Toner

By controlling the size and shape of toner particles, combined with the addition of organic and inorganic particles, the leakage problem of toner in high temperature and high humidity environments and the problem of insufficient thin line reproducibility is solved, achieving higher stability and drawing quality.

CN119072662APending Publication Date: 2024-12-03ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030045.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-17
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing toner is prone to leaking in high temperature and high humidity environments, and the thin line reproducibility is insufficient during continuous printing, making it difficult to meet the needs of high picture quality and high-speed printing.

Method used

By controlling the size and macro shape of the toner particles, a toner containing the colored resin particles and an external additive is used, and the circular area equivalent diameter of the toner is 5.0 μm or more and 10.0 μm or less, and the density is 0.915 or more and 1.000 or less. , the circularity is 0.900 or more and 0.950 or less, and the inorganic fine particles and the number average primary particle size are 6 to 100 nm as external additives.

Benefits of technology

The leakage of toner is effectively suppressed, the stability in high temperature and high humidity environment is improved, and the thin line reproducibility is significantly improved in continuous printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005057450900000331
    Figure BDA0005057450900000331
Patent Text Reader

Abstract

The invention provides a toner which is not easy to cause toner leakage and has excellent thin line reproducibility. The present invention provides a toner containing colored resin particles and an external additive, the colored resin particles containing a binder resin, a colorant, and a release agent, the toner having a circle area equivalent diameter of 5.0 [mu] m or more and 10.0 [mu] m or less as measured by a flow particle image measurement device, and the compactness obtained as the ratio of the circle area equivalent diameter to the maximum length (circle area equivalent diameter / maximum length) is 0.915-1.000 (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a toner for developing an electrostatic latent image in electrophotography, electrostatic recording, electrostatic printing and the like. Background Art

[0002] In image forming apparatuses such as electrophotographic apparatuses, electrostatic recording apparatuses, and electrostatic printing apparatuses, an electrostatic latent image formed on a photoreceptor is developed with a toner, the toner image is transferred to a transfer material such as paper, and then fixed by heating or the like to form a fixed image.

[0003] Such image forming apparatuses are expected to support high image quality and high-speed printing, and this has led to various requirements for toners. Among them, the phenomenon of toner leakage from the ink cartridge, so-called toner leakage, hinders continuous printing and causes toner loss, so it is strongly desired to eliminate this phenomenon.

[0004] As a means of suppressing toner leakage, Patent Document 1 proposes controlling the bulk density after conditioning obtained using a powder flowability analyzer within a specific range by adjusting the type of external additives, external addition treatment conditions, and the like.

[0005] On the other hand, Patent Document 2 discloses a colorant, which is obtained as follows: a colorant-forming material liquid containing a polyester chain segment, a cross-linking agent (molecular extender), a colorant, a solvent, etc. is dispersed in an aqueous medium to form oil droplets, and molecules are extended in the oil droplets to form polyester resin microparticles, the polyester resin microparticles are agglomerated in the aqueous medium to form colored particles, and an external additive is added to the colored particles to obtain the colorant.

[0006] Patent Documents 1 and 2 propose to use a toner having an average circularity close to 1 in order to improve the reproducibility of thin lines in printing.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: International Publication No. 2018 / 061933;

[0010] Patent document 2: International Publication No. 2010 / 001825. Summary of the invention

[0011] Problem that the invention aims to solve

[0012] However, in the means for suppressing toner leakage described in Patent Document 1, toner leakage sometimes occurs after a long period of time in a high temperature and high humidity environment, and further suppression of toner leakage is required. In addition, even if the circularity of the toner is made close to 1, sufficient fine line reproducibility is sometimes not obtained during continuous printing, and further improvement of fine line reproducibility is required.

[0013] An object of the present invention is to provide a toner which is less likely to cause toner leakage and has excellent thin line reproducibility.

[0014] Solutions for solving problems

[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by controlling the size of toner particles and the macroscopic shape of toner particles, toner leakage can be suppressed and thin line reproducibility can be improved.

[0016] That is, the colorant of the present invention is characterized in that it contains colored resin particles and external additives, the above-mentioned colored resin particles contain a binder resin, a colorant and a release agent, the above-mentioned colorant has a circle area equivalent diameter measured by a flow particle image measuring device of 5.0μm or more and 10.0μm or less, and a compactness calculated as a ratio of the circle area equivalent diameter to the maximum length (circle area equivalent diameter / maximum length) is 0.915 or more and 1.000 or less.

[0017] In the toner of the present invention, the ratio of the maximum inscribed circle diameter of the toner to the circle area equivalent diameter (maximum inscribed circle diameter / circle area equivalent diameter) may be 0.900 or more and 0.950 or less.

[0018] In the toner of the present invention, the circularity of the toner may be 0.900 or more and 0.950 or less.

[0019] The toner of the present invention may contain organic fine particles and inorganic fine particles having a number average primary particle size of 6 to 100 nm as the external additives, and the content of the organic fine particles is 0.05 to 1.0 parts by mass based on 100 parts by mass of the colored resin particles.

[0020] In the toner of the present invention, the content of the inorganic fine particles having a number average primary particle size of 6 to 100 nm may be 0.5 parts by mass or more and 6.5 parts by mass or less relative to 100 parts by mass of the colored resin particles.

[0021] In the toner of the present invention, the inorganic fine particles having a number average primary particle size of 6 to 100 nm may include two or more selected from inorganic fine particles A having a number average primary particle size of 36 to 100 nm, inorganic fine particles B having a number average primary particle size of 15 to 35 nm, and inorganic fine particles C having a number average primary particle size of 6 to 14 nm.

[0022] Effects of the Invention

[0023] As described above, according to the present invention, it is possible to provide a toner which can suppress toner leakage for a long period of time under a high-temperature and high-humidity environment and has excellent thin line reproducibility when performing continuous printing. DETAILED DESCRIPTION

[0024] The colorant of the present invention is characterized in that it contains colored resin particles and external additives, the above-mentioned colored resin particles contain a binder resin, a colorant and a release agent, the colorant has a circle area equivalent diameter measured by a flow particle image measuring device of 5.0 μm or more and 10.0 μm or less, and a compactness calculated as a ratio of the circle area equivalent diameter to the maximum length (circle area equivalent diameter / maximum length) is 0.915 or more and 1.000 or less.

[0025] In order to improve the reproducibility of fine lines, first of all, it is important that the size of the toner particles is sufficiently small. In addition, Patent Document 1 states that from the viewpoint of fine line reproducibility, the circularity of the toner is preferably 0.96 to 1.00, and Patent Document 2 states that from the viewpoint of fine line reproducibility, the circularity of the toner is preferably 0.950 to 0.980. By making the circularity of the toner close to 1, the reproducibility of fine lines is improved, but there is a limit to improving the reproducibility of fine lines by adjusting the circularity.

[0026] The circularity is defined as the value obtained by dividing the diameter of a circle having the same area as the projected image of the particle (circle area equivalent diameter) by the diameter of a circle having the same circumference as the projected image of the particle (circumference equivalent circle diameter). In the case where the particle is a perfect sphere, the circularity is 1, and the more complex the surface shape of the particle, the smaller the circularity value. Thus, the circularity can be used as an indicator of the degree of concavity and convexity of the particle surface. Even if the shape is close to a sphere on a macro scale, the circularity becomes smaller when the degree of concavity and convexity on the surface is large, and even if the shape is flat on a macro scale, the circularity becomes larger when the degree of concavity and convexity on the surface is small. Even if the circularity of the toner is close to 1, it is difficult to exclude toner particles with a flat macroscopic shape. In particular, in the method for manufacturing the toner described in Patent Document 2, it is difficult to make the toner particles close to a sphere by agglomerating polyester resin particles and forming colored particles as toner mother particles, so it is inferred that the toner of Patent Document 2 contains more toner particles with a flat macroscopic shape. In a toner whose circularity is controlled to be close to 1, it is estimated that toner particles having a macroscopically flat shape deteriorate thin line reproducibility, and particularly when the number of printed sheets in continuous printing is large, there is a tendency for thin line reproducibility to deteriorate.

[0027] In contrast, the colorant of the present invention has a circle area equivalent diameter of less than 10.0 μm, the colorant particles are not too large, and further, the density is greater than 0.915, and the macroscopic shape of the colorant particles is close to a sphere. It is speculated that this can further improve the fine line reproducibility compared to adjusting the circularity of the colorant.

[0028] Compactness is defined as the value of dividing the equivalent diameter of the circular area of ​​the particle by the maximum length, that is, the ratio of the equivalent diameter of the circular area to the maximum length (equivalent diameter of the circular area / maximum length). Here, the maximum length of the particle refers to the maximum length of two points on the outline of the projection image of the particle. In the case where the particle is a perfect sphere, the compactness is 1. The more distorted the macroscopic shape of the particle is and the larger the aspect ratio is, the smaller the value of the compactness is. The compactness is not easily affected by the degree of concavity and convexity on the surface of the particle, and therefore can be used as an indicator of the macroscopic shape of the particle. Even if the degree of concavity and convexity on the surface is large, when the macroscopic shape is close to a sphere, the compactness becomes larger. Even if the degree of concavity and convexity on the surface is small, if the macroscopic shape is flatter and the aspect ratio is larger, the compactness becomes smaller. The compactness of the toner of the present invention is greater than 0.915 and less than 1.000, so the proportion of toner particles with a flat shape is reduced.

[0029] In addition, it is speculated that the inclusion of flat toner particles in the toner is one of the causes of toner leakage. Flat toner particles are easy to accumulate, so when flat toner particles are included, it is easy to form agglomerates of toner particles. The formed agglomerates may sometimes invade the sealing parts located at both ends of the developing roller to form gaps in the sealing parts. In addition, the smaller the particle size of the toner particles, the easier it is for the toner to leak from the gaps formed in the sealing parts, so toner leakage is easy to occur.

[0030] In the examples of Patent Document 1, it is shown that in a toner leakage test conducted under a high temperature and high humidity environment, no toner leakage was confirmed within 16 hours of the test time, and the toner of the present invention can suppress toner leakage for a longer period of time. Compared with the toner of Patent Document 1, the toner of the present invention has a reduced amount of flat toner particles, so it is presumed that toner leakage can be suppressed for a longer period of time. As described above, it is presumed that the toner disclosed in Patent Document 2 contains a large number of macroscopically flat toner particles, and it is presumed that toner leakage is likely to occur because agglomerates of toner particles are easily formed.

[0031] In contrast, the density of the colorant of the present invention is above 0.915, and the macroscopic shape of the colorant particles is close to a sphere, so it is not easy for the colorant particles to form agglomerates. Furthermore, the circle area equivalent diameter is above 5.0 μm, and the colorant particles are not too small. Therefore, even if a tiny gap is generated in the sealing portion, it is not easy for the colorant to leak. Therefore, it is presumed that it is not easy for the colorant to leak.

[0032] Furthermore, in the toner of the present invention, by making the circularity greater than 0.900 and less than 0.950, the leakage of the toner can be further suppressed. When comparing toners with the same compactness but different circularities, the higher the circularity of the toner, the fewer the surface irregularities of the toner particles, and thus the van der Waals force acting between the toner particles becomes stronger. Therefore, the cohesive force of the toner also becomes stronger, and it is easy to form an agglomerate. When an agglomerate of the toner particles is formed, as described above, a gap is generated in the sealing portion of the agglomerate, resulting in leakage of the toner. When the compactness is as high as greater than 0.915 and less than 1.000, and the circularity is appropriately as low as greater than 0.900 and less than 0.950, the macroscopic shape of the toner particles is close to a sphere, and there are moderate irregularities on the particle surface. Such toner particles are not easy to accumulate, and the van der Waals force acting between the particles is reduced, so that the cohesive force is further weakened, thereby suppressing the formation of agglomerates of the toner particles and further suppressing the leakage of the toner.

[0033] Hereinafter, after describing the size and shape of the toner which are the characteristics of the toner of the present invention, a method for producing the toner of the present invention and the performance of the toner of the present invention will be described in sequence.

[0034] In addition, in the present invention, "to" in a numerical range means that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0035] 1. Toner size and shape

[0036] In the present invention, each parameter related to the size or shape of the toner is measured using a flow particle image measuring device at an image resolution of 0.185 μm / pixel and is an average value of 1000 to 3000 toner particles selected at random.

[0037] As a flow particle image measuring device, for example, the product name "IF-3200" manufactured by Gasco International Inc. can be preferably used. The measurement sample is prepared by, for example, adding 0.10 to 0.12 g of toner to an aqueous solution of sodium linear alkylbenzene sulfonate (concentration 0.3%), and dispersing the resulting mixed solution for 5 minutes using an ultrasonic cleaner.

[0038] The circle area equivalent diameter of the colorant of the present invention is 5.0 μm or more and 10.0 μm or less. From the viewpoint of suppressing colorant leakage, it is preferably 6.0 μm or more, more preferably 7.0 μm or more. From the viewpoint of improving fine line reproducibility, it is preferably 9.5 μm or less, more preferably 9.0 μm or less, and further preferably 8.0 μm or less.

[0039] In a toner obtained by suspension polymerization, the circle area equivalent diameter of the obtained toner can be adjusted by, for example, adjusting the type and amount of a dispersion stabilizer added, adjusting the dispersion treatment time when droplets are formed, and the like.

[0040] The compactness of the colorant of the present invention is greater than 0.915 and less than 1.000. From the viewpoint of suppressing colorant leakage and improving fine line reproducibility, it is preferably greater than 0.920, more preferably greater than 0.925, and further preferably greater than 0.930. From the viewpoint of ease of manufacturing, it is preferably less than 0.990, more preferably less than 0.980, and further preferably less than 0.970.

[0041] In the colorant obtained by the suspension polymerization method, the conditions during the polymerization reaction are likely to affect the compactness of the colorant. Therefore, the compactness of the obtained colorant can be adjusted by, for example, adjusting the stirring conditions just before providing the suspension to the polymerization reaction, adjusting the heating rate during the polymerization reaction, adjusting the time of the state during the polymerization reaction that can change the particle shape, etc.

[0042] The ratio of the maximum inscribed circle diameter of the colorant to the equivalent diameter of the circle area (maximum inscribed circle diameter / equivalent diameter of the circle area) is not easily affected by the degree of unevenness of the particle surface, just like the compactness, and can therefore be used as an indicator of the macroscopic shape of the particle. Here, the maximum inscribed circle diameter of the colorant refers to the diameter of the circle with the largest area in the circle that can be enclosed by the projection image of the toner particle. In the case where the particle is a perfect sphere, the maximum inscribed circle diameter / equivalent diameter of the circle area is 1. The more distorted the macroscopic shape of the particle is and the larger the aspect ratio is, the smaller the value of the maximum inscribed circle diameter / equivalent diameter of the circle area is. Even if the degree of unevenness of the surface is large, when the macroscopic shape is close to a sphere, the maximum inscribed circle diameter / equivalent diameter of the circle area becomes larger. Even if the degree of unevenness of the surface is small, if the macroscopic shape is flatter and the aspect ratio is larger, the maximum inscribed circle diameter / equivalent diameter of the circle area is smaller.

[0043] The maximum inscribed circle diameter / circle area equivalent diameter of the toner of the present invention is not particularly limited, but is preferably 0.900 or more, more preferably 0.905 or more, and further preferably 0.910 or more from the viewpoint of suppressing toner leakage and improving fine line reproducibility. The maximum inscribed circle diameter / circle area equivalent diameter of the toner of the present invention has an upper limit of 1.000 or less, but is not particularly limited, but is preferably 0.980 or less, more preferably 0.960 or less, and further preferably 0.950 or less from the viewpoint of ease of manufacture.

[0044] In the colorant obtained by the suspension polymerization method, since the conditions during the polymerization reaction are likely to affect the maximum inscribed circle diameter / equivalent circle area diameter of the colorant, the maximum inscribed circle diameter / equivalent circle area diameter of the obtained colorant can be adjusted by, for example, adjusting the stirring conditions just before providing the suspension to the polymerization reaction, adjusting the heating rate during the polymerization reaction, adjusting the time of the state during the polymerization reaction that can change the particle shape, etc.

[0045] The circularity of the colorant of the present invention is not particularly limited. From the viewpoint of suppressing colorant leakage, it is preferably 0.950 or less, more preferably less than 0.950, and further preferably 0.945 or less. On the other hand, from the viewpoint of suppressing the deterioration of the colorant leakage suppression effect and suppressing the deterioration of the fine line reproducibility, it is preferably 0.900 or more, more preferably 0.910 or more, further preferably 0.920 or more, and further preferably 0.930 or more.

[0046] 2. Method for manufacturing toner

[0047] The toner of the present invention is obtained by mixing and stirring colored resin particles containing a binder resin, a colorant and a release agent with an external additive to perform an external addition treatment, thereby attaching the external additive to the surface of the colored resin particles.

[0048] Hereinafter, the method for producing colored resin particles and the method for external addition treatment will be described in order.

[0049] <Method for producing colored resin particles>

[0050] The colored resin particles contained in the toner of the present invention are prepared, for example, by a suspension polymerization method according to the following process.

[0051] (1) Preparation process of polymerizable monomer composition

[0052] First, a polymerizable monomer, a colorant, a release agent, and other additives such as a charge control agent and a molecular weight modifier are mixed as needed to prepare a polymerizable monomer composition. The mixing when preparing the polymerizable monomer composition is performed at a temperature of 35 to 55° C. using a disperser such as a pipeline emulsifier disperser or a medium emulsifier disperser.

[0053] In the present invention, a polymerizable monomer refers to a monomer having a functional group that can be polymerized, and the polymerizable monomer is polymerized to form a binder resin. As the main component of the polymerizable monomer, a monovinyl monomer is preferably used. As a monovinyl monomer, for example, styrene; styrene derivatives such as vinyl toluene and α-methylstyrene; acrylic acid and methacrylic acid; acrylates such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate and dimethylaminoethyl acrylate; methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate and dimethylaminoethyl methacrylate; nitrile compounds such as acrylonitrile and methacrylonitrile; amide compounds such as acrylamide and methacrylamide; olefins such as ethylene, propylene and butene. These monovinyl monomers can be used alone or in combination of two or more. Among these, as a monovinyl monomer, styrene, styrene derivatives, and acrylates or methacrylates are preferably used.

[0054] In order to improve hot offset and improve storage properties, it is preferred to use any cross-linking polymerizable monomer together with the monovinyl monomer. A cross-linking polymerizable monomer refers to a monomer having two or more polymerizable functional groups. As cross-linking polymerizable monomers, aromatic divinyl compounds such as divinylbenzene, divinylnaphthalene and their derivatives can be cited; ester compounds formed by ester bonding of alcohols having two or more hydroxyl groups such as ethylene glycol dimethacrylate and diethylene glycol dimethacrylate with two or more carboxylic acids having carbon-carbon double bonds; other divinyl compounds such as N,N-divinylaniline and divinyl ether; compounds having three or more vinyl groups, etc. These cross-linking polymerizable monomers can be used alone or in combination of two or more.

[0055] When the polymerizable monomer contains the cross-linkable polymerizable monomer, the content of the cross-linkable polymerizable monomer is not particularly limited, but is usually 0.1 to 5 parts by mass, preferably 0.3 to 2 parts by mass, based on 100 parts by mass of the monovinyl monomer.

[0056] Furthermore, when a macromonomer is also used as a part of the polymerizable monomer, the balance between the storage stability and low-temperature fixing property of the obtained toner becomes good, which is preferred.

[0057] As the macromonomer, for example, reactive oligomers and polymers having a carbon-carbon unsaturated double bond that can be polymerized at the end of the molecular chain and a number average molecular weight of generally 1000 to 30000 can be cited. As the above-mentioned macromonomer, for example, styrene macromonomer, styrene-acrylonitrile macromonomer, polyacrylate macromonomer and polymethacrylate macromonomer can be cited. In particular, at least one selected from polyacrylate macromonomers and polymethacrylate macromonomers can be preferably used. As the acrylic acid ester used in the polyacrylate macromonomer, for example, the same acrylic acid ester that can be used as the above-mentioned monovinyl monomer can be cited, and as the methacrylate used in the polymethacrylate macromonomer, for example, the same methacrylate that can be used as the above-mentioned monovinyl monomer can be cited. As the above-mentioned macromonomer, it is particularly preferred to appropriately select a macromonomer that, by including the macromonomer in the above-mentioned polymerizable monomer, has a higher glass transition temperature (Tg) of the adhesive resin than when the macromonomer is not included.

[0058] As the macromonomer, a commercial product may be used. Examples of the commercial product of the macromonomer include macromonomer series AA-6, AS-6, AN-6S, AB-6, and AW-6S manufactured by Toagosei Co., Ltd.

[0059] The above-mentioned macromonomers can be used alone or in combination of two or more.

[0060] When the polymerizable monomer contains the macromonomer, the content of the macromonomer is not particularly limited, but is preferably 0.03 to 5 parts by mass, more preferably 0.05 to 1 part by mass, based on 100 parts by mass of the monovinyl monomer.

[0061] The content of the polymerizable monomer is not particularly limited, but is preferably 60 to 95 parts by mass, more preferably 65 to 90 parts by mass, and even more preferably 70 to 85 parts by mass, based on 100 parts by mass of the total solid content of the polymerizable monomer composition.

[0062] In the present invention, the solid content refers to all components except the solvent, and liquid monomers and the like are also included in the solid content.

[0063] As the colorant, any colorant used in existing toners can be appropriately selected and is not particularly limited. When a color toner is produced, black, cyan, yellow, or magenta colorants can be used.

[0064] As the black colorant, for example, carbon black, titanium black, magnetic powder such as iron zinc oxide and iron nickel oxide, etc. can be used.

[0065] As the cyan colorant, for example, phthalocyanine pigments such as copper phthalocyanine pigments and their derivatives, cyan pigments such as anthraquinone pigments, and cyan dyes can be used. Specifically, for example, CI Pigment Blue 2, 3, 6, 15, 15:1, 15:2, 15:3, 15:4, 16, 17:1, 60; CI Solvent Blue 70, etc. can be mentioned.

[0066] As yellow colorants, for example, azo pigments such as monoazo pigments and disazo pigments, yellow pigments such as condensed polycyclic pigments, and yellow dyes can be used. Specifically, for example, CI Pigment Yellow 3, 12, 13, 14, 15, 17, 62, 65, 73, 74, 83, 93, 97, 120, 138, 155, 180, 181, 185, 186, 213, 214; CI Solvent Yellow 98, 162, etc. can be mentioned.

[0067] As the magenta colorant, for example, azo pigments such as monoazo pigments and disazo pigments, magenta pigments such as condensed polycyclic pigments such as quinacridone pigments, and magenta dyes can be used. Specifically, for example, CI Pigment Red 31, 48, 57:1, 58, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 144, 146, 149, 150, 163, 170, 184, 185, 187, 202, 206, 207, 209, 237, 238, 251, 254, 255, 269; CI Pigment Violet 19; CI Solvent Red 1, 3, 8, 23, 24 4, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1; CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28, etc.

[0068] The above colorants can be used alone or in combination of two or more.

[0069] The content of the colorant is not particularly limited, but is preferably 5 to 15 parts by mass, more preferably 7 to 13 parts by mass, relative to 100 parts by mass of the polymerizable monomer, from the viewpoint of obtaining a sufficient image density. In addition, the content of the colorant in the toner is preferably 5 to 15 parts by mass, more preferably 7 to 13 parts by mass, relative to 100 parts by mass of the binder resin.

[0070] The polymerizable monomer composition contains a release agent. By containing a release agent, the release property of the colorant from the fixing roller during fixing can be improved. As a release agent, as long as it is a release agent or a softener commonly used as a colorant, it can be used without particular limitation. For example, synthetic waxes such as low molecular weight polyolefin waxes and hydrocarbon waxes such as petroleum waxes; ester waxes such as dipentaerythritol esters and carnauba; mineral waxes such as ozokerite, etc. can be cited. From the viewpoint of improving the balance between the storage stability and low-temperature fixing property of the colorant, it is particularly preferred to contain at least one selected from hydrocarbon waxes and ester waxes, and it is more preferred to contain at least ester wax or both hydrocarbon waxes and ester waxes.

[0071] Examples of hydrocarbon waxes include low molecular weight polyolefin waxes such as polyethylene wax and polypropylene wax and modified waxes thereof, synthetic waxes such as Fischer-Tropsch wax, and petroleum waxes such as paraffin wax and microcrystalline wax. Fischer-Tropsch wax and petroleum waxes are particularly preferred, petroleum waxes are more preferred, and paraffin wax is further preferred.

[0072] As the ester wax, a synthetic ester wax obtained by esterifying an alcohol with a carboxylic acid is preferred. As the ester wax, any of a monofunctional ester wax and a polyfunctional ester wax is preferably used, and a polyfunctional ester wax obtained by esterifying a polyhydric alcohol with a monocarboxylic acid is more preferred.

[0073] As the polyfunctional ester wax, at least one selected from the group consisting of pentaerythritol ester compounds, glycerol ester compounds and dipentaerythritol ester compounds can be preferably used. Examples of such preferred polyfunctional ester waxes include pentaerythritol ester compounds such as pentaerythritol tetrapalmitate, pentaerythritol tetrabehenate and pentaerythritol tetrastearate; glycerol ester compounds such as hexaglycerol tetrabehenate tetrapalmitate, hexaglycerol octabehenate, pentaglycerol heptabehenate, tetraglycerol hexabehenate, triglycerol pentabehenate, diglycerol tetrabehenate and glycerol tribehenate; and dipentaerythritol ester compounds such as dipentaerythritol hexamyristate and dipentaerythritol hexapalmitate.

[0074] Examples of the monofunctional ester wax (monoester wax) include behenyl palmitate (C 15 H 31 -COO-C 22 H 45 ), Behenyl Stearate (C 17 H 35 -COO-C 22 H 45 ), behenyl eicosanoate (C 19 H 39 -COO-C 22 H 45 ), behenyl behenate (C 21 H 43 -COO-C 22 H 45 ), eicosyl palmitate (C 15 H31 -COO-C 20 H 41 ), Eicosyl stearate (C 17 H 35 -COO-C 20 H 41 ), eicosyl eicosanoate (C 19 H 39 -COO-C 20 H 41 ), eicosyl behenate (C 21 H 43 -COO-C 20 H 41 ), stearyl stearate (C 17 H 35 -COO-C 18 H 37 ), stearyl eicosanoate (C 19 H 39 -COO-C 18 H 37 ), stearyl behenate (C 21 H 43 -COO-C 18 H 37 ), hexadecyl arachidate (C 19 H 39 -COO-C 16 H 33 ), hexadecyl behenate (C 21 H 43 -COO-C 16 H 33 ) etc. Among these, behenyl stearate, behenyl palmitate, and stearyl behenate are preferred.

[0075] The weight average molecular weight Mw of the release agent is not particularly limited, but is preferably within a range of 400 to 3500, more preferably 500 to 3000.

[0076] In the case of ester wax, after extraction with a solvent, it is decomposed into alcohol and carboxylic acid by hydrolysis to perform composition analysis, and the molecular weight can be calculated from the structural formula. The result of the weight average molecular weight Mw of the ester wax is the same as the result of the molecular weight calculated from the structural formula.

[0077] The melting point of the release agent is preferably within a range of 50 to 90°C, more preferably within a range of 60 to 85°C, further preferably within a range of 65 to 80°C, and further preferably within a range of 65 to 75°C.

[0078] The content of the release agent is not particularly limited, but is preferably 1 to 30 parts by mass, more preferably 5 to 20 parts by mass, relative to 100 parts by mass of the polymerizable monomer, from the viewpoint of improving the balance between the storage stability and low-temperature fixing property of the toner. In addition, the content of the release agent in the toner is preferably 1 to 30 parts by mass, more preferably 5 to 20 parts by mass, relative to 100 parts by mass of the binder resin.

[0079] The polymerizable monomer composition preferably contains a positively or negatively chargeable charge control agent, thereby improving the chargeability of the toner.

[0080] The charge control agent is not particularly limited as long as it is a charge control agent commonly used as a charge control agent for colorants. Among the charge control agents, positively or negatively charge control resins are preferred from the viewpoint of high compatibility with polymerizable monomers and ability to impart stable charge properties (charge stability) to the colorant particles.

[0081] As a positively or negatively charged charge control resin, a functional group-containing copolymer can be used. As a positively charged charge control resin, a functional group-containing copolymer containing a structural unit containing a functional group such as an amino group, a quaternary ammonium group or a quaternary ammonium salt group can be used, and examples thereof include polyamine resins, quaternary ammonium group-containing copolymers and quaternary ammonium salt group-containing copolymers. As a negatively charged charge control resin, a functional group-containing copolymer containing a structural unit containing a sulfonic acid group, a sulfonate group, a carboxylic acid group or a carboxylate group can be used, and examples thereof include sulfonic acid group-containing copolymers, sulfonate group-containing copolymers, carboxylic acid group-containing copolymers and carboxylate group-containing copolymers.

[0082] The glass transition temperature (Tg) of the charge control resin is preferably 60 to 90° C., more preferably 65 to 85° C., and further preferably 70 to 80° C. When it is within the above range, the balance between storage stability and fixability is good.

[0083] The weight average molecular weight (Mw) of the charge control resin is preferably 8000 to 28000, more preferably 10000 to 25000, and further preferably 15000 to 23000. When the weight average molecular weight (Mw) is above the above lower limit, the reduction in storage stability and printing durability can be suppressed, and when it is below the above upper limit, the reduction in fixability can be suppressed. In addition, when the weight average molecular weight (Mw) is within the above range, the charge control resin can be well dispersed in the polymerizable monomer composition, so it is easy to obtain a toner that is given a stable charge over time.

[0084] As the charge control agent, a charge control agent other than the charge control resin may be contained.

[0085] Examples of the charge control agent other than the positively chargeable charge control resin include nigrosine dyes, quaternary ammonium salts, triaminotriphenylmethane compounds, and imidazole compounds.

[0086] Examples of the charge control agent other than the negatively chargeable charge control resin include azo dyes containing metals such as Cr, Co, Al, and Fe, salicylic acid metal compounds, and alkyl salicylic acid metal compounds.

[0087] The content of the charge control agent is usually 0.1 to 10 parts by mass, preferably 0.3 to 5 parts by mass, and more preferably 0.6 to 2 parts by mass relative to 100 parts by mass of the polymerizable monomer. In addition, the content of the charge control agent in the toner is usually 0.1 to 10 parts by mass, preferably 0.3 to 5 parts by mass, and more preferably 0.6 to 2 parts by mass relative to 100 parts by mass of the binder resin.

[0088] When the content of the charge control agent is within the above range, the printing performance is likely to be good. In addition, when the content of the charge control agent is above the above lower limit, the generation of fog can be suppressed, and when it is below the above upper limit, printing contamination can be suppressed.

[0089] The polymerizable monomer composition may also contain a polar resin. When the colored resin particles contain a polar resin, the storage property and printing durability of the toner can be improved. The polar resin tends to be concentrated on the surface side of the colored resin particles, reinforces the particle surface, and inhibits the degradation of the colored resin particles, thereby improving the storage property and printing durability of the toner.

[0090] As the polar resin, a copolymer containing an acidic group is preferably used, and an acrylate copolymer having an acidic group is particularly preferred. As the acrylate copolymer having an acidic group, for example, a copolymer of (meth)acrylate and (meth)acrylic acid is preferably used. In addition, the copolymer of (meth)acrylate and (meth)acrylic acid is a copolymer of at least one selected from acrylate and methacrylate and at least one selected from acrylic acid and methacrylic acid.

[0091] Examples of the copolymer include copolymers of acrylate and acrylic acid, copolymers of acrylate and methacrylic acid, copolymers of methacrylate and acrylic acid, copolymers of methacrylate and methacrylic acid, copolymers of acrylate, methacrylate and acrylic acid, copolymers of acrylate, methacrylate and methacrylic acid, and copolymers of acrylate, methacrylate, acrylic acid and methacrylic acid, etc. Among them, copolymers of acrylate, methacrylate and acrylic acid are preferred.

[0092] Examples of the (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, sec-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, neohexyl (meth)acrylate, sec-hexyl (meth)acrylate, and tert-hexyl (meth)acrylate.

[0093] As the acrylic acid ester, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, and n-butyl acrylate are particularly preferred, and ethyl acrylate and n-butyl acrylate are more preferred.

[0094] As the methacrylate, methyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, and n-butyl methacrylate are particularly preferred, and methyl methacrylate is more preferred.

[0095] It is preferred that the mass ratio of each monomer unit constituting the acrylic ester-based copolymer be adjusted so as to satisfy the acid value and glass transition temperature Tg described below.

[0096] The lower limit of the content of the (meth)acrylic acid unit in 100% by mass of all monomer units constituting the above-mentioned acrylic ester copolymer is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, and further preferably 0.3% by mass or more, and the upper limit is preferably 1.0% by mass or less, more preferably 0.6% by mass or less, and further preferably 0.5% by mass or less.

[0097] The lower limit of the content of the (meth)acrylate unit in 100% by mass of all monomer units constituting the above-mentioned acrylate copolymer is preferably 99.0% by mass or more, more preferably 99.4% by mass or more, and further preferably 99.5% by mass or more, and the upper limit is preferably 99.95% by mass or less, more preferably 99.9% by mass or less, and further preferably 99.7% by mass or less.

[0098] The above-mentioned acrylate copolymer may also contain other monomer units different from the (meth)acrylate unit and the (meth)acrylic acid unit within the scope that does not impair the purpose of the present invention. As such other monomers, for example, styrene derivatives, nitrile compounds and amide compounds exemplified in the monovinyl monomer constituting the above-mentioned binder resin can be cited.

[0099] In the acrylic ester copolymer, the content of the other monomer units is preferably 10% by mass or less, more preferably 2% by mass or less, and most preferably 0% by mass, based on 100% by mass of the (meth)acrylic ester units.

[0100] The acid value of the polar resin is not particularly limited, but is preferably 0.5 mgKOH / g or more, more preferably 1.0 mgKOH / g or more, and further preferably 2.0 mgKOH / g or more as the lower limit, and is preferably 5.0 mgKOH / g or less, more preferably 4.0 mgKOH / g or less, and further preferably 3.0 mgKOH / g or less as the upper limit. When the acid value of the polar resin is within the above range, a toner having excellent low-temperature fixability, storage stability, and printing durability can be easily obtained.

[0101] In the present invention, the acid value of the resin can be measured in accordance with JIS K 0070.

[0102] The weight average molecular weight (Mw) of the polar resin is not particularly limited, but is preferably 6,000 or more, more preferably 7,000 or more, and further preferably 9,000 or more as the lower limit, and is preferably 50,000 or less, more preferably 45,000 or less, and further preferably 40,000 or less as the upper limit.

[0103] When the weight average molecular weight (Mw) of the polar resin is within the above range, a toner excellent in low-temperature fixing ability, storage stability, and printing durability can be easily obtained.

[0104] The glass transition temperature Tg of the polar resin is not particularly limited, but is preferably 60°C or higher, more preferably 65°C or higher, and further preferably 70°C or higher as the lower limit, and is preferably 85°C or lower, more preferably 80°C or lower, and further preferably 77°C or lower as the upper limit.

[0105] When the glass transition temperature Tg of the polar resin is within the above range, a toner excellent in low-temperature fixing ability, storage stability, and printing durability can be easily obtained.

[0106] In addition, the glass transition temperature Tg can be obtained according to ASTM D3418-82.

[0107] Relative to 100 parts by mass of the binder resin, the lower limit of the polar resin content is preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, and further preferably 1 part by mass or more, and the upper limit is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, further preferably 2 parts by mass or less, and further preferably 1.5 parts by mass or less.

[0108] When the content of the polar resin is above the lower limit, the reduction in printing durability can be suppressed. When it is below the upper limit, the charge amount of the colorant tends to become moderate, especially suppressing the reduction in the charge amount of the colorant. In addition, the reduction in production stability and the reduction in low-temperature fixing properties are suppressed.

[0109] The polar resin may be a commercially available product, or may be produced by a known polymerization method such as solution polymerization, aqueous solution polymerization, ion polymerization, high temperature and high pressure polymerization, or suspension polymerization.

[0110] Typical examples of the method for producing the polar resin are as follows. In addition, the method for producing the polar resin is not limited to the following typical examples.

[0111] First, a solvent is appropriately added to a reaction vessel, and after replacing the reaction vessel with an inactive environment, the temperature is raised, and the raw monomer is added to the reaction vessel. At this time, a polymerization initiator is preferably added together. In addition, a mixture of the raw monomer and the polymerization initiator is preferably slowly added dropwise to the reaction vessel. Next, the temperature is raised to a temperature for performing a polymerization reaction, and polymerization is initiated. After the polymerization is completed, the desired polar resin can be obtained by appropriately distilling off the solvent.

[0112] In the polymerizable monomer composition, when polymerizing the polymerizable monomer, it is preferred to use a molecular weight modifier as another additive.

[0113] The molecular weight modifier is not particularly limited as long as it is a molecular weight modifier generally used as a molecular weight modifier for toners, and examples thereof include mercaptans such as tert-dodecyl mercaptan, n-dodecyl mercaptan, n-octyl mercaptan, and 2,2,4,6,6-pentamethylheptane-4-mercaptan; thiuram disulfides such as tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, N,N′-dimethyl-N,N′-diphenylthiuram disulfide, and N,N′-dioctadecyl-N,N′-diisopropylthiuram disulfide, etc. These molecular weight modifiers may be used alone or in combination of two or more.

[0114] The content of the molecular weight modifier is usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the monovinyl monomer.

[0115] (2) Suspension step of obtaining a suspension (droplet formation step)

[0116] Next, the polymerizable monomer composition is dispersed in an aqueous medium containing a dispersion stabilizer, and after adding a polymerization initiator, droplets of the polymerizable monomer composition are formed. The polymerization initiator may be added after the polymerizable monomer composition is dispersed in the aqueous medium and before droplets are formed as described above, or may be added to the polymerizable monomer composition before being dispersed in the aqueous medium.

[0117] As polymerization initiators, persulfates such as potassium persulfate and ammonium persulfate can be cited; azo compounds such as 4,4′-azobis(4-cyanovaleric acid), 2,2′-azobis(2-methyl-N-(2-hydroxyethyl)propionamide), 2,2′-azobis(2-amidinopropane)dichloride, 2,2′-azobis(2,4-dimethylvaleronitrile), and 2,2′-azobisisobutyronitrile; organic peroxides such as di-tert-butyl peroxide, benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-2-ethylbutyrate, tert-hexyl peroxy-2-ethylbutyrate, tert-butyl peroxydiethylacetate, diisopropyl peroxydicarbonate, di-tert-butyl peroxyisophthalate, and tert-butyl peroxyisobutyrate. Among these, organic peroxides are preferably used from the viewpoint of being able to reduce residual polymerizable monomers and having excellent printing durability. Among organic peroxides, peroxy esters are preferred, and non-aromatic peroxy esters, ie, peroxy esters having no aromatic ring, are more preferred, from the viewpoint of good initiator efficiency and ability to reduce residual polymerizable monomers.

[0118] These polymerization initiators can be used alone or in combination of two or more.

[0119] The amount of the polymerization initiator used for polymerization of the polymerizable monomer composition is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the monovinyl monomer.

[0120] In the present invention, the aqueous medium refers to a medium containing water as a main component, and is typically water.

[0121] The aqueous medium preferably contains a dispersion stabilizer. Examples of the dispersion stabilizer include sulfates such as barium sulfate and calcium sulfate; carbonates such as barium carbonate, calcium carbonate, and magnesium carbonate; phosphates such as calcium phosphate; metal oxides such as aluminum oxide and titanium oxide; metal hydroxides such as aluminum hydroxide, magnesium hydroxide, and ferrous hydroxide; inorganic compounds such as silicon dioxide; water-soluble polymers such as polyvinyl alcohol, methylcellulose, and gelatin; anionic surfactants; nonionic surfactants; organic compounds such as amphoteric surfactants. The above-mentioned dispersion stabilizers can be used alone or in combination of two or more.

[0122] Among the above-mentioned dispersion stabilizers, inorganic compounds, especially colloids of poorly water-soluble metal hydroxides, are preferred. By using inorganic compounds, especially colloids of poorly water-soluble metal hydroxides, the particle size distribution of the colored resin particles can be narrowed, and the amount of the dispersion stabilizer remaining after washing can be reduced, so that the obtained toner can reproduce images clearly and has excellent environmental stability.

[0123] The poorly water-soluble metal hydroxide colloid can be prepared, for example, by reacting at least one selected from an alkali metal hydroxide and an alkaline earth metal hydroxide with a water-soluble polyvalent metal salt (excluding an alkaline earth metal hydroxide) in an aqueous medium.

[0124] Examples of the alkali metal hydroxide salt include lithium hydroxide, sodium hydroxide, potassium hydroxide, etc. Examples of the alkaline earth metal hydroxide salt include barium hydroxide, calcium hydroxide, etc.

[0125] As the water-soluble polyvalent metal salt, any polyvalent metal salt showing water solubility other than the compounds belonging to the above-mentioned alkaline earth metal hydroxide salts may be mentioned, for example, magnesium metal salts such as magnesium chloride, magnesium phosphate, and magnesium sulfate; calcium metal salts such as calcium chloride, calcium nitrate, calcium acetate, and calcium sulfate; aluminum metal salts such as aluminum chloride and aluminum sulfate; barium salts such as barium chloride, barium nitrate, and barium acetate; zinc salts such as zinc chloride, zinc nitrate, and zinc acetate, etc. Among them, magnesium metal salts, calcium metal salts, and aluminum metal salts are preferred, magnesium metal salts are more preferred, and magnesium chloride is particularly preferred.

[0126] The method for reacting at least one selected from the above-mentioned alkali metal hydroxides and alkaline earth metal hydroxides with the above-mentioned water-soluble polyvalent metal salt in an aqueous medium is not particularly limited, and an example includes a method of mixing an aqueous solution of at least one selected from the above-mentioned alkali metal hydroxides and alkaline earth metal hydroxides with an aqueous solution of a water-soluble polyvalent metal salt.

[0127] Alternatively, colloidal silica may be used as a colloidal dispersion containing colloidal particles of a poorly water-soluble inorganic compound.

[0128] The content of the dispersion stabilizer is appropriately adjusted in a manner to obtain a toner with a desired particle size, and is not particularly limited. It is preferably 0.5 to 10 parts by mass, and more preferably 1.0 to 8.0 parts by mass, relative to 100 parts by mass of the polymerizable monomer in the above-mentioned polymerizable monomer composition. By making the content of the dispersion stabilizer above the above-mentioned lower limit, the droplets of the polymerizable monomer composition can be fully dispersed in the suspension without being combined. On the other hand, by making the content of the dispersion stabilizer below the above-mentioned upper limit, the viscosity of the suspension can be prevented from increasing during granulation, avoiding the failure of the suspension clogging the granulator.

[0129] The content of the dispersion stabilizer is usually 1 to 15 parts by mass, preferably 1 to 8 parts by mass, relative to 100 parts by mass of the aqueous medium.

[0130] By adding the polymerizable monomer composition to an aqueous medium containing a dispersion stabilizer and vigorously stirring the composition, a suspension in which droplets of the polymerizable monomer composition are dispersed in the aqueous medium can be obtained.

[0131] The vigorous stirring for forming droplets of the polymerizable monomer composition is not particularly limited, and can be carried out using a disperser such as Milder (: trade name) manufactured by Ohyo Kiko Co., Ltd., Cavitron (: trade name) manufactured by Eurotec, a horizontal or vertical pipeline disperser such as a pipeline disperser manufactured by IKA (for example, DISPAX-REACTOR (registered trademark) DRS (: trade name)); an emulsifying disperser such as the HOMOMIXER MARK II series manufactured by PRIMIX Co., Ltd.

[0132] The time of stirring performed in the suspension step is appropriately adjusted according to the amount of the polymerizable monomer composition and is not particularly limited.

[0133] In addition, the particle size of the toner particles, that is, the equivalent circle area diameter, can be adjusted by adjusting the stirring conditions in the suspension process. The stirring conditions in the suspension process have little effect on the compactness and the maximum inscribed circle diameter / equivalent circle area diameter of the toner.

[0134] (3) Polymerization process

[0135] After droplets of the polymerizable monomer composition are formed as in the above-mentioned (2), the polymerizable monomer composition is subjected to a polymerization reaction in the presence of a polymerization initiator to form colored resin particles. That is, a suspension in which droplets of the polymerizable monomer composition are dispersed is heated to allow the polymerization reaction of the polymerizable monomer to proceed, thereby obtaining an aqueous dispersion of colored resin particles.

[0136] In the present invention, from the viewpoint of obtaining a toner having a desired compactness and maximum inscribed circle diameter / circle area equivalent diameter, it is preferred that before heating the suspension to the polymerization reaction temperature, stirring is performed under the conditions of a front end speed of a stirring blade of 0.8 to 2.5 m / s and a stirring time of 5 minutes to 10 hours. The stirring conditions are preferably appropriately adjusted in a manner to obtain a toner having a desired compactness and maximum inscribed circle diameter / circle area equivalent diameter, and are not particularly limited. The lower limit of the front end speed of the stirring blade is more preferably 0.9 m / s or more, and the upper limit is more preferably 2.0 m / s or less, more preferably 1.8 m / s or less, and even more preferably 1.6 m / s or less. The upper limit of the stirring time is more preferably 8 hours or less, and even more preferably 6 hours or less.

[0137] In addition, the tip speed of the stirring blade can be calculated by the following formula.

[0138] Stirring blade tip speed (m / s) = circumference × stirring blade diameter (m) × speed (s -1 )

[0139] Here, the stirring blade diameter is a value twice the maximum value of the straight line distance from the central axis of the shaft to the front end of the stirring blade when the stirring blade is viewed in the central axis direction of the shaft.

[0140] The temperature during stirring of the suspension before initiating the polymerization reaction is not particularly limited, but is preferably 35 to 55° C., more preferably 40 to 50° C., from the viewpoint of preventing the release agent dissolved in the droplets from precipitating and inhibiting the progress of the polymerization reaction.

[0141] By stirring the suspension before the initiation of the polymerization reaction under the above-mentioned conditions and continuing to stir during the polymerization reaction, the collision between the droplets can be suppressed and the shear force applied to the droplets can be reduced. It is speculated that a colorant with the desired compactness and maximum inscribed circle diameter / circle area equivalent diameter can be obtained.

[0142] The heating temperature when the suspension is subjected to the polymerization reaction is not particularly limited. From the viewpoint of causing the polymerization reaction to proceed rapidly, it is preferably 60° C. or higher, more preferably 70° C. or higher. On the other hand, from the viewpoint of suppressing the rapid polymerization reaction and stabilizing the quality of the obtained toner, it is preferably 95° C. or lower.

[0143] The heating time is preferably 1 to 20 hours, more preferably 2 to 15 hours.

[0144] In addition, from the viewpoint of obtaining a toner having a desired compactness and maximum inscribed circle diameter / circle area equivalent diameter, it is preferred that the dispersion in the polymerization reaction be stirred at a stirring blade tip speed of 0.8 to 2.5 m / s. The stirring conditions are preferably appropriately adjusted so as to obtain a toner having a desired compactness and maximum inscribed circle diameter / circle area equivalent diameter, and are not particularly limited. The lower limit of the stirring blade tip speed is more preferably 0.9 m / s or more, and the upper limit is more preferably 2.0 m / s or less, further preferably 1.8 m / s or less, and further preferably 1.6 m / s or less. From the viewpoint of obtaining a toner having a desired compactness and maximum inscribed circle diameter / circle area equivalent diameter, in the polymerization reaction of the polymerizable monomer composition, it is preferred that the dispersion be stirred at the same stirring blade tip speed as that used for stirring the suspension before initiating the polymerization reaction.

[0145] In the present invention, the colored resin particles obtained by the above-mentioned polymerization process may be used as a toner by adding an external additive, but the colored resin particles obtained by the above-mentioned polymerization process are preferably used as the core layer of the so-called core-shell type (or also called "capsule type") colored resin particles. The core-shell type colored resin particles have a structure in which the outer side of the core layer is coated with a shell layer formed using a material different from the core layer. By coating the core layer composed of a material having a low softening point with a material having a higher softening point than the core layer, the low-temperature fixability and storage property of the toner can be improved in a balanced manner.

[0146] The method for producing the core-shell type colored resin particles using the colored resin particles obtained by the above-mentioned polymerization step is not particularly limited, and the core-shell type colored resin particles can be produced by a conventionally known method. From the viewpoint of production efficiency, an in-situ polymerization method or a phase separation method is preferred.

[0147] Hereinafter, a method for producing core-shell type colored resin particles using an in-situ polymerization method will be described.

[0148] Core-shell type colored resin particles can be obtained by adding a polymerizable monomer for forming a shell layer (shell polymerizable monomer) and a polymerization initiator to an aqueous dispersion in which colored resin particles are dispersed, and performing polymerization.

[0149] As the polymerizable monomer for the shell, the same monomers as those described above can be used. In particular, it is preferred to use monomers that can give a polymer having a Tg of more than 80° C., such as styrene, acrylonitrile, and methyl methacrylate, alone or in combination of two or more.

[0150] Examples of polymerization initiators used for polymerization of the polymerizable monomer for the shell include metal persulfate salts such as potassium persulfate and ammonium persulfate, and water-soluble polymerization initiators such as azo initiators such as 2,2′-azobis(2-methyl-N-(2-hydroxyethyl)propionamide) and 2,2′-azobis(2-methyl-N-(1,1-bis(hydroxymethyl)-2-hydroxyethyl)propionamide). These can be used alone or in combination of two or more.

[0151] The amount of the polymerization initiator is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the polymerizable monomer for a shell.

[0152] The polymerization temperature of the shell layer is not particularly limited, but is preferably 60° C. or higher, more preferably 70° C. or higher, from the viewpoint of rapidly advancing the polymerization reaction, and is preferably 95° C. or lower from the viewpoint of suppressing volatilization of the polymerizable monomer for the shell.

[0153] The reaction time for the polymerization of the shell layer is preferably 1 to 20 hours, more preferably 2 to 15 hours.

[0154] From the viewpoint of making the polymerizable monomer for the shell uniformly adhere to the core layer, the dispersion in the polymerization reaction of the shell layer is preferably stirred at a tip speed of the stirring blade of 0.8 to 2.5 m / s. In addition, the polymerization conditions of the shell layer have little effect on the compactness and the maximum inscribed circle diameter / circle area equivalent diameter of the toner.

[0155] (4) Cleaning, filtering, dehydration and drying processes

[0156] After the polymerization is completed, it is preferred that a series of operations of washing, filtering, dehydrating and drying the aqueous dispersion of the colored resin particles obtained by the polymerization be repeated several times as necessary according to a conventional method.

[0157] As the above-mentioned cleaning method, when an inorganic compound is used as a dispersion stabilizer, it is preferred to remove the dispersion stabilizer by adding an acid or an alkali to the aqueous dispersion of the colored resin particles so that the dispersion stabilizer is dissolved in water. When a colloid of a poorly water-soluble inorganic hydroxide is used as a dispersion stabilizer, it is preferred to add an acid to adjust the pH of the aqueous dispersion of the colored resin particles to 6.5 or less. As the acid to be added, inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as formic acid and acetic acid can be used. Sulfuric acid is particularly preferred from the viewpoint of high removal efficiency and low burden on manufacturing equipment.

[0158] The dehydration and filtration methods can use various known methods, etc., and are not particularly limited. For example, centrifugal filtration, vacuum filtration, pressure filtration, etc. can be mentioned. In addition, the drying method is also not particularly limited, and various methods can be used.

[0159] In the present invention, the binder resin contained in the colored resin particles is typically a polymer of the above-mentioned polymerizable monomers, and may also contain a small amount of polyester resins, epoxy resins, etc., which have been widely used as binder resins for toners, and unreacted polymerizable monomers. The content of the polyester resin contained in 100 parts by mass of the above-mentioned binder resin is particularly preferably 5 parts by mass or less, more preferably 1 part by mass or less, and further preferably 0.1 parts by mass or less, and it is particularly preferred that the polyester resin is not contained. By making the content of the polyester resin below the above-mentioned upper limit, the environmental stability of the toner can be improved, and in particular, the change in the charge of the toner caused by humidity changes can be suppressed.

[0160] In addition, when the above-mentioned adhesive resin contains a resin other than the polymer of the above-mentioned polymerizable monomer, the content of the polymer of the above-mentioned polymerizable monomer in 100 parts by mass of the adhesive resin is preferably 95 parts by mass or more, more preferably 97 parts by mass or more, and further preferably 99 parts by mass or more.

[0161] <External addition treatment method>

[0162] The toner of the present invention can be processed by external addition by mixing and stirring the colored resin particles obtained by the above method with an external additive, so that the external additive is attached to the surface of the colored resin particles to form a single-component toner (developer). In addition, the single-component toner can be further mixed and stirred with mixed carrier particles to form a two-component developer.

[0163] As a method for external addition treatment for attaching the external additive to the surface of the colored resin particles, a known external addition treatment method can be adopted without particular limitation. For example, a mixer capable of mixing and stirring, such as Henschel mixer (: trade name, manufactured by Mitsui Mining Co., Ltd.), FM Mixer (: trade name, manufactured by Nippon Coking Industry Co., Ltd.), Super Mixer (: trade name, manufactured by Kawada Manufacturing Co., Ltd.), Q Mixer (: trade name, manufactured by Nippon Coking Industry Co., Ltd.), Mechanofusion System (: trade name, manufactured by Hosokawa Micron Co., Ltd.), and Mechano Mill (: trade name, manufactured by Okada Seiko Co., Ltd.), can be used to mix and stir the colored resin particles and the external additive, thereby performing external addition treatment.

[0164] The peripheral speed of the stirring blade during the external addition treatment is not particularly limited, but is preferably 30 to 50 m / s. The time for the external addition treatment is not particularly limited, but is preferably 1 to 15 minutes.

[0165] The toner of the present invention preferably contains any one of the inorganic fine particles A to C described below as an external additive, that is, preferably contains inorganic fine particles with a number average primary particle size of 6 to 100 nm, more preferably contains any two, and further preferably contains all three. By appropriately adjusting the particle size and addition amount of the inorganic fine particles A to C, the low-temperature fixability and storage stability of the toner can be improved in a balanced manner.

[0166] The inorganic particles A are inorganic particles having a number average primary particle size of 36 to 100 nm. When the number average primary particle size of the inorganic particles A is less than 36 nm, the spacing effect is reduced, and sometimes fogging and the like are generated, which have an adverse effect on the printing performance. On the other hand, when the number average primary particle size of the inorganic particles A is greater than 100 nm, the inorganic particles A are easily freed from the surface of the toner particles, and the function as an external additive is reduced, which sometimes has an adverse effect on the printing performance.

[0167] The lower limit of the number average primary particle size of the inorganic fine particles A is more preferably 40 nm or more, and further preferably 45 nm, and the upper limit is more preferably 80 nm or less, and further preferably 70 nm or less.

[0168] Furthermore, the inorganic fine particles A are preferably subjected to a hydrophobic treatment.

[0169] In the present invention, as the hydrophobizing agent, for example, a silane coupling agent, silicone oil, fatty acid, fatty acid metal salt, etc. can be used. Among these, a silane coupling agent and silicone oil are preferred.

[0170] The lower limit of the content of the inorganic fine particles A relative to 100 parts by mass of the colored resin particles is preferably 0.30 parts by mass or more, more preferably 0.50 parts by mass or more, and further preferably 1.00 parts by mass or more, and the upper limit is preferably 3.00 parts by mass or less, more preferably 2.50 parts by mass or less, and further preferably 2.00 parts by mass or less.

[0171] When the content of inorganic particles A is above the above lower limit, inorganic particles A can fully exert their function as an external additive, thereby suppressing the deterioration of printing performance or storage stability. On the other hand, when the content of inorganic particles A is below the above upper limit, the deterioration of printing performance is suppressed by suppressing the release of inorganic particles A from the surface of the toner particles.

[0172] The inorganic particles B are inorganic particles having a number average primary particle size of 15 to 35 nm. When the number average primary particle size of the inorganic particles B is less than 15 nm, the inorganic particles B are easily buried from the surface of the colored resin particles to the inside, so that the toner particles cannot be sufficiently given fluidity, which sometimes has an adverse effect on the printing performance. On the other hand, when the number average primary particle size of the inorganic particles B is greater than 35 nm, the proportion (coverage) of the inorganic particles B on the surface of the toner particles is reduced, so that the toner particles cannot be sufficiently given fluidity.

[0173] The lower limit of the number average primary particle size of the inorganic fine particles B is more preferably 17 nm or more, and further preferably 20 nm, and the upper limit is more preferably 30 nm or less, and further preferably 25 nm or less.

[0174] Furthermore, the inorganic fine particles B are preferably subjected to a hydrophobic treatment.

[0175] The lower limit of the content of the inorganic fine particles B relative to 100 parts by mass of the colored resin particles is preferably 0.10 parts by mass or more, more preferably 0.30 parts by mass or more, and further preferably 0.50 parts by mass or more, and the upper limit is preferably 2.00 parts by mass or less, more preferably 1.50 parts by mass or less, and further preferably 1.00 parts by mass or less.

[0176] When the content of the inorganic fine particles B is above the above lower limit, the inorganic fine particles B can fully exert their function as an external additive, thereby suppressing the reduction of fluidity and suppressing the deterioration of storage properties or durability. On the other hand, when the content of the inorganic fine particles B is below the above upper limit, the inorganic fine particles B are suppressed from being freed from the surface of the toner particles, thereby suppressing the deterioration of the charging characteristics, thereby suppressing the generation of fog.

[0177] The inorganic particles C are inorganic particles having a number average primary particle size of 6 to 14 nm. When the number average primary particle size of the inorganic particles C is less than 6 nm, the inorganic particles C are easily buried from the surface of the colored resin particles to the inside, so that the toner particles cannot be sufficiently given fluidity, which sometimes has an adverse effect on the printing performance. On the other hand, when the number average primary particle size of the inorganic particles C is greater than 14 nm, the proportion (coverage) of the inorganic particles C on the surface of the toner particles is reduced, so that the toner particles cannot be sufficiently given fluidity.

[0178] The lower limit of the number average primary particle size of the inorganic fine particles C is more preferably 6.5 nm or more, and further preferably 7.0 nm, and the upper limit is more preferably 12 nm or less, and further preferably 10 nm or less.

[0179] Furthermore, it is preferred that the inorganic fine particles C be subjected to a hydrophobic treatment.

[0180] The lower limit of the content of the inorganic fine particles C relative to 100 parts by mass of the colored resin particles is preferably 0.10 parts by mass or more, more preferably 0.15 parts by mass or more, and further preferably 0.20 parts by mass or more, and the upper limit is preferably 1.50 parts by mass or less, more preferably 1.00 parts by mass or less, further preferably 0.80 parts by mass or less, and further preferably 0.60 parts by mass or less.

[0181] When the content of the inorganic fine particles C is above the above lower limit, the inorganic fine particles C can fully exert their function as an external additive, thereby suppressing the decrease in fluidity and suppressing the deterioration of storage stability. On the other hand, when the content of the inorganic fine particles C is below the above upper limit, the inorganic fine particles C are suppressed from being freed from the surface of the toner particles, thereby suppressing the deterioration of the charging characteristics, thereby suppressing the generation of fog.

[0182] Examples of inorganic particles A to C include silicon dioxide, titanium oxide, aluminum oxide, zinc oxide, tin oxide, calcium carbonate, calcium phosphate, cerium oxide, barium titanate, and strontium titanate. The materials of the inorganic particles A to C may be different from each other, but are preferably composed of the same material. The inorganic particles A to C preferably contain at least one selected from silicon dioxide and titanium oxide, and more preferably are all silicon dioxide particles.

[0183] As the inorganic fine particles A, various commercially available silica fine particles can be used, for example, VPNA50H (: trade name, number average primary particle size: 40 nm) manufactured by Nippon Aerosil Co., Ltd., H05TA (: trade name, number average primary particle size: 50 nm) manufactured by Clariant, etc.

[0184] As the inorganic fine particles B, various commercially available silica fine particles can be used, for example, NA50Y (: trade name, number average primary particle size: 35 nm) manufactured by Nippon Aerosil Co., Ltd.; MSP-012 (: trade name, number average primary particle size: 16 nm) manufactured by Tayca Corporation; TG-7120 (: trade name, number average primary particle size: 20 nm) manufactured by Cabot Corporation, etc.

[0185] As the inorganic fine particles C, various commercially available silica fine particles can be used, for example, HDK2150 (: trade name, number average primary particle size: 12 nm) manufactured by Clariant; R504 (: trade name, number average primary particle size: 12 nm) and RA200HS (: trade name, number average primary particle size: 12 nm) manufactured by Nippon Aerosil; MSP-013 (: trade name, number average primary particle size: 12 nm) manufactured by Tayca Corporation; TG-820F (: trade name, number average primary particle size: 7 nm) manufactured by Cabot Corporation, etc.

[0186] The content of the inorganic fine particles having a number average primary particle size of 6 to 100 nm contained as an external additive, that is, the total content of the inorganic fine particles A to C is not particularly limited, but is preferably 0.50 parts by mass or more, more preferably 1.00 parts by mass or more, and further preferably 1.70 parts by mass or more, as a lower limit, and is preferably 6.50 parts by mass or less, more preferably 5.00 parts by mass or less, and further preferably 4.00 parts by mass or less, relative to 100 parts by mass of the colored resin particles.

[0187] In addition, the toner of the present invention preferably contains organic particles as an external additive. As the organic particles, it is preferred to contain organic particles D having a number average primary particle size of 1.0 μm or less. When the organic particles D are contained as an external additive, the aggregation of the toner can be suppressed, so that the leakage of the toner can be suppressed, and filming on the photoreceptor is not likely to occur, and the toner particles are given a stable charge property over time, so that even if a large number of sheets are continuously printed, it is not easy to cause the deterioration of the image quality due to fogging, etc.

[0188] From the viewpoint of making it easy to exert the effect brought about by such organic microparticles D, the lower limit of the number average primary particle size of the organic microparticles D is preferably 0.1 μm or more, more preferably 0.3 μm or more, further preferably 0.4 μm or more, and particularly preferably 0.5 μm or more, and the upper limit is more preferably 0.9 μm or less, further preferably 0.8 μm or less.

[0189] The lower limit of the content of the organic fine particles D relative to 100 parts by mass of the colored resin particles is preferably 0.05 parts by mass or more, more preferably 0.07 parts by mass or more, and further preferably 0.10 parts by mass or more, and the upper limit is preferably 1.0 parts by mass or less, more preferably 0.50 parts by mass or less, further preferably 0.30 parts by mass or less, and further preferably 0.20 parts by mass or less.

[0190] When the content of the organic fine particles D is above the above lower limit, the organic fine particles D can fully function as an external additive, so that the above-mentioned effect of the organic fine particles D can be easily obtained. On the other hand, when the content of the organic fine particles D is below the above upper limit, the deterioration of the fixing property of the toner due to an excessive amount of the external additive can be suppressed. In addition, when the content of the organic fine particles D is below the above upper limit, the organic fine particles D can be suppressed from being released from the surface of the toner particles, thereby suppressing the decrease in fluidity.

[0191] As organic fine particles D, for example, fatty acid metal salt particles such as zinc stearate and magnesium stearate, silicone polymer particles such as silicone resin particles, methacrylate polymer particles, acrylate polymer particles, styrene-methacrylate copolymer particles, styrene-acrylate copolymer particles, core-shell particles formed by a styrene polymer core and a methacrylate polymer shell, melamine resin particles, etc. As organic fine particles D, fatty acid metal salt particles are particularly preferably used.

[0192] The fatty acid site (R-COO - ) can be a monocarboxylic acid containing only one carboxyl group (-COOH), preferably a monocarboxylic acid having a chain structure, more preferably a saturated monocarboxylic acid having a chain structure, and further preferably a straight-chain saturated monocarboxylic acid.

[0193] In addition, it is preferred that the fatty acid moiety (R-COO - ) is derived from a higher fatty acid having a large number of carbon atoms in the alkyl group (R-). The number of carbon atoms in the alkyl group in the fatty acid portion is not particularly limited, but is preferably 12 to 24, more preferably 14 to 22, and even more preferably 16 to 20.

[0194] Examples of higher fatty acids preferably used as a raw material for the fatty acid metal salt particles include lauric acid (CH3(CH2) 10 COOH), tridecanoic acid (CH3(CH2) 11 COOH), myristic acid (CH3(CH2) 12 COOH), pentadecanoic acid (CH3(CH2) 13 COOH), palmitic acid (CH3(CH2) 14 COOH), heptadecanoic acid (CH3(CH2) 15 COOH), stearic acid (CH3(CH2) 16 COOH), arachidic acid (CH3(CH2) 18 COOH), behenic acid (CH3(CH2) 20 COOH), lignoceric acid (CH3(CH2) 22 COOH) etc. Stearic acid and behenic acid are particularly preferred, and stearic acid is more preferred.

[0195] These fatty acids used as the raw material of the fatty acid metal salt particles can be used alone or in combination of two or more kinds. From the viewpoint of obtaining uniform properties, they are preferably used alone.

[0196] The metal contained in the fatty acid metal salt particles may be an alkali metal, an alkaline earth metal or a metal element of Group 12 of the periodic table, and examples thereof include Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, Ba, Zn, etc. In particular, an alkaline earth metal or a metal element of Group 12 of the periodic table is preferred, and at least one selected from Mg and Zn is more preferred, and Zn is further preferred.

[0197] As the fatty acid metal salt particles, various commercially available products can be used, for example, SPZ-100F (: trade name, zinc stearate particles, number average primary particle size: 0.5 μm) and SPX-100F (: trade name, magnesium stearate particles, number average primary particle size: 0.72 μm) manufactured by Sakai Chemical Industry Co., Ltd. are mentioned.

[0198] In addition, the number average primary particle size of the external additive used in the toner of the present invention is measured, for example, as follows: about 0.1 g of a measurement sample is weighed into a beaker, 0.1 mL of an alkylbenzenesulfonic acid aqueous solution (manufactured by Fujifilm Corporation, trade name: DRIWEL) is added as a dispersant, and 10 to 30 mL of a diluent (manufactured by Beckman Coulter, Inc., trade name: ISOTON II) is further added to the beaker, and after dispersing for 3 minutes using a 20 W (watt) ultrasonic disperser, the number average primary particle size is measured using a particle size measuring machine (manufactured by Beckman Coulter, Inc., trade name: Multisizer) under the conditions of aperture: 100 μm, medium: ISOTON II, and number of particles to be measured: 100,000.

[0199] 3. Toner performance

[0200] The toner of the present invention suppresses toner leakage. After the toner of the present invention is left at high temperature and high humidity for 24 hours, a toner leakage test is repeatedly performed in the same environment in which a printer filled with toner is run for 10 seconds and then stopped for 10 seconds. The time until toner leakage is confirmed is preferably 17 hours or more, more preferably 18 hours or more, further preferably 19 hours or more, and further preferably 20 hours or more.

[0201] The toner leakage test and the method for confirming toner leakage can be performed by the same method as the toner leakage evaluation in Examples described later.

[0202] The toner of the present invention has excellent fine line reproducibility. After the toner of the present invention is placed in a low-temperature and low-humidity environment for 24 hours, in a fine line reproducibility test of continuously forming a line image with 2×2 dot lines (width 85 μm) in the same environment, the number of sheets that can maintain a line width difference of 10 μm or less from the first line image is preferably 8,000 sheets or more, more preferably 9,000 sheets or more, and even more preferably 10,000 sheets or more.

[0203] The thin line reproducibility test and the measurement of the line width of the line image can be performed by the same method as the thin line reproducibility evaluation in the examples described later.

[0204] Example

[0205] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. In addition, parts and % are based on mass unless otherwise specified.

[0206] [Example 1]

[0207] 1. Production of colored resin particles

[0208] 1-1. Preparation of core polymerizable monomer composition

[0209] 77 parts of styrene and 23 parts of n-butyl acrylate as polymerizable monomers and 7 parts of carbon black as a black colorant were dispersed using an inline emulsifier disperser (manufactured by Ohirayo Kiko Co., Ltd., trade name: Milder) to obtain a polymerizable monomer mixture.

[0210] To the above polymerizable monomer mixture, 1.6 parts of a charge control resin (a copolymer containing a quaternary ammonium salt group) as a charge control agent, 5 parts of hexaglycerol octabehenate (melting point 70°C) and 5 parts of paraffin wax (melting point 68°C) as a release agent, 0.3 parts of a polymethacrylate macromonomer (manufactured by Toagosei Chemical Industry Co., Ltd., trade name: AA-6) as a macromonomer, 0.6 parts of divinylbenzene as a cross-linking polymerizable monomer, and 1.5 parts of tert-dodecyl mercaptan as a molecular weight regulator were added, and the mixture was mixed and dissolved while heating to 45°C to prepare a core polymerizable monomer composition.

[0211] 1-2. Preparation of aqueous dispersion medium

[0212] To an aqueous solution prepared by dissolving 10.2 parts of magnesium chloride (water-soluble multivalent metal salt) in 250 parts of ion-exchanged water, an aqueous solution prepared by dissolving 6.2 parts of sodium hydroxide (alkali metal hydroxide) in 50 parts of ion-exchanged water was slowly added under stirring to prepare a magnesium hydroxide colloid (water-insoluble metal hydroxide colloid) dispersion.

[0213] 1-3. Suspension process (droplet formation process)

[0214] At room temperature, the core polymerizable monomer composition was added to the magnesium hydroxide colloidal dispersion and stirred. After 4.4 parts of diethyl peroxy tert-butyl acetate as a polymerization initiator was added thereto, a pipeline emulsifying disperser (manufactured by Pacific Machinery Co., Ltd., trade name: Milder) was used to disperse the core polymerizable monomer composition at a speed of 15,000 rpm with high-speed shear stirring for 10 minutes to form droplets of the core polymerizable monomer composition, thereby obtaining a suspension in which droplets of the core polymerizable monomer composition were dispersed.

[0215] 1-4. Polymerization process

[0216] The suspension is put into a reactor equipped with a stirring blade and stirred at 50°C for 5 minutes at 250 rpm (the front speed of the stirring blade: 0.90 m / s). After that, the temperature is raised to 90°C to initiate the polymerization reaction. When the polymerization conversion rate reaches approximately 100%, 2 parts of methyl methacrylate as a polymerizable monomer for the shell and 0.3 parts of 2,2′-azobis(2-methyl-N-(2-hydroxyethyl)-propionamide) (Wako Pure Chemical Industries, Ltd., trade name: VA-086, water-soluble) as a polymerization initiator for the shell dissolved in 10 parts of ion exchange water are added. After continuing the reaction at 90°C for 4 hours, the reaction is terminated by water cooling to obtain an aqueous dispersion of colored resin particles having a core-shell structure. In addition, the front speed of the stirring blade is maintained until the polymerization reaction of the shell is terminated.

[0217] 1-5. Post-processing process

[0218] The aqueous dispersion of the colored resin particles was stirred while sulfuric acid was added dropwise at room temperature to perform acid washing until the pH was 6.5 or less. Next, filtration was performed, 500 parts of ion exchange water was added to the obtained solid component, and the solid component was re-slurried, and the water washing treatment (washing, filtering and dehydration) was repeated several times. Next, filtration was performed, and the obtained solid component was placed in a container of a dryer and dried at 45°C for 48 hours to obtain colored resin particles.

[0219] 2. Manufacture of toner

[0220] To 100 parts of the colored resin particles obtained above were added as external additives 1.3 parts of silica fine particles having a number average primary particle size of 50 nm (manufactured by Clariant, trade name: H05TA), 0.5 parts of silica fine particles having a number average primary particle size of 20 nm (manufactured by Cabot Corporation, trade name: TG-7120), 0.2 parts of silica fine particles having a number average primary particle size of 7 nm (manufactured by Cabot Corporation, trade name: TG-820F), and 0.1 parts of zinc stearate fine particles having a number average primary particle size of 0.5 μm (manufactured by Sakai Chemical Industry Co., Ltd., trade name: SPZ-100F), and the mixture was stirred using a laboratory-scale high-speed stirring apparatus having a capacity of 10 L with a cooling jacket (manufactured by Nippon Coking Industry Co., Ltd., trade name: FM The toner of Example 1 was prepared by mixing and stirring the mixture under the conditions of a stirring blade with a peripheral speed of 32.2 m / s and an external addition treatment time of 6.0 minutes.

[0221] [Examples 2, 4, 6, 7 and Comparative Examples 1 and 2]

[0222] In Example 1, during the above-mentioned "1-4. Polymerization step", the stirring conditions before the temperature is raised to 90°C, that is, before the polymerization reaction is initiated, are changed according to Table 1, and the front end speed of the stirring blade shown in Table 1 is maintained until the polymerization reaction is terminated. Except for this, the same procedure as in Example 1 is carried out to obtain the colorants of Examples 2, 4, 6, and 7 and the colorants of Comparative Examples 1 and 2.

[0223] [Example 3]

[0224] In Example 1, in the above "1-2. Preparation of aqueous dispersion medium", the amount of magnesium chloride added was changed to 12.5 parts, and the amount of sodium hydroxide added was changed to 7.6 parts. In the above "1-4. Polymerization step", the stirring conditions before heating to 90°C, that is, before the polymerization reaction was initiated, were changed according to Table 1, and the front end speed of the stirring blade shown in Table 1 was maintained until the polymerization reaction was terminated. Furthermore, in the above "2. Production of toner", the amount of silica fine particles having a number average primary particle size of 50 nm (manufactured by Clariant, trade name: H05TA) was changed to 2.3 parts, and the amount of silica fine particles having a number average primary particle size of 20 nm (manufactured by Cabot Corporation, trade name: TG-7120) was changed to 0.8 parts. Except for this, the same procedures as in Example 1 were carried out to obtain the toner of Example 3.

[0225] [Example 5]

[0226] In Example 1, in the above "1-2. Preparation of aqueous dispersion medium", the amount of magnesium chloride added was changed to 8.2 parts, and the amount of sodium hydroxide added was changed to 5.0 parts. In the above "1-4. Polymerization step", the stirring conditions before heating to 90°C, i.e., before the polymerization reaction was initiated, were changed according to Table 1, and the front end speed of the stirring blade shown in Table 1 was maintained until the polymerization reaction was terminated. Furthermore, in the above "2. Production of toner", the amount of silica fine particles having a number average primary particle size of 50 nm (manufactured by Clariant, trade name: H05TA) was changed to 0.8 parts, and the amount of silica fine particles having a number average primary particle size of 20 nm (manufactured by Cabot Corporation, trade name: TG-7120) was changed to 0.3 parts. Except for this, the same procedures as in Example 1 were carried out to obtain the toner of Example 5.

[0227] [Comparative Example 3]

[0228] In Example 1, in the above-mentioned "1-2. Preparation of aqueous dispersion medium", the addition amount of magnesium chloride was changed to 14.0 parts, and the addition amount of sodium hydroxide was changed to 8.5 parts. In the above-mentioned "1-4. Polymerization step", the stirring conditions before heating to 90°C, that is, before the polymerization reaction was initiated, were changed according to Table 1, and the front end speed of the stirring blade shown in Table 1 was maintained until the polymerization reaction was terminated. Furthermore, in the above-mentioned "2. Production of toner", the addition amount of silica fine particles having a number average primary particle size of 50 nm (manufactured by Clariant, trade name: H05TA) was changed to 2.4 parts, and the addition amount of silica fine particles having a number average primary particle size of 20 nm (manufactured by Cabot Corporation, trade name: TG-7120) was changed to 0.9 parts. Except for this, the same procedures as in Example 1 were carried out to obtain the toner of Comparative Example 3.

[0229] [Comparative Example 4]

[0230] In Example 1, in the above-mentioned "1-2. Preparation of aqueous dispersion medium", the addition amount of magnesium chloride is changed to 6.5 parts, and the addition amount of sodium hydroxide is changed to 4.0 parts. In the above-mentioned "1-4. Polymerization step", the stirring conditions before heating to 90°C, that is, before the polymerization reaction is initiated, are changed according to Table 1, and the front end speed of the stirring blade shown in Table 1 is maintained until the polymerization reaction is terminated. Furthermore, in the above-mentioned "2. Production of toner", the addition amount of silica fine particles having a number average primary particle size of 50 nm (manufactured by Clariant, trade name: H05TA) is changed to 0.7 parts, and the addition amount of silica fine particles having a number average primary particle size of 20 nm (manufactured by Cabot Corporation, trade name: TG-7120) is changed to 0.3 parts. Except for this, the same procedures as in Example 1 are carried out to obtain the toner of Comparative Example 4.

[0231] [Example 8]

[0232] In Example 1, the above "1-1. Preparation of polymerizable monomer composition for core" is changed as follows: in the above "1-4. Polymerization step", the stirring conditions before heating to 90°C, i.e., before the polymerization reaction is initiated, are changed according to Table 1, and the front end speed of the stirring blade shown in Table 1 is maintained until the polymerization reaction is terminated. Other than this, the same procedures as in Example 1 are carried out to obtain the colorant of Example 8.

[0233] The steps for preparing the core polymerizable monomer composition in Example 8 are as follows.

[0234] First, 72 parts of styrene and 28 parts of n-butyl acrylate as polymerizable monomers, 9 parts of carbon black as a black colorant, and 1.0 part of methyl methacrylate / ethyl acrylate / acrylic acid copolymer (Tg=76°C, acid value 2.6 mgKOH / g) as a polar resin are dispersed using an inline emulsifier disperser (manufactured by Ohirayo Kiko Co., Ltd., trade name: Milder) to obtain a polymerizable monomer mixture.

[0235] To the above-mentioned polymerizable monomer mixture, 1.6 parts of a charge control resin (a copolymer containing a quaternary ammonium salt group) as a charge control agent, 20 parts of behenyl stearate (melting point 67°C) as a release agent, 0.6 parts of divinylbenzene as a cross-linking polymerizable monomer, and 1.5 parts of tert-dodecyl mercaptan as a molecular weight regulator were added, and the mixture was mixed and dissolved while heating to 45°C to prepare a core polymerizable monomer composition.

[0236] 3. Measurement of toner

[0237] 0.10 to 0.12 g of toner was added to an aqueous solution of sodium linear alkylbenzene sulfonate (concentration 0.3%), and the resulting mixed solution was dispersed and treated for 5 minutes using an ultrasonic cleaner to prepare a measurement sample. The toner particles contained in the measurement sample were measured under the following measurement conditions using a flow particle image measuring device (manufactured by Jasco International, trade name: IF-3200). The smaller the particle size of the toner particles, the greater the number of toner particles contained in the measurement sample, but the number of toner particles in each example and each comparative example was within the range of 1000 to 3000.

[0238] (Measurement conditions)

[0239] Flow cell spacer thickness: 50 μm

[0240] Telecentric zoom lens magnification: 4.5x

[0241] Total magnification: 9.0 times

[0242] Measurement volume: 0.5mL

[0243] Image resolution: 0.185μm / pixel

[0244] Detection algorithm: Ghost detection

[0245] Threshold: 15%

[0246] 3-1. Equivalent diameter of a circle

[0247] The circle area equivalent diameter of each toner particle is measured, and the arithmetic average of the circle area equivalent diameters of the measured number of particles is taken as the circle area equivalent diameter of the toner.

[0248] 3-2. Tightness

[0249] The circle area equivalent diameter and the maximum length of each toner particle are measured, and the compactness is calculated according to the following formula. The arithmetic average of the compactness of the measured number of particles is taken as the compactness of the toner.

[0250] Compactness = equivalent diameter of circle area / maximum length

[0251] 3-3. Maximum inscribed circle diameter / circle area equivalent diameter

[0252] The maximum inscribed circle diameter and the equivalent circle area diameter of each colorant particle are measured, and the value is obtained by dividing the maximum inscribed circle diameter by the equivalent circle area diameter. The arithmetic average of the maximum inscribed circle diameter / equivalent circle area diameter of the measured number of particles is taken as the maximum inscribed circle diameter / equivalent circle area diameter of the colorant.

[0253] 3-4. Roundness

[0254] The circle area equivalent diameter and the circumference equivalent circle diameter of each toner particle are measured, and the circularity is calculated by the following formula. The arithmetic average of the circularities of the measured particles is taken as the circularity of the toner.

[0255] Circularity = equivalent diameter of circle area / equivalent diameter of circle circumference

[0256] 4. Evaluation of toner

[0257] 4-1. Toner leakage

[0258] In the toner leakage test, a printer (printing speed: 40 sheets / minute) was used, which was modified from a commercially available printer of a non-magnetic single-component development method. First, after the toner box of the printer was filled with toner, it was placed in a high temperature and high humidity (H / H) environment (temperature 32.5°C, humidity 80% RH) for 24 hours. Next, under the same environment, the following toner leakage test was carried out, the toner box was set in the printer, and a cycle of running the printer for 10 seconds and then stopping for 10 seconds was repeated for a total of 20 hours. At this time, the sealing part between the axial ends of the developing roller and the housing of the developing box was observed every two hours to confirm whether there was toner leakage.

[0259] The same test was carried out three times, and the average time of toner leakage was calculated as the toner leakage time. The longer the toner leakage time is, the less likely the toner is to leak. In addition, in the test results of Table 1, ">20" means that no toner leakage was confirmed even after the toner leakage test was carried out for 20 hours.

[0260] 4-2. Thin line reproducibility

[0261] The toner cartridge of a commercially available non-magnetic single-component developing printer (printing speed: 24 sheets / minute) was filled with toner, and copy paper was set. After being placed in a low temperature and low humidity (L / L) environment (temperature 10°C, humidity 20% RH) for 24 hours, a fine line reproducibility test of continuously forming a line image with 2×2 dot lines (width 85μm) was conducted in the same environment. Every 500 sheets were measured by a printing evaluation system (manufactured by YA-MA, trade name: RT2000), and the concentration distribution data of the line image was collected. At this time, the full width at the half value of the maximum concentration was taken as the line width, the line width of the first line image was taken as the reference, and the line image whose line width difference was less than 10μm was taken as the line image that reproduced the first sheet. The number of sheets that could keep the line width difference of the line image less than 10μm was investigated, and the investigation was conducted until 10,000 sheets. In the test results of Table 1, “>10000” means that even if the thin line reproducibility test is performed up to 10000 sheets, a line image satisfying the above-mentioned standard can be maintained, and the thin line reproducibility is good.

[0262] [Table 1]

[0263]

[0264] [Investigation]

[0265] The compactness of the toner in Comparative Examples 1 and 2 is less than 0.915, so the toner leakage time is short, the toner leakage is easy to occur, and the thin line reproducibility is poor. In Comparative Examples 1 and 2, it is presumed that the stirring time of the suspension before the polymerization reaction is initiated is too long, so the compactness of the toner is reduced.

[0266] Since the circle area equivalent diameter of the toner of Comparative Example 3 is less than 5.0 μm, the toner leakage time is short and the toner leakage easily occurs.

[0267] The toner of Comparative Example 4 has a circle area equivalent diameter larger than 10.0 μm, and thus has poor thin line reproducibility.

[0268] In contrast, the toners of Examples 1 to 8 have an equivalent circle area diameter of 5.0 μm to 10.0 μm and a compactness of 0.915 to 1.000, so that the toner leakage time is long, toner leakage is suppressed, and thin line reproducibility is excellent.

Claims

1. A toner comprising colored resin particles and an external additive, wherein the colored resin particles contain a binder resin, a colorant and a release agent, The toner has an equivalent circular diameter of 5.0 μm or more and 10.0 μm or less as measured by a flow-type particle image measuring apparatus, and a compactness obtained as a ratio of the equivalent circular diameter to the maximum length (equivalent circular diameter / maximum length) of 0.915 or more and 1.000 or less.

2. The toner according to claim 1, wherein The toner has a ratio of a maximum inscribed circle diameter to a circle area equivalent diameter (maximum inscribed circle diameter / circle area equivalent diameter) of 0.900 or more and 0.950 or less.

3. The toner according to claim 1 or 2, wherein The circularity of the toner is 0.900 or more and 0.950 or less.

4. The toner according to any one of claims 1 to 3, wherein The toner contains organic fine particles and inorganic fine particles having a number average primary particle size of 6 to 100 nm as the external additives, and the content of the organic fine particles is 0.05 parts by mass or more and 1.0 parts by mass or less based on 100 parts by mass of the colored resin particles.

5. The toner according to claim 4, wherein The content of the inorganic fine particles having a number average primary particle size of 6 to 100 nm is 0.5 parts by mass or more and 6.5 parts by mass or less relative to 100 parts by mass of the colored resin particles.

6. The toner according to claim 4 or 5, wherein The inorganic fine particles having a number average primary particle size of 6 to 100 nm include two or more selected from inorganic fine particles A having a number average primary particle size of 36 to 100 nm, inorganic fine particles B having a number average primary particle size of 15 to 35 nm, and inorganic fine particles C having a number average primary particle size of 6 to 14 nm.