounds obtained by further copolymerizing monomers having functional groups that serve as crosslinking points. Examples of monomers having functional groups include glycidyl methacrylate and allyl glycidyl ether.

[0128] Examples of the acrylic elastomer include acrylonitrile-butyl acrylate copolymer, acrylonitrile-butyl acrylate-ethyl acrylate copolymer, methyl methacrylate-butyl acrylate-methacrylic acid copolymer, and acrylonitrile-butyl acrylate-glycidyl methacrylate copolymer.

[0129] The number average molecular weight of the acrylic elastomer may be 1,000 to 50,000 or 2,000 to 30,000.

[0130] Silicone elastomers are compounds containing organopolysiloxane as a main component. Examples of organopolysiloxanes include polydimethylsiloxane, polymethylphenylsiloxane, and polydiphenylsiloxane. Silicone elastomers may be compounds obtained by modifying a portion of organopolysiloxane with a vinyl group, an alkoxy group, or the like.

[0131] The number average molecular weight of the silicone elastomer may be 1,000 to 50,000 or 2,000 to 30,000.

[0132] From the viewpoint of compatibility and solubility with other components of the photosensitive resin composition and adhesion of the cured product, the component (G) preferably comprises at least one selected from the group consisting of olefin elastomers, polyester elastomers and urethane elastomers, and more preferably comprises a polyester elastomer. From the same viewpoint, the component (G) is preferably an elastomer that is liquid at room temperature.

[0133] When the photosensitive resin composition of the present embodiment contains component (G), its content can be 0.5 to 20 mass %, 0.5 to 15 mass %, 0.5 to 10 mass %, 1.0 to 6 mass % or 1.0 to 4.0 mass % based on the total solid content of the photosensitive resin composition. When the content of component (G) is within the above range, there is a tendency for the resolution and the adhesion and electrical insulation reliability of the cured product to be better.

[0134] (Other ingredients)

[0135] The photosensitive resin composition of the present embodiment may further include various additives as required. Examples of additives include polymerization inhibitors such as thermal polymerization initiators, hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, and gallol; thickeners such as bentonite and montmorillonite; defoamers such as silicone, fluorine, and vinyl resins; silane coupling agents; flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, phosphate compounds, aromatic condensed phosphates, and halogen-containing condensed phosphates; and thermoplastic resins such as polyester polyurethane resins.

[0136] (Solvent)

[0137] The photosensitive resin composition according to the present embodiment may contain a solvent as needed. The photosensitive resin composition according to the present embodiment contains a solvent for dissolving / dispersing each component, so that coating on a substrate becomes easy and a coating film with uniform thickness can be formed, thereby forming a higher-definition pattern.

[0138] As the solvent, an organic solvent can be mentioned. As the organic solvent, for example, ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, propylene glycol monoethyl ether acetate, butyl cellosolve acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, naphtha, hydrogenated naphtha, and solvent naphtha. Among these, ketones and esters are preferred, and esters are more preferred. The solvent can be used alone or in combination of two or more.

[0139] The amount of the solvent added can be appropriately selected so that the concentration of the total solid content in the photosensitive resin composition becomes 40 to 90 mass %, 45 to 80 mass %, or 45 to 70 mass %.

[0140] The photosensitive resin composition of the present embodiment can be prepared by uniformly mixing the above-mentioned components using a roll mill, a bead mill, etc. The photosensitive resin composition of the present embodiment may be used in a liquid state or in a film state as in the photosensitive element described below.

[0141] [Photosensitive element]

[0142] The photosensitive element according to the present embodiment includes a support film and a photosensitive layer containing the above-mentioned photosensitive resin composition. Figure 1 FIG. 2 is a cross-sectional view schematically showing a photosensitive element according to the present embodiment. Figure 1 As shown, the photosensitive element 1 includes a support film 10 and a photosensitive layer 20 formed on the support film 10. The photosensitive element 1 may further include a protective film 30 on the photosensitive layer 20.

[0143] The photosensitive element 1 can be produced by coating the photosensitive resin composition according to the present embodiment on a support film 10 using a known coating apparatus such as a teasing coater, a bar coater, a kiss coater, a roll coater, a gravure coater, a die coater, and then drying the coating to form a photosensitive layer 20. The thickness of the photosensitive layer is not particularly limited, and may be 1 to 100 μm, 1 to 50 μm, or 5 to 40 μm from the viewpoint of reducing the thickness of the printed wiring board.

[0144] The coating film can be dried using a hot air dryer, a dryer using far infrared rays or near infrared rays, etc. The drying temperature can be 60 to 150° C., 70 to 120° C., or 80 to 100° C. The drying time can be 1 to 60 minutes, 2 to 30 minutes, or 5 to 20 minutes. From the viewpoint of avoiding diffusion of the solvent in the manufacturing process of the printed wiring board, the content of the residual solvent in the dried coating film can be 3% by mass or less, 2% by mass or less, or 1% by mass or less.

[0145] Examples of the support film include polyester films such as polyethylene terephthalate films and polybutylene terephthalate films, and polyolefin films such as polypropylene films and polyethylene films. The thickness of the support film may be, for example, 5 to 100 μm, 5 to 60 μm, or 15 to 45 μm.

[0146] For example, a polymer film such as polyethylene or polypropylene can be used as the protective film 30. The protective film 30 may be the same film as the support film 10 or a different film.

[0147] The photosensitive resin composition of the present embodiment is suitable as a permanent resist such as an interlayer insulating layer of a printed wiring board. In addition, the photosensitive resin composition of the present embodiment is also useful for forming a cavity for a built-in chip or a passive component. The photosensitive resin composition of the present embodiment is also useful for forming a surface protective layer of a printed wiring board.

[0148] [Printed circuit board]

[0149] The printed wiring board according to the present embodiment includes an interlayer insulating layer formed of a cured product of the photosensitive resin composition according to the present embodiment.

[0150] The method for manufacturing a printed wiring board according to the present embodiment includes the steps of forming a photosensitive layer on a substrate using the photosensitive resin composition or photosensitive element according to the present embodiment, exposing and developing the photosensitive layer to form a resist pattern, and curing the resist pattern to form an interlayer insulating layer.

[0151] Figure 2 This is a schematic cross-sectional view showing an example of a method for producing a multilayer printed wiring board having a cured product of the photosensitive resin composition according to the present embodiment as an interlayer insulating layer. Figure 2 The multilayer printed wiring board 100A shown in (f) has a wiring pattern on the surface and inside. The multilayer printed wiring board 100A can be obtained by stacking copper-clad laminates, interlayer insulating layers, metal foils, etc. and forming the wiring pattern appropriately by etching or semi-additive method. Figure 2 , a method for manufacturing the multilayer printed wiring board 100A is briefly described.

[0152] First, interlayer insulating layers 103 (see FIG. 1 ) are formed on both sides of a substrate (eg, a copper-clad laminate) 101 having a wiring pattern 102 on its surface. Figure 2 (a)). The interlayer insulating layer 103 can also be formed by printing the photosensitive resin composition involved in this embodiment using a screen printer or a roll coater, or by preparing the photosensitive element involved in this embodiment in advance and attaching the photosensitive layer in the photosensitive element to the surface of the substrate 101 using a laminator.

[0153] Next, a YAG laser or a carbon dioxide laser is used to form a guide hole (opening) 104 at a location that needs to be electrically connected to the outside (see Figure 2 (b)) Stain (residue) around the guide hole 104 can be removed by desmearing treatment.

[0154] Next, a seed layer 105 is formed by electroless plating (see Figure 2 (c)) A photosensitive layer including a photosensitive resin composition is formed on the seed layer 105, and a predetermined portion is exposed and developed to form a resin pattern 106 (see Figure 2 (d)).

[0155] Next, the wiring pattern 107 is formed on the portion of the seed layer 105 where the resin pattern 106 is not formed by electrolytic plating. Then, after the resin pattern 106 is further removed by a stripping solution, the portion of the seed layer 105 where the wiring pattern 107 is not formed is removed by etching (refer to Figure 2 (e)).

[0156] By repeatedly performing the above operation and forming the solder resist 108 including the cured product of the photosensitive resin composition according to the present embodiment on the outermost surface, a multilayer printed wiring board 100A can be manufactured (see Figure 2 (f)) The multilayer printed wiring board 100A obtained in this way can be equipped with semiconductor elements, for example, at corresponding locations to ensure electrical connection.

[0157] The photosensitive resin composition of the present embodiment can be used to prepare a semiconductor element having an interlayer insulating layer formed by a cured product of the photosensitive resin composition, and an electronic device including the semiconductor element. The semiconductor element can be, for example, a memory, a package, etc. having a multilayer wiring structure, a redistribution structure, etc. As electronic devices, for example, mobile phones, smart phones, tablet terminals, personal computers, and hard disk suspension devices can be cited. By having a pattern cured product formed by the photosensitive resin composition of the present embodiment, a semiconductor element and an electronic device with excellent reliability can be provided.

[0158] Example

[0159] Hereinafter, the present invention will be described in further detail by way of examples, but the present invention is not limited to these examples.

[0160] (Synthesis example 1)

[0161] 250 parts by mass of dicyclopentadiene epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name "XD-1000"), 70 parts by mass of acrylic acid, 0.5 parts by mass of methylhydroquinone and 120 parts by mass of carbitol acetate were stirred and mixed at 90°C. The mixed solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the mixture was reacted at 100°C until the acid value of the solution reached 1 mgKOH / g. 98 parts by mass of tetrahydrophthalic anhydride and 850 parts by mass of carbitol acetate were added to the reaction solution, and the mixture was heated to 80°C and reacted for 6 hours. Thereafter, the reaction solution was cooled to room temperature to obtain a solution of an acid-modified epoxy acrylate resin (A-1) as the first resin of component (A) (solid content concentration 65% by mass). The Mw of the obtained acid-modified epoxy acrylate resin (A-1) was 1800.

[0162] (Synthesis example 2)

[0163] 350 parts by mass of bisphenol F novolac epoxy resin (manufactured by DIC Corporation, product name "EXA-7376"), 70 parts by mass of acrylic acid, 0.5 parts by mass of methylhydroquinone and 120 parts by mass of carbitol acetate were stirred and mixed at 90°C. The mixed solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the mixture was reacted at 100°C until the acid value of the solution became 1 mgKOH / g or less. 98 parts by mass of tetrahydrophthalic anhydride and 850 parts by mass of carbitol acetate were added to the reaction solution, and the mixture was reacted at 80°C for 6 hours. Thereafter, the reaction solution was cooled to room temperature to obtain a solution of acid-modified epoxy acrylate (A-2) as component (A) (solid content concentration: 73% by mass). The Mw of the obtained acid-modified epoxy acrylic resin (A-2) was 4500.

[0164] The following materials were prepared as components (B) to (F).

[0165] B-1: 2-methyl-[4-(methylthio)phenyl]-2-morpholinyl-1-propane (manufactured by IGM Resins BV, product name "Omnirad 907")

[0166] B-2: 2,4-diethylthioxanthone (manufactured by Nagase & Co., Ltd., product name "SBPI799")

[0167] C-1: Dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd., product name "DPHA")

[0168] C-2: dicyclopentanyl acrylate (manufactured by Resonac Holdings Corporation, product name "FA-513AS")

[0169] D-1: Bisphenol novolac type epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name "RE-306")

[0170] D-2: Tetramethylbiphenol type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "YX4000")

[0171] E-1: Silica (average particle size 0.5 μm) (manufactured by ADMATECHS COMPANY LIMITED, Adma fine (registered trademark))

[0172] F-1: Phthalocyanine pigment (manufactured by SANYO COLOR WORKS, Ltd.)

[0173] [Photosensitive resin composition]

[0174] Each component was blended in the blended amounts (parts by mass, solid content conversion amount) shown in Table 1, and kneaded using a three-roll mill. Then, carbitol acetate was added so that the solid content concentration became 60% by mass, thereby preparing a photosensitive resin composition.

[0175] [Photosensitive element]

[0176] A polyethylene terephthalate film (manufactured by TEIJIN LIMITED, product name "G2-16") with a thickness of 16 μm was prepared as a support film. The photosensitive resin composition was applied to the support film so that the thickness after drying became 18 μm, and dried at 75° C. for 30 minutes using a hot air convection dryer to form a photosensitive layer. Next, a polyethylene film (manufactured by TAMAPOLY CO., LTD., product name "NF-15") was laminated as a protective film on the surface opposite to the side in contact with the support film of the photosensitive layer to obtain a photosensitive element.

[0177] (Bottom residue evaluation)

[0178] A copper-clad laminate substrate (manufactured by Resonac Holdings Corporation, product name "MCL-E-67") with a thickness of 0.6 mm was prepared. The protective film was peeled off from the photosensitive element, and a photosensitive layer was laminated on the copper-clad laminate substrate using a pressurized vacuum laminator (manufactured by Meiki Co., Ltd., product name "MVLP-500") under the conditions of crimping pressure: 0.4 MPa, pressurized heating plate temperature: 80°C, vacuuming time: 25 seconds, lamination pressurization time: 25 seconds, and air pressure: 4 kPa or less to obtain a laminate. Next, an i-ray exposure device (manufactured by Ushio Co., Ltd., product name "UX-2240SM-XJ-01") was used through a negative mask having a through-hole pattern with an opening diameter of 30 μm at a temperature of 100 to 1000 mJ / cm 2 The range is changed by 50 mJ / cm 2 Then, a 1 mass % sodium carbonate aqueous solution was used to develop the photosensitive layer at 1.765×10 5 The unexposed area was developed by spraying at a pressure of 2000 mJ / cm 2After exposure at an exposure amount of , a test piece having a cured film with a through-hole pattern having an opening diameter of 30 μm on a copper-clad laminate substrate was prepared. The presence or absence of residue at the bottom of the guide hole pattern portion of the test piece was confirmed using a scanning electron microscope. The following criteria were used for evaluation. The results are shown in Table 1.

[0179] <Evaluation Criteria>

[0180] A: No residue was observed at the bottom.

[0181] B: Residue was observed in a part of the bottom.

[0182] C: Residue was observed on the entire surface of the bottom.

[0183] [Table 1]

[0184]

[0185] Explanation of symbols

[0186] 1-photosensitive element, 10-support film, 20-photosensitive layer, 30-protective film, 100A-multilayer printed wiring board, 101-substrate, 102, 107-wiring pattern, 103-interlayer insulating layer, 104-guide hole, 105-seed layer, 106-resin pattern, 108-solder resist.

Claims

1. A photosensitive resin composition comprising (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound, and (D) a thermosetting resin, wherein: The (A) acid-modified vinyl-containing resin comprises a first resin having a weight average molecular weight of less than 4000 and a second resin having a weight average molecular weight of 4000 or more. The content of the first resin is more than 60% by mass based on the total amount of the (A) acid-modified vinyl-containing resin. The content of the (A) acid-modified vinyl-containing resin is 33% by mass or less based on the total solid content of the photosensitive resin composition.

2. The photosensitive resin composition according to claim 1, wherein The first resin includes an acid-modified epoxy (meth)acrylate having an alicyclic skeleton.

3. The photosensitive resin composition according to claim 1, wherein The second resin includes an acid-modified epoxy (meth)acrylate having no alicyclic skeleton.

4. The photosensitive resin composition according to claim 1, wherein The content of the second resin is 5% by mass or more based on the total amount of the (A) acid-modified vinyl-containing resin. The photosensitive resin composition according to claim 1 , further comprising (E) an inorganic filler. The photosensitive resin composition according to claim 1 , further comprising (F) a pigment.

7. A photosensitive element comprising a support film and a photosensitive layer formed on the support film, The photosensitive layer comprises the photosensitive resin composition according to any one of claims 1 to 6. 8 . A printed wiring board comprising an interlayer insulating layer comprising a cured product of the photosensitive resin composition according to claim 1 .

9. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 6; A step of exposing and developing the photosensitive layer to form a resist pattern; and The step of curing the resist pattern to form an interlayer insulating layer.

10. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive element according to claim 7; A step of exposing and developing the photosensitive layer to form a resist pattern; and The step of curing the resist pattern to form an interlayer insulating layer.