Negative electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

By covering the GaN layer on the surface of Si particles as the negative electrode active substance, the problem of reducing conductivity and safety of the nonaqueous electrolyte secondary battery is solved, and more efficient battery performance is achieved.

CN119072798APending Publication Date: 2024-12-03PANASONIC ENERGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380034744.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When using Si-based materials in the existing non-aqueous electrolyte secondary batteries, the battery capacity is reduced due to the reduction of conductivity caused by the skeleton forming agent, and the battery capacity is not effectively taken into account the safety of the battery and the charge and discharge cycle characteristics.

Method used

A composite material containing Si particles is used as the negative electrode active material, and the GaN layer is covered on the surface of Si particles to improve conductivity and maintain charge and discharge cycle characteristics.

Benefits of technology

The safety and charge and discharge cycle characteristics of the nonaqueous electrolyte secondary battery are improved, and the problem of reduced conductivity is avoided, and more efficient battery performance is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072798A_ABST
    Figure CN119072798A_ABST
Patent Text Reader

Abstract

Provided is a nonaqueous electrolyte secondary battery having excellent safety and charge / discharge cycle characteristics. A negative electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention contains a Si-containing composite material, wherein the Si-containing composite material contains base particles in which fine Si particles are dispersed in a base phase, and GaN covering the surfaces of the base particles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode active material for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art

[0002] In recent years, from the viewpoint of high capacity, Si-based materials are sometimes used as negative electrode active materials of non-aqueous electrolyte secondary batteries. Patent Document 1 discloses the following technology: in a negative electrode containing Si-based materials, a skeleton forming agent containing a silicate having a siloxane bond or a phosphate having an aluminum phosphate bond is used to form a skeleton in the negative electrode mixture layer, thereby suppressing short circuit during a nail penetration test.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-85276 Summary of the invention

[0006] However, if the technology described in Patent Document 1 is used, the conductivity of the negative electrode may be reduced due to the skeleton formed by the skeleton forming agent, and the battery capacity may be reduced due to repeated charge and discharge. Patent Document 1 does not study the balance between battery safety and charge and discharge cycle characteristics, and there is still room for improvement.

[0007] An object of the present invention is to provide a nonaqueous electrolyte secondary battery having excellent safety and charge-discharge cycle characteristics.

[0008] A negative electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present invention is characterized by comprising a Si-containing composite material including mother particles in which Si fine particles are dispersed in a mother phase, and GaN coating the surface of the mother particles.

[0009] A nonaqueous electrolyte secondary battery as one embodiment of the present invention is characterized by comprising a negative electrode including the negative electrode active material for a nonaqueous electrolyte secondary battery, a positive electrode, and a nonaqueous electrolyte.

[0010] According to the negative electrode active material for a non-aqueous electrolyte secondary battery of the present invention, the safety and charge-discharge cycle characteristics of the non-aqueous electrolyte secondary battery can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is an axial cross-sectional view of a cylindrical secondary battery as an example of an embodiment.

[0012] Figure 2 This is a cross-sectional view of a Si-containing composite material in one example of an embodiment. DETAILED DESCRIPTION

[0013] Below, while referring to the attached Figure 1 An example of an embodiment of the cylindrical secondary battery of the present invention is described in detail. In the following description, specific shapes, materials, values, directions, etc. are for easy understanding of the examples of the present invention, and may be appropriately changed according to the specifications of the secondary battery. In addition, the following example illustrates a cylindrical secondary battery in which a wound electrode body is housed in a cylindrical outer body, but the electrode body is not limited to a wound type, and may also be a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one through a separator. The outer body is not limited to a cylindrical shape, for example, it may also be a square, a coin shape, etc. In addition, the outer body may also be a bag-type composed of a laminated sheet comprising a metal layer and a resin layer. In addition, in this specification, the description of "value (A) to value (B)" means above value (A) and below value (B).

[0014] Figure 1 FIG. 1 is a cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1 As shown, the secondary battery 10 includes a wound electrode body 14, a nonaqueous electrolyte, and an outer can 16 for storing the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a winding structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The outer can 16 is a metal container in the shape of a bottomed cylindrical body with one side open in the axial direction, and the opening of the outer can 16 is blocked by a sealing body 17. In the following, for convenience of description, the sealing body 17 side of the battery is set as the upper side, and the bottom side of the outer can 16 is set as the lower side.

[0015] The positive electrode 11, the negative electrode 12 and the separator 13 constituting the electrode body 14 are all strip-shaped long bodies, which are alternately stacked in the radial direction of the electrode body 14 by being wound into a spiral shape. The separator 13 separates the positive electrode 11 and the negative electrode 12 from each other. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one size larger than the positive electrode 11. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the long dimension direction and the width direction (short dimension direction). The two separators 13 are formed to be at least one size larger than the positive electrode 11, and are arranged, for example, in a manner of sandwiching the positive electrode 11. The electrode body 14 includes a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.

[0016] Insulating plates 18 and 19 are disposed above and below the electrode body 14, respectively. Figure 1In the example shown, the positive electrode lead 20 extends toward the sealing body 17 through the through hole of the insulating plate 18, and the negative electrode lead 21 extends toward the bottom side of the outer can 16 through the outer side of the insulating plate 19. The positive electrode lead 20 is connected to the lower surface of the internal terminal plate 23 of the sealing body 17 by welding or the like, and the top plate of the sealing body 17, that is, the lid 27 electrically connected to the internal terminal plate 23, serves as the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 serves as the negative terminal.

[0017] A gasket 28 is provided between the outer can 16 and the sealing body 17 to ensure the airtightness inside the battery. A groove 22 is formed in the outer can 16, in which a part of the side surface extends inward and supports the sealing body 17. The groove 22 is preferably formed in an annular shape along the circumference of the outer can 16, and supports the sealing body 17 on its upper surface. The sealing body 17 is fixed to the upper part of the outer can 16 through the groove 22 and the open end of the outer can 16 riveted to the sealing body 17.

[0018] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions. If the internal pressure of the battery rises due to abnormal heat, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cover 27 side, thereby cutting off the current path between the lower valve body 24 and the upper valve body 26. If the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.

[0019] Hereinafter, the positive electrode 11 , the negative electrode 12 , the separator 13 , and the nonaqueous electrolyte constituting the secondary battery 10 , particularly the negative electrode 12 , will be described in detail.

[0020] [negative electrode]

[0021] The negative electrode 12, for example, has a negative electrode current collector and a negative electrode mixture layer formed on the surface of the negative electrode current collector. The negative electrode mixture layer is preferably formed on both sides of the negative electrode current collector. The negative electrode current collector can use a foil of a metal such as copper that is stable within the potential range of the negative electrode, a film obtained by configuring the metal on the surface layer, etc. The negative electrode mixture layer, for example, contains a negative electrode active material, a binder, etc. The negative electrode 12 can be made, for example, in the following manner: a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. is applied to both sides of the negative electrode current collector, dried to form a negative electrode mixture layer, and then the negative electrode mixture layer is rolled.

[0022] As the binder contained in the negative electrode mixture layer, for example, fluorine resin, polyimide resin, acrylic resin, polyolefin resin, polyacrylonitrile (PAN), styrene-butadiene rubber (SBR), nitrile rubber (NBR), carboxymethyl cellulose (CMC) or its salt, polyacrylic acid (PAA) or its salt (PAA-Na, PAA-K, etc., and partially neutralized salt), polyvinyl alcohol (PVA), etc. can be cited. These can be used alone or in combination of two or more.

[0023] The negative electrode active material contained in the negative electrode mixture layer includes a composite material 30 containing Si. Figure 2 FIG. 4 is a cross-sectional view of a Si-containing composite material 30 in one example of an embodiment. Figure 2 As shown, the Si-containing composite material 30 includes a mother particle 35 in which Si particles 32 are dispersed in a mother phase 34 and GaN 36 coated on the surface of the mother particle 35. As a result, the safety and charge-discharge cycle characteristics of the secondary battery can be improved. It is speculated that by coating the surface with GaN 36, the thermal conductivity of the Si-containing composite material 30 is improved, and the safety of the secondary battery is improved. In addition, generally, if a compound such as a semiconductor is coated on the surface of the mother particle 35, the charge-discharge cycle characteristics are reduced, but according to the research of the inventors, it is clear that when GaN 36 is coated, the charge-discharge cycle characteristics will not be specifically reduced.

[0024] The mother particle 35 has, for example, a sea-island structure in which Si particles 32 are substantially uniformly dispersed in a mother phase 34. The mother phase 34 is composed of, for example, a collection of particles finer than the Si particles 32. The content of the Si particles 32 is, for example, 30% to 70% by mass relative to the total mass of the mother particle 35.

[0025] The parent phase 34 is, for example, a silicate phase. The parent phase 34 may be a lithium silicate phase. The lithium silicate phase is, for example, a phase having the general formula Li 2z SiO (2+z) The matrix phase 34 may be a silicon oxide (SiO2) phase. In addition, the matrix phase 34 may be an amorphous carbon phase.

[0026] The mother particle 35 may have a carbon film 38 on the surface. As a result, the conductivity of the Si-containing composite material 30 is improved. Figure 2 As shown, the carbon film 38 may exist in a dotted form so as to cover at least a portion of the surface of the particle including the Si fine particles 32 and the matrix 34, or may exist so as to cover the entire surface of the particle including the Si fine particles 32 and the matrix 34. In order to take into account both the conductivity and the diffusion of Li ions into the particle, the thickness of the carbon film 38 is preferably 1 nm to 200 nm.

[0027] When the mother particle 35 has a carbon film 38 on the surface, GaN 36 preferably covers at least a portion of the surface of the carbon film 38. In this case, GaN 36 may cover the surface of the mother particle 35 where the carbon film 38 does not exist. Figure 2 As shown, the GaN 36 may exist in a dotted form so as to cover at least a part of the surface of the mother particle 35 , or may exist so as to cover the entire surface of the mother particle 35 .

[0028] For the Si-containing composite material 30, the mass of GaN 36 is preferably 10 to 20 parts by mass, based on 100 parts by mass of the mother particle 35. When the amount of GaN 36 is within this range, the above-mentioned effect of GaN becomes more significant.

[0029] The negative electrode active material contained in the negative electrode mixture layer may include graphite in addition to the Si-containing composite material 30. Examples of graphite include natural graphite such as flaky graphite, blocky artificial graphite, and artificial graphite such as graphitized mesophase carbon microbeads. In addition, the negative electrode active material may also include metals such as Si and Sn alloyed with lithium, or alloys thereof.

[0030] The ratio of the Si-containing composite material 30 in the negative electrode active material is preferably 1 mass % to 15 mass % relative to the total mass of the negative electrode active material. When the ratio of the Si-containing composite material 30 is within this range, the above-mentioned effect of GaN becomes more significant.

[0031] The method for forming the GaN 36 film on the surface of the mother particle 35 is not particularly limited, and for example, evaporation, sputtering, etc. can be used. GaN 36 is preferably formed by sputtering. GaN 36 is formed, for example, by sputtering while flowing the mother particle 35. As a method for flowing the mother particle 35, for example, rotating or vibrating the container containing the mother particle 35 can be cited.

[0032] [positive electrode]

[0033] The positive electrode 11, for example, has a positive electrode collector and a positive electrode mixture layer formed on the surface of the positive electrode collector. The positive electrode mixture layer is preferably formed on both sides of the positive electrode collector. The positive electrode collector can use a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, a film obtained by configuring the metal on the surface, etc. The positive electrode mixture layer, for example, contains a positive electrode active material, a binder, a conductive agent, etc. The positive electrode 11 can be made, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive agent, etc. on both sides of the positive electrode collector, drying to form a positive electrode mixture layer, and then rolling the positive electrode mixture layer.

[0034] Examples of the positive electrode active material include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. For example, lithium transition metal oxides are Li x CoO2、Li x NiO2、Li x MnO2、Li x Co y Ni 1-y O2、Li x Co y M 1-y O z , Li x Ni 1- y M y O z , Li x Mn2O4、Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3). These can be used alone or in combination. In order to achieve a high capacity of the non-aqueous electrolyte secondary battery, the positive electrode active material preferably contains Li x NiO2、Li x Co y Ni 1-y O2、Li x Ni 1-y M y O z Lithium nickel composite oxides such as (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3).

[0035] Examples of the conductive agent include carbon black (CB), acetylene black (AB), Ketjen black, carbon nanotubes (CNT), graphene, graphite and other carbon particles, etc. These may be used alone or in combination of two or more.

[0036] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF), polyimide-based resins, acrylic resins, polyolefin-based resins, and polyacrylonitrile (PAN), etc. These may be used alone or in combination of two or more.

[0037] [Spacer]

[0038] The spacer 13 may be made of, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, and the like. Suitable materials for the spacer include olefin resins such as polyethylene and polypropylene, and cellulose. The spacer 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it may be a multilayer spacer including a polyethylene layer and a polypropylene layer, or a spacer obtained by coating the surface of the spacer 13 with materials such as aramid resins and ceramics.

[0039] [Non-aqueous electrolyte]

[0040] The non-aqueous electrolyte is a liquid electrolyte (electrolyte) containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more thereof. The non-aqueous solvent may also contain a halogen substituted body formed by replacing at least a portion of the hydrogen of these solvents with a halogen atom such as fluorine.

[0041] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone and γ-valerolactone; and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate.

[0042] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethylethylene. Chain ethers such as 1,2-dimethoxyethane, 1,2-dibutyloxyethane, 1,1-dimethoxymethane, 1,1-diethoxyethane, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, etc.

[0043] As the halogen-substituted product, preferably used are fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylates such as fluoromethyl propionate (FMP), and the like.

[0044] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1<x<6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lower aliphatic carboxylic acid lithium, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2) {l, m is an integer greater than 1} and other imide salts. The lithium salt may be used alone or in combination. Among these, LiPF6 is preferably used from the viewpoint of ion conductivity, electrochemical stability, etc. The concentration of the lithium salt is preferably set to 0.8 to 1.8 mol per 1 L of solvent.

[0045] Example

[0046] Hereinafter, the present invention will be further described by way of examples, but the present invention is not limited to these examples.

[0047] <Example 1>

[0048] [Production of positive electrode]

[0049] As the positive electrode active material, powdered LiNi 0.88 Co 0.09 Al 0.03 Lithium transition metal oxide represented by O2. 95 parts by mass of positive electrode active material, 2.5 parts by mass of acetylene black (AB) and 2.5 parts by mass of polyvinylidene fluoride (PVDF) are mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) is further added to prepare a positive electrode mixture slurry. The positive electrode mixture slurry is applied to both sides of a positive electrode collector formed of aluminum foil, and after the coating is dried, the coating is rolled using a calendering roller to produce a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode collector.

[0050] [Production of Si-containing composite materials]

[0051] SiO2 and Li2CO3 were mixed so that the atomic ratio of Si:Li was 1.05:1, and the mixture was calcined at 950°C for 10 hours in an air atmosphere to obtain lithium silicate represented by Li2O·2.1SiO2. Next, the obtained lithium silicate was pulverized to an average particle size of 10 μm.

[0052] The lithium silicate (Li2O·2.1SiO2) was mixed with raw material Si (3N, average particle size 10 μm) at a mass ratio of 50:50. Next, the mixture was filled into a SUS tank (volume 500 mL) of a planetary ball mill (FRITSCH, P-5). In addition, 24 SUS balls with a diameter of 20 mm were placed in the tank, and a composite treatment was performed at 200 rpm for 50 hours in an inert atmosphere. Furthermore, the composited mixture was sintered at 600°C for 4 hours in an inert atmosphere, thereby obtaining a sintered body of particles with Si microparticles dispersed in the lithium silicate phase.

[0053] The sintered body was crushed and passed through a 400 μm sieve, coal tar (MCP250 manufactured by JFE Chemical) was added, and then calcined at 800°C for 5 hours in an inert atmosphere to prepare mother particles having a carbon coating on the surface. The amount of the carbon coating was set to 5% by mass relative to the total mass of the mother particles. Then, the mother particles were crushed and classified using an air flow classification device. The average particle size of the classified mother particles was 10 μm.

[0054] Next, the surface of the mother particle is coated with GaN by sputtering to prepare a composite material containing Si. Specifically, 100g of mother particles are arranged in a vacuum chamber of a sputtering device, and a GaN target with a diameter of 5 inches is used to perform sputtering film formation in an RF manner. The amount of GaN film formed is set to 20% by mass relative to the mass of the mother particles. As for sputtering film formation, after evacuating the vacuum chamber until the pressure becomes 1.8Pa, it is carried out in an Ar gas flow environment in a manner such that the pressure of the vacuum chamber becomes about 1Pa. The film forming temperature is 1000°C. In addition, as for sputtering film formation, the container containing the mother particles is rotated so that the mother particles flow. The mother particles after sputtering film formation are crushed and classified by an airflow classification device, thereby preparing a composite material containing Si with an average particle size of 10μm.

[0055] [Production of negative electrode]

[0056] The above-mentioned Si-containing composite material is mixed with graphite with an average particle size of 22 μm in a mass ratio of 4.8:95.2 to prepare a negative electrode active material. 100 parts by mass of the negative electrode active material, 1 part by mass of carboxymethyl cellulose (CMC) and 1 part by mass of styrene-butadiene copolymer rubber (SBR) are mixed, and the mixture is kneaded in water to prepare a negative electrode mixture slurry. The negative electrode mixture slurry is applied to both sides of a negative electrode collector formed of copper foil, and after the coating is dried, the coating is rolled using a calendering roller to produce a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector.

[0057] [Preparation of non-aqueous electrolyte]

[0058] A non-aqueous electrolyte was prepared by dissolving LiPF6 at a concentration of 1.0 mol / L in a non-aqueous solvent prepared by mixing ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 3:7.

[0059] [Manufacturing of Secondary Batteries]

[0060] An aluminum positive electrode lead is installed on the positive electrode collector, a nickel negative electrode lead is installed on the negative electrode collector, and the positive electrode and the negative electrode are wound into a spiral shape through a polyolefin separator to produce a wound electrode body. The electrode body is housed in a bottomed cylindrical battery case body with an outer diameter of 18.2 mm and a height of 65 mm, and after the above-mentioned non-aqueous electrolyte is injected, the opening of the battery case body is sealed with a gasket and a sealing body to produce a 18650 type cylindrical secondary battery.

[0061] <Example 2>

[0062] In the preparation of the Si-containing composite material, a secondary battery was prepared in the same manner as in Example 1 except that the amount of GaN formed was changed to 10% by mass relative to the mass of the mother particles.

[0063] <Example 3>

[0064] In the production of the negative electrode, a secondary battery was produced in the same manner as in Example 1 except that the mixing ratio of the Si-containing composite material and graphite constituting the negative electrode active material was changed to a mass ratio of 15:85.

[0065] <Example 4>

[0066] In the preparation of the Si-containing composite material, the film formation amount of GaN is changed to 10 mass % relative to the mass of the mother particles, and in the preparation of the negative electrode, the mixing ratio of the Si-containing composite material and graphite constituting the negative electrode active material is changed to a mass ratio of 15:85. Except for the above, the secondary battery is prepared in the same manner as in Example 1.

[0067] <Example 5>

[0068] In the production of the negative electrode, a secondary battery was produced in the same manner as in Example 1 except that the mixing ratio of the Si-containing composite material and graphite constituting the negative electrode active material was changed to a mass ratio of 2.8:97.2.

[0069] <Comparative Example 1>

[0070] A secondary battery was produced in the same manner as in Example 1 except that GaN film formation was not performed in the production of the Si-containing composite material.

[0071] <Comparative Example 2>

[0072] In the preparation of the Si-containing composite material, GaN film formation is not carried out, and in the preparation of the negative electrode, the mixing ratio of the Si-containing composite material and graphite constituting the negative electrode active material is changed to a mass ratio of 4.0:95.2, and GaN powder is added to the negative electrode active material in such a manner that the mass ratio of the negative electrode active material to the GaN powder becomes 99.2:0.8. Except for the above, the same operations as in Example 1 are carried out to prepare a secondary battery.

[0073] <Comparative Example 3>

[0074] In the production of the Si-containing composite material, a secondary battery was produced in the same manner as in Example 1, except that the target for sputtering film formation was changed to form a film of Ga2O3 instead of GaN.

[0075] <Comparative Example 4>

[0076] In the production of the Si-containing composite material, a secondary battery was produced in the same manner as in Example 1, except that the target for sputtering film formation was changed to form a film of AlN instead of GaN.

[0077] <Comparative Example 5>

[0078] In the production of the Si-containing composite material, a secondary battery was produced in the same manner as in Example 1, except that the target for sputtering film formation was changed to form a SiC film instead of GaN.

[0079] <Comparative Example 6>

[0080] In the production of the Si-containing composite material, a secondary battery was produced in the same manner as in Example 1, except that the target for sputtering film formation was changed to form a Si 3 N 4 film instead of GaN.

[0081] [Nail penetration test]

[0082] For each battery of the example and the comparative example, a nail penetration test was performed according to the following procedure.

[0083] (1) In an environment of 25°C, constant current charging was performed at 0.5C until the battery voltage reached 4.2V, and then constant voltage charging was performed at 4.2V until the current value reached 1 / 50C.

[0084] (2) Under a 25°C environment, a 2 mm diameter iron nail is inserted into the center of the side surface of the secondary battery after charge in (1) at a speed of 5 mm / sec, and the side surface temperature of the battery is measured to determine the maximum temperature at that time.

[0085] (3) When the secondary battery did not rupture or catch fire and the maximum temperature was 100° C. or less, the evaluation was “0”. When the secondary battery did not rupture or catch fire but the maximum temperature exceeded 100° C., the evaluation was “△”. When the secondary battery ruptured or caught fire, the evaluation was “×”.

[0086] [Cycle test]

[0087] At an ambient temperature of 25°C, the secondary batteries of each embodiment and each comparative example were charged at a constant current of 0.5C until the battery voltage was 4.2V, and then charged at a constant voltage of 4.2V until the current value was 1 / 50C. Then, they were discharged at a constant current of 0.5C to 2.85V. This charge and discharge was regarded as one cycle, and a cycle test of 200 cycles was performed. The capacity retention rate of the secondary batteries of each embodiment and each comparative example in the charge and discharge cycle was calculated by the following formula.

[0088] Capacity retention rate = (discharge capacity at the 200th cycle / discharge capacity at the 1st cycle) × 100

[0089] The evaluation results of the nail penetration test and the cycle test of each secondary battery of the Example and the Comparative Example are summarized in Table 1. Table 1 also shows the type and addition amount of the coating material in the Si-containing composite material and the ratio of the Si-containing composite material in the negative electrode active material.

[0090] [Table 1]

[0091]

[0092] The secondary battery of the embodiment has a good result of the nail penetration test and a capacity retention rate that is equal to or higher than that of the secondary battery of Comparative Example 1. On the other hand, the capacity retention rate of Comparative Example 2, in which GaN is not coated on the Si-containing composite material but GaN is contained in the negative electrode mixture layer, is lower than that of the secondary battery of Comparative Example 1. In addition, in the secondary batteries of Comparative Examples 3 to 6 using Si-containing composite materials coated with materials other than GaN, no result that can take into account both the nail penetration test and the capacity retention rate is obtained. According to these results, by coating the surface of the mother particle with GaN, the safety of the secondary battery can be improved without reducing the charge and discharge cycle characteristics.

[0093] The present invention will be further described by the following embodiments.

[0094] Composition 1:

[0095] A negative electrode active material for a non-aqueous electrolyte secondary battery, comprising a composite material containing Si,

[0096] The Si-containing composite material includes mother particles in which Si fine particles are dispersed in a matrix phase, and GaN coating the surface of the mother particles.

[0097] Composition 2:

[0098] The negative electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 1, wherein the base particle has a carbon coating on the surface.

[0099] Composition 3:

[0100] The negative electrode active material for a non-aqueous electrolyte secondary battery according to Configuration 2, wherein the GaN covers at least a portion of the surface of the carbon film.

[0101] Composition 4:

[0102] The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the parent phase is a silicate phase.

[0103] Composition 5:

[0104] The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the parent phase is a silicate phase.

[0105] Composition 6:

[0106] The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 3, wherein the parent phase is an amorphous carbon phase.

[0107] Composition 7:

[0108] The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of configurations 1 to 6, wherein in the Si-containing composite material, the mass of the GaN is 10 to 20 parts by mass, based on 100 parts by mass of the mother particle.

[0109] Composition 8:

[0110] The negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of configurations 1 to 7, wherein the ratio of the Si-containing composite material in the negative electrode active material for a non-aqueous electrolyte secondary battery is 1 mass % to 15 mass % relative to the total mass of the negative electrode active material for a non-aqueous electrolyte secondary battery.

[0111] Composition 9:

[0112] A non-aqueous electrolyte secondary battery comprises a negative electrode including the negative electrode active material for a non-aqueous electrolyte secondary battery according to any one of Configurations 1 to 8, a positive electrode, and a non-aqueous electrolyte.

[0113] Description of Reference Numerals

[0114] 10: non-aqueous electrolyte secondary battery, 11: positive electrode, 12: negative electrode, 13: separator, 14: electrode body, 16: outer can, 17: sealing body, 18, 19: insulating plate, 20: positive electrode lead, 21: negative electrode lead, 22: slotted portion, 23: internal terminal plate, 24: lower valve body, 25: insulating member, 26: upper valve body, 27: cover, 28: gasket, 30: composite material containing Si, 32: Si fine particles, 34: parent phase, 35: parent particle, 36: GaN, 38: carbon film

Claims

1. A negative electrode active material for a non-aqueous electrolyte secondary battery, comprising a composite material containing Si, The Si-containing composite material includes mother particles in which Si fine particles are dispersed in a matrix phase, and GaN coating the surface of the mother particles.

2. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The mother particles have a carbon coating on the surface.

3. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 2, wherein The GaN covers at least a portion of the surface of the carbon film.

4. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The parent phase is a silicate phase.

5. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The parent phase is a lithium silicate phase.

6. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The parent phase is an amorphous carbon phase.

7. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein In the Si-containing composite material, when the mass of the mother particles is 100 parts by mass, the mass of the GaN is 10 parts by mass to 20 parts by mass.

8. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein The ratio of the Si-containing composite material in the negative electrode active material for a non-aqueous electrolyte secondary battery is 1 mass % to 15 mass % with respect to the total mass of the negative electrode active material for a non-aqueous electrolyte secondary battery. 9 . A non-aqueous electrolyte secondary battery comprising a negative electrode comprising the negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 , a positive electrode, and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Skeleton forming agent and negative electrode using the same

    JP2018085276A