Glass cloth, prepreg, and printed wiring board

By adjusting the glass filament diameter, number of roots and braiding density of the glass cloth, the fiber opening efficiency between the yarns is optimized, and the delay time difference and signal quality problems in the printed wiring board are solved, thereby achieving efficient signal transmission and high productivity.

CN119073006AActive Publication Date: 2024-12-03NITTO BOSEKI CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380035776.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-08
Filing Date
2023-06-01
Publication Date
2024-12-03
Estimated Expiration
2043-06-01

AI Technical Summary

Technical Problem

The existing glass cloth has problems with delay time difference and signal quality deterioration in printed wiring boards, and has low productivity, mainly due to instability in signal transmission caused by excessive gaps between yarns and braiding density.

Method used

The structure is made of a specific glass cloth. By adjusting the diameter, number of roots and braiding density of the glass filaments, the fiber opening efficiency coefficient of the warp and weft yarns is within a specific range, reducing the gaps and overlap between the yarns, and improving signal transmission efficiency.

Benefits of technology

The delay time difference of the printed wiring board is effectively reduced, the deterioration of signal quality is suppressed, and the productivity of the glass cloth is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a glass cloth, a prepreg and a printed wiring board. The glass cloth can reduce the delay time difference of a printed wiring board and realize high productivity. In the glass cloth, the diameters of the glass filaments of the warp yarns and the weft yarns are respectively 0.5-4.5 [mu] m, the number of the glass filaments is respectively 150-3000, the weaving densities are respectively 1.0-50.0 pieces / 25 mm or less, the average yarn width is respectively 550-10000 [mu] m, the splitting efficiency coefficients are respectively 0.600-1.500, the ratio of the number of the filaments to the diameters of the filaments is respectively 68.6-555.5, the geometric average of the splitting efficiency coefficients of the warp yarns and the weft yarns is 0.770-1.200, and the diameter of the warp yarns and the diameter of the weft yarns are respectively 0.5-4.5 [mu] m. And the thickness of the glass cloth is less than 10.0 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to glass cloth, prepreg and printed wiring board. Background Art

[0002] Conventionally, as an insulating material in a printed wiring board, a prepreg made of glass cloth impregnated with a resin such as epoxy resin or modified polyphenylene ether is used. The glass cloth is composed of warp yarns and weft yarns, and the warp yarns and weft yarns are formed by bundling a plurality of glass filaments.

[0003] In order to realize the miniaturization and thinning of electronic equipment, the printed wiring board and the prepreg are also required to be thin. Therefore, a glass cloth with reduced thickness is required. As a glass cloth with reduced thickness, the following glass cloth is proposed (for example, refer to patent document 1): the glass cloth uses warp yarns and weft yarns formed by a small amount of glass filaments with small fiber diameters, improves the warp yarn weaving density and the weft yarn weaving density, and performs a strong fiber opening treatment to increase the warp yarn width and the weft yarn width.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 6536764 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In recent years, it is known that with the increase in the speed and frequency of data communication, the signal degradation caused by distortion called skew, which leads to the degradation of signal quality, has become significant in the above-mentioned printed wiring board, and therefore it is required to suppress the degradation of signal quality during signal transmission (delay time difference reduction). In addition, with the increase in demand for thinner printed wiring boards, it is required to increase the supply speed of glass cloth.

[0009] However, the conventional glass cloth described in Patent Document 1 has the following problems: due to the small number of filaments, strong fiber opening treatment, etc., there are gaps between warp yarns or weft yarns, especially gaps between glass filaments constituting weft yarns, deviations in yarn width of warp yarns or weft yarns, and portions where glass cloth does not exist in the printed wiring board. In addition, if portions where glass cloth does not exist are generated in the above-mentioned printed wiring board, there is a problem that the delay time difference cannot be reduced sufficiently. In addition, in the above-mentioned conventional glass cloth, there is a problem that sufficient productivity cannot be achieved due to the high weaving density.

[0010] Therefore, an object of the present invention is to provide a glass cloth which can solve the above-mentioned problems, reduce the delay time difference of a printed wiring board, suppress the degradation of signal quality, and achieve high productivity.

[0011] Means for solving problems

[0012] In order to achieve the above-mentioned object, the technical content of the glass cloth of the present invention is as follows. The glass cloth is composed of warp yarns and weft yarns respectively formed by bundling a plurality of glass filaments. The glass cloth is characterized in that the filament diameter Dt of the glass filaments constituting the warp yarns and the filament diameter Dy of the glass filaments constituting the weft yarns are respectively independently in the range of 0.5 μm or more and 4.5 μm or less, the number of filaments Ft of the glass filaments constituting the warp yarns and the number of filaments Fy of the glass filaments constituting the weft yarns are respectively independently in the range of 150 or more and 3000 or less, the weaving density Wt of the warp yarns and the weaving density Wy of the weft yarns are respectively independently in the range of 1.0 filament / 25 mm or more and 50.0 filament / 25 mm or less, the average yarn width Bt of the warp yarns and the average yarn width By of the weft yarns are respectively independently in the range of 550 μm or more and 1000 μm or less. 00 μm or less, a warp yarn opening efficiency coefficient Pt obtained by the following formula (1) from the Dt, the Ft, the Wt and the Bt is in the range of 0.600 or more and 1.500 or less, a weft yarn opening efficiency coefficient Py obtained by the following formula (2) from the Dy, the Fy, the Wy and the By is in the range of 0.600 or more and 1.500 or less, a ratio Ft / Dt, i.e., Rt, of the number of glass filaments Ft constituting the warp yarn to the filament diameter Dt of the glass filaments constituting the warp yarn and a ratio Fy / Dy, i.e., Ry, of the number of glass filaments Fy constituting the weft yarn to the filament diameter Dy of the glass filaments constituting the weft yarn are independently in the range of 68.6 or more and 555.5 or less, the Pt and Py satisfy the following formula (3), and the thickness of the glass cloth is less than 10.0 μm,

[0013] Pt={(Bt / (Dt×Ft))×Bt / (25000 / Wt)} 1 / 2 ×{(Dt×Ft) / (25000 / Wt)}…(1),

[0014] Py={(By / (Dy×Fy))×By / (25000 / Wy)} 1 / 2 ×{(Dy×Fy) / (25000 / Wy)}…(2),

[0015] 0.770≤(Pt×Py) 1 / 2 ≤1.200…(3).

[0016] According to the glass cloth of the present invention, by having the above-mentioned configuration, the glass cloth can reduce the delay time difference of the printed wiring board, suppress the degradation of the signal quality, and realize high productivity.

[0017] In the glass cloth of the present invention, it is preferred that the filament diameter Dt of the glass filaments constituting the warp yarns and the filament diameter Dy of the glass filaments constituting the weft yarns are independently in the range of 2.0 μm or more and 3.8 μm or less, and the above Pt and Py satisfy the following formula (4):

[0018] 0.890≤(Pt×Py) 1 / 2 ≤0.970…(4).

[0019] The present invention also relates to a prepreg containing the glass cloth of the present invention and a printed wiring board containing the glass cloth of the present invention. DETAILED DESCRIPTION

[0020] Next, embodiments of the present invention will be described in further detail.

[0021] The glass cloth of the present embodiment is composed of warp yarns and weft yarns respectively formed by bundling a plurality of glass filaments, and the glass cloth is characterized in that the filament diameter Dt of the glass filaments constituting the warp yarns and the filament diameter Dy of the glass filaments constituting the weft yarns are respectively independently in the range of 0.5 μm or more and 4.5 μm or less, the number of filaments Ft of the glass filaments constituting the warp yarns and the number of filaments Fy of the glass filaments constituting the weft yarns are respectively independently in the range of 150 or more and 3000 or less, the weaving density Wt of the warp yarns and the weaving density Wy of the weft yarns are respectively independently in the range of 1.0 filament / 25 mm or more and 50.0 filaments / 25 mm or less, and the average yarn width Bt of the warp yarns and the average yarn width By of the weft yarns are respectively independently in the range of 550 μm or more and 10000 μm or less. the warp yarn opening efficiency coefficient Pt obtained by the following formula (1) from the Dt, Ft, Wt and Bt is in the range of 0.600 or more and 1.500 or less, the weft yarn opening efficiency coefficient Py obtained by the following formula (2) from the Dy, Fy, Wy and By is in the range of 0.600 or more and 1.500 or less, the ratio of the number of glass filaments Ft constituting the warp yarn to the filament diameter Dt of the glass filaments constituting the warp yarn (Ft / Dt), i.e., Rt, and the ratio of the number of glass filaments Fy constituting the weft yarn to the filament diameter Dy of the glass filaments constituting the weft yarn (Fy / Dy), i.e., Ry, are independently in the range of 68.6 or more and 555.5 or less, the Pt and the Py satisfy the following formula (3), the thickness of the glass cloth is less than 10.0 μm,

[0022] Pt={(Bt / (Dt×Ft))×Bt / (25000 / Wt)} 1 / 2 ×{(Dt×Ft) / (25000 / Wt)}…(1),

[0023] Py={(By / (Dy×Fy))×By / (25000 / Wy)} 1 / 2 ×{(Dy×Fy) / (25000 / Wy)}…(2),

[0024] 0.770≤(Pt×Py) 1 / 2 ≤1.200…(3).

[0025] In the glass cloth of the present embodiment, when the filament diameter Dt of the glass filaments constituting the warp yarn or the filament diameter Dy of the glass filaments constituting the weft yarn is less than 0.5 μm, it is difficult to continuously and stably produce. On the other hand, when the filament diameter Dt of the glass filaments constituting the warp yarn or the filament diameter Dy of the glass filaments constituting the weft yarn is independently greater than 4.5 μm, it is impossible to achieve sufficient thinning of the glass cloth.

[0026] The filament diameter Dt of the glass filaments constituting the warp yarn or the filament diameter Dy of the glass filaments constituting the weft yarn is preferably independently in the range of 2.0 to 3.8 μm, more preferably in the range of 2.5 to 3.7 μm, and further preferably in the range of 2.6 to 3.6 μm.

[0027] In addition, the ratio Dt / Dy of the filament diameter Dt of the glass filaments constituting the above-mentioned warp yarn to the filament diameter Dy of the glass filaments constituting the above-mentioned weft yarn is, for example, in the range of greater than 0.90 and less than 1.10, preferably in the range of greater than 0.95 and less than 1.05, more preferably in the range of greater than 0.97 and less than 1.03, further preferably in the range of greater than 0.98 and less than 1.02, particularly preferably in the range of greater than 0.99 and less than 1.01, and most preferably in the range of 1.00.

[0028] In addition, in the glass cloth of the present embodiment, if the number of filaments Ft of the glass filaments constituting the warp yarn and the number of filaments Fy of the glass filaments constituting the weft yarn are each independently less than 150, it is sometimes impossible to fully suppress the generation of gaps between the filaments. On the other hand, when the number of filaments Ft of the glass filaments constituting the warp yarn and the number of filaments Fy of the glass filaments constituting the weft yarn are each independently more than 3000, it is impossible to achieve a sufficient thinning of the glass cloth.

[0029] Preferably, the number Ft of glass filaments constituting the warp yarn and the number Fy of glass filaments constituting the weft yarn are each independently within a range of 415 or more and 990 or less.

[0030] In addition, the ratio Ft / Fy of the number of glass filaments Ft constituting the above-mentioned warp yarn to the number of glass filaments Fy constituting the above-mentioned weft yarn is, for example, in the range of greater than 0.90 and less than 1.10, and is preferably in the range of greater than 0.95 and less than 1.05, more preferably in the range of greater than 0.97 and less than 1.03, further preferably in the range of greater than 0.98 and less than 1.02, particularly preferably in the range of greater than 0.99 and less than 1.01, and most preferably in the range of 1.00.

[0031] In addition, in the glass cloth of the present embodiment, if the weaving density Wt of the warp yarn and the weaving density Wy of the weft yarn are each independently less than 1.0 yarn / 25 mm, it is sometimes impossible to fully suppress the generation of gaps between the warp yarns or between the weft yarns. On the other hand, if the weaving density Wt of the warp yarn and the weaving density Wy of the weft yarn are each independently greater than 50.0 yarn / 25 mm, it is impossible to fully improve the productivity of the glass cloth.

[0032] The weaving density Wt of the warp yarns and the weft yarns Wy are each independently preferably in the range of 2.0 yarns / 25 mm to 40.0 yarns / 25 mm, more preferably in the range of 3.0 yarns / 25 mm to 33.0 yarns / 25 mm, and further preferably in the range of 3.8 yarns / 25 mm to 29.0 yarns / 25 mm.

[0033] In addition, the ratio Wt / Wy of the weaving density Wt of the warp yarn to the weaving density Wy of the weft yarn is, for example, in the range of greater than 0.90 and less than 1.10, preferably in the range of greater than 0.95 and less than 1.05, more preferably in the range of greater than 0.97 and less than 1.03, further preferably in the range of greater than 0.98 and less than 1.02, particularly preferably in the range of greater than 0.99 and less than 1.01, and most preferably in the range of 1.00.

[0034] In addition, in the glass cloth of the present embodiment, when the average yarn width Bt of the warp yarn and the average yarn width By of the weft yarn are each independently less than 550 μm, it is sometimes not possible to sufficiently suppress the generation of gaps between the warp yarns or between the weft yarns. On the other hand, when the average yarn width Bt of the warp yarn and the average yarn width By of the weft yarn each independently exceed 10000 μm, it is sometimes not possible to sufficiently suppress the generation of gaps between the filaments.

[0035] Preferably, the average yarn width Bt of the warp yarn and the average yarn width By of the weft yarn are independently in the range of 1000 μm or more and 5500 μm or less, and more preferably in the range of 1200 μm or more and 3450 μm or less.

[0036] In addition, the ratio Bt / By of the average yarn width Bt of the above-mentioned warp yarn to the average yarn width By of the above-mentioned weft yarn is, for example, in the range of greater than 0.80 and less than 1.20, preferably in the range of greater than 0.85 and less than 1.15, more preferably in the range of greater than 0.90 and less than 1.10, further preferably in the range of greater than 0.93 and less than 1.07, particularly preferably in the range of greater than 0.95 and less than 1.05, particularly preferably in the range of greater than 0.96 and less than 1.04, and most preferably in the range of greater than 0.97 and less than 1.03.

[0037] The coefficient of variation of the yarn width of the warp yarn (standard deviation of the yarn width of the warp yarn / average yarn width of the warp yarn Bt) and the coefficient of variation of the yarn width of the weft yarn (standard deviation of the yarn width of the weft yarn / average yarn width of the weft yarn By) are each independently, for example, 0.20 or less, preferably 0.15 or less, more preferably 0.10 or less, and further preferably 0.05 or less. In addition, as the lower limit of the coefficient of variation of the yarn width of the warp yarn and the coefficient of variation of the yarn width of the weft yarn, 0.01 can be cited. In addition, the average value of the coefficient of variation of the yarn width of the warp yarn and the coefficient of variation of the yarn width of the weft yarn is, for example, 0.20 or less, preferably 0.15 or less, more preferably 0.10 or less, and further preferably 0.05 or less.

[0038] In the glass cloth of this embodiment, if the warp yarn opening efficiency coefficient Pt is less than 0.600 or exceeds 1.500, it is difficult to reduce the delay time difference of the printed wiring board. The warp yarn opening efficiency coefficient Pt is obtained from the Dt, Ft, Wt and Bt by the formula (1).

[0039] The warp yarn opening efficiency coefficient Pt is preferably in the range of 0.770 to 1.200, more preferably in the range of 0.800 to 1.100, further preferably in the range of 0.890 to 1.000, particularly preferably in the range of 0.925 to 0.970.

[0040] Here, the "Bt / (Dt×Ft)" part in the above formula (1) reflects the degree of occurrence of gaps between the filaments or overlaps between the filaments in the filaments constituting the warp yarn. There is a tendency that the larger "Bt / (Dt×Ft)" is above 1.000, the more gaps are generated between the filaments, and the gaps make it difficult to reduce the delay time difference of the printed wiring board. On the other hand, there is a tendency that the smaller "Bt / (Dt×Ft)" is than 1.000, the more overlaps between the filaments are generated, and the overlaps make it difficult to reduce the delay time difference of the printed wiring board.

[0041] In the above formula (1), the "Bt / (25000 / Wt)" part reflects the degree of occurrence of gaps between the warp yarns or overlaps between the warp yarns. There is a tendency that the larger the value of "Bt / (25000 / Wt)" exceeds 1.000, the more overlaps will occur between the ends of the warp yarns, and the overlap will make it difficult to reduce the delay time difference of the printed wiring board. On the other hand, there is a tendency that the smaller the value of "Bt / (25000 / Wt)" is, the more gaps will occur between the warp yarns, and the gaps will make it difficult to reduce the delay time difference of the printed wiring board.

[0042] In the above formula (1), as described above, the "(Dt×Ft) / (25000 / Wt)" portion preferably has the "Bt / (Dt×Ft)" portion and "Bt / (25000 / Wt)" both close to 1.000, and when the "Bt / (Dt×Ft)" portion and "Bt / (25000 / Wt)" are both close to 1.000, the value of the above formula (1) can be close to 1.000. Therefore, the above formula (1) reflects the above tendency and indicates the possibility of reducing the delay time difference of the printed wiring board caused by the gaps or overlaps between the filaments constituting the above warp yarns, or the gaps or overlaps between the above warp yarns.

[0043] In the glass cloth of the present embodiment, when the weft opening efficiency coefficient Py is less than 0.600 or exceeds 1.500, it is difficult to reduce the delay time difference of the printed wiring board. The weft opening efficiency coefficient Py is obtained from Dy, Fy, Wy and By by the above formula (2).

[0044] The weft opening efficiency coefficient Py is preferably in the range of 0.770 to 1.200, more preferably in the range of 0.800 to 1.100, further preferably in the range of 0.890 to 1.000, particularly preferably in the range of 0.925 to 0.970.

[0045] Here, the above formula (2) represents the possibility of reducing the delay time difference of the printed wiring board caused by the gaps or overlaps between the filaments constituting the above weft yarns, or the gaps or overlaps between the weft yarns, similarly to the above formula (1).

[0046] In addition, the above formula (3) reflects the above characteristics of the above formulas (1) and (2), and shows the possibility of reducing the delay time difference of the printed wiring board caused by the gaps or overlaps between the filaments in the entire glass cloth, or the gaps or overlaps between the filaments.

[0047] In the glass cloth of the present embodiment, if Rt and Ry are each independently less than 68.6, it is difficult to improve the productivity of the glass cloth while reducing the delay time difference of the printed wiring board and reducing the thickness of the glass cloth.

[0048] On the other hand, if Rt and Ry independently exceed 555.5, it is difficult to achieve a stable warp width or weft width, and it is difficult to reduce the delay time difference of the printed wiring board caused by the gaps between the warp yarns or the weft yarns due to the deviation of the yarn width.

[0049] The Rt is the ratio of the number of glass filaments Ft constituting the warp yarn to the filament diameter Dt of the glass filaments constituting the warp yarn (Ft / Dt). In addition, the Ry is the ratio of the number of glass filaments Fy constituting the weft yarn to the filament diameter Dy of the glass filaments constituting the weft yarn (Fy / Dy).

[0050] It is preferred that the above Rt and Ry are each independently in the range of 115.5 or more and 277.2 or less.

[0051] In addition, the ratio Rt / Ry of the above-mentioned Rt to the above-mentioned Ry is, for example, in the range of greater than 0.90 and less than 1.10, and is preferably in the range of greater than 0.95 and less than 1.05, more preferably in the range of greater than 0.97 and less than 1.03, further preferably in the range of greater than 0.98 and less than 1.02, particularly preferably in the range of greater than 0.99 and less than 1.01, and most preferably in the range of 1.00.

[0052] In the glass cloth of the present embodiment, Pt and Py preferably satisfy the following formula (3-1), more preferably satisfy the following formula (3-2), and further preferably satisfy the following formula (3-3).

[0053] 0.800≤(Pt×Py) 1 / 2 ≤1.100…(3-1),

[0054] 0.890≤(Pt×Py) 1 / 2 ≤0.970…(3-2),

[0055] 0.900≤(Pt×Py) 1 / 2 ≤0.952…(3-3).

[0056] In addition, the ratio of the above-mentioned Pt to the above-mentioned Py, Pt / Py, is, for example, in the range of greater than 0.80 and less than 1.20, preferably in the range of greater than 0.85 and less than 1.15, more preferably in the range of greater than 0.90 and less than 1.10, further preferably in the range of greater than 0.93 and less than 1.07, particularly preferably in the range of greater than 0.95 and less than 1.05, particularly preferably in the range of greater than 0.96 and less than 1.04, and most preferably in the range of greater than 0.97 and less than 1.03.

[0057] In addition, in the glass cloth of the present embodiment, the tex count (tex count) (mass in grams per 1 km) of the warp yarn and the weft yarn are independently, for example, in the range of 3.0 to 50.0 tex (g / km), more preferably in the range of 3.5 to 25.0 tex (g / km), and further preferably in the range of 4.0 to 18.0 tex (g / km).

[0058] In the glass cloth of the present embodiment, the warp yarn or the weft yarn may be twisted. At this time, the number of twists of the warp yarn or the number of twists of the weft yarn is independently, for example, in the range of 1.00 times / 25 mm or less, preferably in the range of 0.70 times / 25 mm or less, more preferably in the range of 0.50 times / 25 mm or less, further preferably in the range of 0.40 times / 25 mm or less, particularly preferably in the range of 0.20 times / 25 mm or less, particularly preferably in the range of 0.09 times / 25 mm or less, and most preferably in the range of 0.00 times / 25 mm. Here, according to JIS R 3912:2000, a twist tester is used to calculate the number of twists of the warp yarn or the weft yarn based on the number of twists required for untwisting the test piece and the length of the test piece under the standard tension before untwisting.

[0059] The glass cloth of the present embodiment has the above-mentioned structure and has a thickness of less than 10.0 μm, preferably 9.4 μm or less, more preferably 9.0 μm or less, and further preferably 8.5 μm or less. The lower limit of the thickness of the glass cloth of the present embodiment is, for example, 2.0 μm.

[0060] The mass per unit area of ​​the glass cloth of the present embodiment is, for example, 5.0 to 30.0 g / m 2 The range is preferably between 6.0 and 24.0 g / m 2 The range is preferably 7.0 to 21.0 g / m 2 The range is particularly preferably 8.0 to 16.0 g / m 2 Here, the mass per unit area of ​​the glass cloth is the average value of: the mass of three glass cloths cut into a size of 200 mm × 200 mm is measured using a scale in accordance with JIS R3420:2013, and the mass per 1 m2 The quality values ​​are taken as the average value.

[0061] In the glass cloth of this embodiment, the ratio of the mass per unit area of ​​the glass cloth to the thickness of the glass cloth (mass per unit area of ​​the glass cloth / thickness of the glass cloth) is, for example, in the range of 1.20 to 3.60, preferably in the range of 1.25 to 2.50, and more preferably in the range of 1.30 to 1.95.

[0062] In the glass cloth of the present embodiment, it is preferred that the filament diameter Dt of the glass filaments constituting the warp yarns and the filament diameter Dy of the glass filaments constituting the weft yarns are independently within a range of 2.0 μm to 3.8 μm, and that Pt and Py satisfy the following formula (4).

[0063] 0.890≤(Pt×Py) 1 / 2 ≤0.970…(4).

[0064] The filament diameter of the warp yarn or the weft yarn is the average value of the following measured values: the measured value when the diameter of each 50 cross sections of the glass filaments constituting the warp yarn or the weft yarn is measured using a scanning electron microscope (manufactured by Hitachi High-Technologies Corporation, trade name: S-3400N, magnification: 3000 times). In addition, the number of glass filaments constituting the warp yarn or the weft yarn is the average value of the following measured values: the average value of the measured value when the number of each 50 cross sections of the glass filaments constituting the warp yarn or the weft yarn is measured using a scanning electron microscope (manufactured by Hitachi High-Technologies Corporation, trade name: S-3400N, magnification: 500 times).

[0065] In addition, the weaving density of the warp yarn can be obtained by the following method: according to JIS R3420, the number of warp yarns in the range of 25 mm in the weft direction can be counted using a fabric analyzer. In addition, the weaving density of the weft yarn can be obtained by the following method: according to JIS R 3420, the number of weft yarns in the range of 25 mm in the warp direction can be counted using a fabric analyzer.

[0066] In addition, the average yarn width of the above-mentioned warp yarn or the above-mentioned weft yarn is the average value of the following measured values: three samples of 100 mm×100 mm are cut out from respective separated positions of the glass cloth, and the yarn widths of 10 warp yarns or weft yarns in each sample are measured using a microscope (manufactured by KEYENCE Co., Ltd., trade name: VHX-6000, magnification: 200 times).

[0067] The thickness of the glass cloth is a value measured at 15 locations on the glass cloth using a micrometer in accordance with JISR 3420:2013.

[0068] The glass filaments can be obtained by melting a predetermined glass batch (glass raw material) and fiberizing it. For example, glass filaments having a composition of E glass fiber (general-purpose glass fiber), a high-strength glass fiber, a low dielectric constant glass fiber, etc. can be used.

[0069] Here, the above-mentioned E glass fiber composition is as follows: it contains 52-56 mass% of SiO2, 5-10 mass% of B2O3, 12-16 mass% of Al2O3, a total of 20-25 mass% of CaO and MgO, and a total of 0-1 mass% of Na2O, K2O and Li2O.

[0070] In addition, the above-mentioned high-strength glass fiber composition is as follows: it contains 57-70 mass% of SiO2, 18-30 mass% of Al2O3, 0-13 mass% of CaO, 5-15 mass% of MgO, a total of 0-1 mass% of Na2O, K2O and Li2O, 0-1 mass% of TiO2, and 0-2 mass% of B2O3.

[0071] In addition, the above-mentioned low dielectric constant glass fiber has the following composition: 48 to 62 mass% of SiO2, 17 to 26 mass% of B2O3, 9 to 18 mass% of Al2O3, 0.1 to 9 mass% of CaO, 0 to 6 mass% of MgO, a total of 0.05 to 0.5 mass% of Na2O, K2O and Li2O, 0 to 5 mass% of TiO2, 0 to 6 mass% of SrO, a total of 0 to 3 mass% of F2 and Cl2, and 0 to 6 mass% of P2O5.

[0072] From the viewpoint of versatility, the glass filaments are preferably the E glass fiber composition, and from the viewpoint of suppressing warpage after being made into prepreg, the glass filaments are preferably the high-strength glass fiber composition. In this case, the high-strength glass fiber composition further preferably contains 64-66% by mass of SiO2, 24-26% by mass of Al2O3, 9-11% by mass of MgO, and contains SiO2, Al2O3 and MgO in a total amount of more than 99% by mass.

[0073] The glass filaments having a number of 150 to 3000 are bundled by a known method and wound on a winding tube, or further unwound from the winding tube to a bobbin. The material formed by winding the bundled glass filaments (glass strands) on the winding tube is sometimes called a spindle. In addition, the device formed by winding the glass strands on the bobbin is sometimes called a glass yarn package.

[0074] Here, the glass filaments usually have a circular cross-sectional shape, but may also have a flat cross-sectional shape such as an ellipse or an oblong. When the glass filaments have a flat cross-sectional shape, the ratio of major diameter / minor diameter is, for example, in the range of 1.1 to 10.0. In addition, when the glass filaments have a flat cross-sectional shape, the filament diameter refers to the diameter of a circle having the same area as the flat cross-sectional shape. It should be noted that when the glass filaments have a circular cross-sectional shape, the ratio of major diameter / minor diameter is equivalent to 1.0.

[0075] The above-mentioned glass raw yarn is pulled out from the above-mentioned spindle or the above-mentioned glass yarn is pulled out from the above-mentioned glass yarn package, the number of twists of the above-mentioned glass raw yarn or the above-mentioned glass yarn package is adjusted as needed, and the yarn is opened, thereby the above-mentioned warp yarn and the above-mentioned weft yarn used for the glass cloth of this embodiment can be obtained.

[0076] In order to facilitate the opening of the glass strands or the glass yarn packages in the yarn opening process, the twist number of the glass strands or the glass yarn packages is adjusted. The twist number of the glass strands or the glass yarn packages can be adjusted to, for example, 1.0 times / 25 mm or less, preferably 0.7 times / 25 mm or less, and more preferably 0.2 times / 25 mm or less. The twist number of the glass strands or the glass yarn packages can be adjusted using an untwisting machine or a twisting machine.

[0077] Examples of the yarn opening treatment include opening using water pressure, opening using high-frequency vibrations such as ultrasonic waves using a liquid as a medium, opening using fluid pressure having a surface pressure, and opening using roller pressure.

[0078] The glass cloth of this embodiment can be obtained by weaving the warp yarn and the weft yarn using a known loom and performing a fiber opening treatment. Examples of the loom include jet looms such as air jet looms and water jet looms, shuttle looms, rapier looms, etc. In addition, examples of weaving methods using the loom include plain weave, satin weave, basket weave, twill weave, etc.

[0079] Examples of the fiber-opening treatment include fiber-opening using water pressure, fiber-opening using high-frequency vibrations such as ultrasonic waves using liquid as a medium, fiber-opening using fluid pressure having surface pressure, and fiber-opening using roller pressure. Among these fiber-opening treatments, fiber-opening using water pressure or fiber-opening using high-frequency vibrations such as ultrasonic waves using liquid as a medium can reduce the yarn width deviation of the warp yarn and the weft yarn after the fiber-opening treatment, respectively, and therefore the fiber-opening treatment is preferred. In addition, by using a plurality of fiber-opening treatment methods in combination as the fiber-opening treatment, it is possible to suppress the appearance defects of the glass cloth such as weft skew caused by the fiber-opening treatment.

[0080] The glass cloth of this embodiment may be subjected to surface treatment so that a treatment liquid containing a silane coupling agent is attached to the surface of the glass cloth. Here, the surface treatment may be performed, for example, by applying a treatment liquid containing the silane coupling agent by a known method and drying the treatment liquid.

[0081] Examples of the silane coupling agent include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, and (meth)acrylic silane. In the glass cloth of the present embodiment, the above silane coupling agents may be used alone or in combination of two or more.

[0082] Examples of the aminosilane include γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N′-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinopropyltrimethoxysilane.

[0083] Examples of the chlorosilane include γ-chloropropyltrimethoxysilane and the like.

[0084] Examples of the epoxysilane include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane.

[0085] Examples of the mercaptosilane include γ-mercaptotrimethoxysilane and the like.

[0086] Examples of the vinyl silane include vinyltrimethoxysilane and N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane.

[0087] Examples of the (meth)acrylic silane include γ-methacryloxypropyltrimethoxysilane and the like.

[0088] Furthermore, the treatment liquid containing the silane coupling agent may contain, for example, a surfactant and a pH adjuster in addition to the silane coupling agent.

[0089] Examples of the surfactant include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants. In the glass cloth of the present embodiment, the surfactants described above may be used alone or in combination of two or more thereof.

[0090] Examples of the nonionic surfactant include ethylene oxide propylene oxide alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene-polyoxypropylene-block copolymer ethers, alkyl polyoxyethylene-polyoxypropylene-block copolymer ethers, polyoxyethylene fatty acid esters, polyoxyethylene fatty acid monoesters, polyoxyethylene fatty acid diesters, polyoxyethylene sorbitan fatty acid esters, glycerol fatty acid ester ethylene oxide adducts, polyoxyethylene stearyl ethers, hydrogenated castor oil ethylene oxide adducts, alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, glycerol fatty acid esters, polyglycerol fatty acid esters, pentaerythritol fatty acid esters, sorbitol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyhydric alcohol alkyl ethers, fatty acid alkanolamides, acetylene glycols, acetylene alcohols, ethylene oxide adducts of acetylene glycols, and ethylene oxide adducts of acetylene alcohols.

[0091] Examples of the cationic surfactant include alkyl dimethyl benzyl ammonium chloride, alkyl trimethyl ammonium chloride, alkyl dimethyl ethyl ammonium ethyl sulfate, higher alkyl amine acetates, ethylene oxide adducts of higher alkyl amines, condensates of higher fatty acids and polyalkylene polyamines, salts of esters of higher fatty acids and alkanolamines, higher fatty acid amide salts, imidazoline type cationic surfactants, and alkyl pyridinium salts. Examples of the higher alkyl amine acetates include acetates and hydrochlorides.

[0092] Examples of the anionic surfactant include higher alcohol sulfates, higher alkyl ether sulfates, α-olefin sulfates, alkylbenzene sulfonates, α-olefin sulfonates, reaction products of fatty acid halides and N-methyltaurine, dialkyl sulfosuccinates, higher alcohol phosphates, and phosphates of higher alcohol ethylene oxide adducts.

[0093] Examples of the amphoteric surfactant include amino acid-type amphoteric surfactants such as alkylaminopropionic acid alkali metal salts, betaine-type amphoteric surfactants such as alkyldimethylbetaine, and imidazoline-type amphoteric surfactants.

[0094] Examples of the pH adjuster include acetic acid, formic acid and propionic acid.

[0095] When the glass cloth of the present embodiment is subjected to surface treatment and has organic matter attached thereto, the amount of the organic matter attached thereto is, for example, in the range of 0.05 to 5.00 parts by mass relative to 100 parts by mass of the glass cloth having the organic matter attached thereto. Here, the ratio of the mass of the organic matter to the mass of the glass cloth having the organic matter attached thereto can be obtained by measuring the mass of the test piece before and after heating and drying in accordance with JIS R3420:2013. It should be noted that when the mass of the glass cloth is reduced due to heating and drying, the amount of the organic matter attached thereto is measured taking into account the reduced amount.

[0096] The prepreg of the present embodiment includes the glass cloth of the present embodiment described above.

[0097] The prepreg of the present embodiment can be obtained by impregnating the above-mentioned glass cloth with a resin by a method known per se and semi-curing the impregnated glass cloth.

[0098] In the prepreg of this embodiment, the resin impregnated in the above-mentioned glass cloth is not particularly limited. As a thermosetting resin of such resin, for example, epoxy resin, phenolic resin, unsaturated polyester resin, melamine resin, modified polyimide resin, maleimide resin, thermosetting polyphenylene ether resin, thermosetting modified polyphenylene ether resin, etc. can be cited. In addition, as a thermoplastic resin, polyamide resin, polyimide resin, polybutylene terephthalate resin, polyethylene terephthalate resin, polyphenylene sulfide resin, polyphenylene ether resin, thermoplastic modified polyphenylene ether resin, fluororesin, liquid crystal polymer (LCP), cycloolefin resin, etc. can be cited.

[0099] Furthermore, the printed wiring board of the present embodiment is formed of a prepreg including the glass cloth of the present embodiment described above.

[0100] The glass cloth of the present embodiment can be used for a housing of an electronic device, a separator of a fuel cell, and the like in addition to a printed wiring board.

[0101] Next, examples of the present invention and comparative examples are shown.

[0102] Example

[0103] 〔Reference Example 1〕

[0104] In this reference example, first, glass filaments composed of E glass fibers are spun to obtain glass yarns constituting the basis of warp yarns and weft yarns. The warp yarns and weft yarns are respectively formed by bundling glass filaments having a filament number (Ft, Fy) of 38 and a filament diameter (Dt, Dy) of 3.6 μm, and have a mass of 0.99 tex (g / km).

[0105] Next, the warp and weft yarns were woven using a rapier loom so that the warp yarn weaving density (Wt) was 105 yarns / 25 mm and the weft yarn weaving density (Wy) was 110 yarns / 25 mm to obtain a plain woven glass cloth. Next, the plain woven glass cloth was subjected to deoiling treatment, surface treatment and fiber opening treatment.

[0106] The deoiling treatment was performed by placing the woven glass cloth in a heating furnace at an atmosphere temperature of 350°C to 400°C for 60 hours, and thermally decomposing the spinning sizing agent and the weaving sizing agent attached to the woven glass cloth. In addition, as the surface treatment, methacryloylsilane was applied to the woven glass cloth and cured while continuously passing through a heating furnace at 130°C. In addition, as the fiber opening treatment, a tension of 50N was applied to the warp yarn of the woven glass cloth, and the fiber opening treatment was performed by setting the water pressure to 1.0 MPa.

[0107] It should be noted that the tension applied to the warp yarn of the above-mentioned plain woven glass cloth in the process other than the above-mentioned fiber opening treatment was 70 to 120 N. In the above-mentioned fiber opening treatment, the value of the tension detected by the tension detector was fed back to the guide roller conveying the above-mentioned plain woven glass cloth, and the tension was adjusted by changing the position of the guide roller. As a result, the glass cloth shown in Table 2 was obtained.

[0108] Next, the glass cloth obtained in this reference example is immersed in an epoxy resin diluted with methyl ethyl ketone (manufactured by DIC Corporation, trade name: EPICLON121N-80N), the resin is impregnated into the glass cloth, and the glass cloth is passed through a slit with a width of 13 μm to remove excess resin. The glass cloth is then kept at a temperature of 150°C for 1 minute in a dryer to semi-cure the glass cloth impregnated with the epoxy resin to prepare a prepreg.

[0109] Next, four sheets of the obtained prepreg were stacked, and heated and pressed under conditions of 200° C. and 3 MPa for 2 hours to prepare an evaluation substrate A which is a cured product of the prepreg.

[0110] Next, three sheets of the obtained prepreg were stacked, copper foil (manufactured by Furukawa Electric Co., Ltd., trade name: FV-WS) was placed on both sides, and heated and pressed for 2 hours at 200°C and 3 MPa to prepare an evaluation substrate B. The evaluation substrate B was a copper-clad laminate (metal-clad laminate) with a thickness of 200 μm and copper foil bonded to both sides.

[0111] Next, the metal foil (copper foil) on one side of the evaluation substrate B was processed to form 10 wirings with a yarn width of 100 to 300 μm, a line length of 100 mm, and a line spacing of 20 mm. Prepreg and metal foil (copper foil) were laminated twice on the surface of the evaluation substrate B on the side where the wiring was formed, thereby forming a three-layer board. It should be noted that the yarn width of the wiring was adjusted so that the circuit characteristic impedance of the three-layer board after the production became 50Ω.

[0112] Next, the delay time of the above three-layer board at 20 GHz was measured, and the difference between the maximum value and the minimum value of the obtained delay time was calculated as the delay time difference.

[0113] Furthermore, there is a tendency that when the delay time difference is large, the signal quality is easily degraded due to the skew of the differential signal, while when the delay time difference is small, the signal quality is not easily degraded due to the skew. Therefore, the signal quality based on the skew can be evaluated using the delay time difference as an indicator.

[0114] [Example 1]

[0115] In this embodiment, first, glass filaments having an E glass fiber composition are spun to obtain glass yarns constituting the basis of warp yarns and weft yarns. The glass yarns are formed by bundling 496 glass filaments with a filament diameter of 3.6 μm and have a mass of 12.92 tex (g / km).

[0116] Next, the glass yarn wound on the bobbin is twisted in a direction opposite to the twisting direction of the glass yarn, and is pulled out from the bobbin, and is sent out without being twisted, and the glass yarn is opened in a water tank at 60°C by applying ultrasonic waves generated by a vibrator with a frequency of 100 kHz and an output power of 1.2 kW. Next, the opened glass yarn (opened glass yarn) is wound on the bobbin in a manner that the opening direction of the glass yarn is parallel to the longitudinal direction of the bobbin, thereby obtaining a opened glass yarn package.

[0117] The average yarn width of the above-mentioned open fiber glass yarn as the basis of the warp and weft yarn is 1700 μm. Here, the measured values ​​of the yarn width of the above-mentioned open fiber glass yarn are measured at 30 positions every 10 cm using a microscope (manufactured by KEYENCE Co., Ltd., trade name: VHX-6000), and the average yarn width of the above-mentioned open fiber glass yarn is calculated based on the measured values.

[0118] Next, the above-mentioned open fiber glass yarn was pulled out from a plurality of the above-mentioned open fiber glass yarn packages to form warp yarn or weft yarn, and a plain woven glass cloth having a warp weaving density (Wt) of 14.0 yarns / 25 mm and a weft weaving density (Wy) of 14.0 yarns / 25 mm was woven using a rapier loom. Next, the above-mentioned plain woven glass cloth was subjected to deoiling treatment, surface treatment and open fiber treatment in exactly the same manner as in Reference Example 1. As a result, the glass cloth shown in Table 1 was obtained.

[0119] Next, except for using the glass cloth of this embodiment, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0120] Next, the degree of reduction in the delay time difference of the glass cloth of this example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in the following manner.

[0121] [Degree of reduction of delay time difference]

[0122] Taking the delay time difference of Reference Example 1 as a benchmark, the case where the delay time difference is 50% or less is evaluated as "A (excellent)", the case where the delay time difference is more than 50% and less than 90% is evaluated as "B (good)", and the case where the delay time difference is more than 90% is evaluated as "C (acceptable ~ equivalent)".

[0123] [Glass cloth width stability]

[0124] Three samples of 100 mm x 100 mm were cut out at mutually separated positions of the glass cloth, and the yarn widths of 10 warp yarns or weft yarns of each sample were measured using a microscope (manufactured by KEYENCE Co., Ltd., trade name: VHX-6000). Based on the measured values, the average value and standard deviation of the warp yarns and the weft yarns were calculated, and the coefficient of variation (standard deviation / average value) was calculated based on the average value and the standard deviation. Next, the average value (average coefficient of variation) of the coefficient of variation of the warp yarns and the coefficient of variation of the weft yarns was calculated. The case where the average coefficient of variation was 0.10 or less was evaluated as "A", and the case where the average coefficient of variation exceeded 0.10 was evaluated as "B".

[0125] [Glass cloth productivity]

[0126] The time required to weave 1000 m of glass cloth using a rapier loom (1000 m weaving time) was measured. Based on the 1000 m weaving time of Reference Example 1, a case where the 1000 m weaving time was 30% or less was evaluated as "OK", and a case where the 1000 m weaving time exceeded 30% was evaluated as "NG".

[0127] [Example 2]

[0128] In this example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 334 glass filaments with a filament diameter of 3.6 μm and having a mass of 8.70 tex (g / km). Next, a glass yarn having an average yarn width of 1081 μm obtained by opening the glass yarns was used, and the warp yarn weaving density (Wt) was set to 20.8 yarns / 25 mm, and the weft yarn weaving density (Wy) was set to 20.8 yarns / 25 mm. The glass cloth shown in Table 1 was obtained in exactly the same manner as in Example 1 except that the above-mentioned glass yarns were opened and the average yarn width was 1081 μm.

[0129] Next, except for using the glass cloth of this embodiment, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0130] Next, the degree of reduction in the delay time difference of the glass cloth of this example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 1.

[0131] [Example 3]

[0132] In this example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 360 glass filaments with a filament diameter of 2.6 μm and having a mass of 4.89 tex (g / km). Next, a glass yarn having an average yarn width of 925 μm obtained by opening the glass yarns was used, and the warp yarn weaving density (Wt) was set to 26.0 yarns / 25 mm, and the weft yarn weaving density (Wy) was set to 26.0 yarns / 25 mm, and the glass cloth shown in Table 1 was obtained in exactly the same manner as in Example 1, except that the above-mentioned glass yarns were opened and the average yarn width was 925 μm.

[0133] Next, except for using the glass cloth of this embodiment, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0134] Next, the degree of reduction in the delay time difference of the glass cloth of this example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 1.

[0135] [Example 4]

[0136] In this example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 1500 glass filaments with a filament diameter of 3.6 μm and having a mass of 39.08 tex (g / km). Next, a glass yarn having an average yarn width of 5260 μm obtained by opening the glass yarns was used, and the warp yarn weaving density (Wt) was set to 4.7 yarns / 25 mm, and the weft yarn weaving density (Wy) was set to 4.7 yarns / 25 mm. The glass cloth shown in Table 1 was obtained in exactly the same manner as in Example 1 except that the above-mentioned glass yarns were opened and the average yarn width was 5260 μm.

[0137] Next, except for using the glass cloth of this embodiment, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0138] Next, the degree of reduction in the delay time difference of the glass cloth of this example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 1.

[0139] [Example 5]

[0140] In this embodiment, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 496 glass filaments with a filament diameter of 3.6 μm and having a mass of 12.92 tex (g / km). Next, the glass yarns were opened in the same manner as in Embodiment 1 except that a vibrator with a frequency of 100 kHz and an output power of 1.6 kW was used to obtain opened glass yarns with an average yarn width of 2230 μm, and the warp weaving density (Wt) was set to 14.0 yarns / 25 mm and the weft weaving density (Wy) was set to 14.0 yarns / 25 mm, and the glass cloth shown in Table 1 was obtained in the same manner as in Embodiment 1 except that the warp weaving density (Wt) was set to 14.0 yarns / 25 mm and the weft weaving density (Wy) was set to 14.0 yarns / 25 mm.

[0141] Next, except for using the glass cloth of this embodiment, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0142] Next, the degree of reduction in the delay time difference of the glass cloth of this example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 1.

[0143] [Example 6]

[0144] In this example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 550 glass filaments with a filament diameter of 4.0 μm and having a mass of 17.69 tex (g / km). Next, a glass yarn having an average yarn width of 2120 μm obtained by opening the glass yarn was used, and the warp weaving density (Wt) was set to 11.3 yarns / 25 mm, and the weft weaving density (Wy) was set to 11.3 yarns / 25 mm, and the glass cloth shown in Table 1 was obtained in exactly the same manner as in Example 1 except that the above-mentioned glass yarn was opened and the average yarn width was 2120 μm.

[0145] Next, except for using the glass cloth of this embodiment, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0146] Next, the degree of reduction in the delay time difference of the glass cloth of this example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 1.

[0147] [Comparative Example 1]

[0148] In this comparative example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 496 glass filaments with a filament diameter of 3.6 μm and having a mass of 12.92 tex (g / km). Next, the glass yarns were opened in the same manner as in Example 1 except that a vibrator with a frequency of 100 kHz and an output power of 0.6 kW was used to obtain opened glass yarns with an average yarn width of 891 μm, and the warp weaving density (Wt) was set to 28.0 yarns / 25 mm and the weft weaving density (Wy) was set to 28.0 yarns / 25 mm, and the glass cloth shown in Table 2 was obtained in the same manner as in Example 1 except that the warp weaving density (Wt) was set to 28.0 yarns / 25 mm and the weft weaving density (Wy) was set to 28.0 yarns / 25 mm.

[0149] Next, except for using the glass cloth of this comparative example, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0150] Next, the degree of reduction in the delay time difference of the glass cloth of this comparative example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 2.

[0151] [Comparative Example 2]

[0152] In this comparative example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 496 glass filaments with a filament diameter of 3.6 μm and having a mass of 12.92 tex (g / km). Next, the glass yarns were opened in the same manner as in Example 1 except that a vibrator with a frequency of 100 kHz and an output power of 0.8 kW was used to obtain opened glass yarns with an average yarn width of 1158 μm, and the warp weaving density (Wt) was set to 14.0 yarns / 25 mm and the weft weaving density (Wy) was set to 14.0 yarns / 25 mm, and the glass cloth shown in Table 2 was obtained in the same manner as in Example 1 except that the warp weaving density (Wt) was set to 14.0 yarns / 25 mm and the weft weaving density (Wy) was set to 14.0 yarns / 25 mm.

[0153] Next, except for using the glass cloth of this comparative example, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0154] Next, the degree of reduction in the delay time difference of the glass cloth of this comparative example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 2.

[0155] [Comparative Example 3]

[0156] In this comparative example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 2500 glass filaments with a filament diameter of 3.6 μm and having a mass of 65.13 tex (g / km). Next, a glass yarn having an average yarn width of 8760 μm obtained by opening the glass yarn was used, and the warp yarn weaving density (Wt) was set to 2.8 yarns / 25 mm, and the weft yarn weaving density (Wy) was set to 2.8 yarns / 25 mm. The glass cloth shown in Table 2 was obtained in exactly the same manner as in Example 1 except that the above-mentioned glass yarn was opened and the average yarn width was 8760 μm.

[0157] Next, except for using the glass cloth of this comparative example, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0158] Next, the degree of reduction in the delay time difference of the glass cloth of this comparative example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 2.

[0159] [Comparative Example 4]

[0160] In this comparative example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 160 filaments with a filament diameter of 3.6 μm and having a mass of 4.17 tex (g / km). Next, a glass yarn having an average yarn width of 550 μm obtained by opening the glass yarn was used, and the warp weaving density (Wt) was set to 43.4 yarns / 25 mm, and the weft weaving density (Wy) was set to 43.4 yarns / 25 mm. The glass cloth shown in Table 2 was obtained in exactly the same manner as in Example 1 except that the above-mentioned glass yarn was opened and the warp weaving density (Wt) was set to 43.4 yarns / 25 mm, and the weft weaving density (Wy) was set to 43.4 yarns / 25 mm.

[0161] Next, except for using the glass cloth of this comparative example, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0162] Next, the degree of reduction in the delay time difference of the glass cloth of this comparative example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 2.

[0163] [Comparative Example 5]

[0164] In this comparative example, first, glass filaments composed of E glass fibers were spun to obtain glass yarns constituting the basis of warp yarns and weft yarns, the glass yarns being composed of 689 glass filaments with a filament diameter of 5.0 μm and having a mass of 34.63 tex (g / km). Next, a glass yarn having an average yarn width of 3250 μm obtained by opening the glass yarns was used, and the warp yarn weaving density (Wt) was set to 7.3 yarns / 25 mm, and the weft yarn weaving density (Wy) was set to 7.3 yarns / 25 mm, and the glass cloth shown in Table 2 was obtained in exactly the same manner as in Example 1 except that the above-mentioned glass yarns were opened and the average yarn width was 3250 μm.

[0165] Next, except for using the glass cloth of this comparative example, a prepreg, an evaluation substrate A as a cured product of the prepreg, and a three-layer board consisting of an evaluation substrate B as a copper-clad laminate (metal-clad laminate) are prepared in exactly the same manner as in Reference Example 1, and the delay time difference of the three-layer board is calculated.

[0166] Next, the degree of reduction in the delay time difference of the glass cloth of this comparative example, the stability of the glass cloth yarn width, and the glass cloth productivity were evaluated in exactly the same manner as in Example 1. The results are shown in Table 2.

[0167] [Table 1]

[0168] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Warp yarn filament diameter (μm); Dt 3.6 3.6 2.6 3.6 3.6 4.0 Number of warp filaments (pieces); Ft 496 334 360 1500 496 550 Warp yarn weaving density (root / 25mm); Wt 14.0 20.8 26.0 4.7 11.0 11.3 Average warp yarn width (μm); Bt 1690 1080 920 5250 2200 2100 Warp filament number / warp filament diameter; Rt 137.8 92.8 138.5 416.7 137.8 137.5 Warp yarn opening efficiency coefficient; Pt 0.946 0.899 0.944 0.994 0.858 0.947 Weft yarn filament diameter (μm); Dy 3.6 3.6 2.6 3.6 3.6 4.0 Number of weft filaments (roots); Fy 496 334 360 1500 496 550 Weft yarn weaving density (root / 25mm); Wy 14.0 20.8 26.0 4.7 11.0 11.3 Average weft yarn width (μm); By 1710 1083 930 5270 2250 2130 Weft yarn filament number / weft yarn filament diameter; Rv 137.8 92.8 138.5 416.7 137.8 137.5 Weft yarn opening efficiency coefficient; Py 0.958 0.901 0.954 0.998 0.878 0.960 <![CDATA[(Pt×Py) 1 / 2 ]]> 0.952 0.900 0.949 0.996 0.868 0.953 Glass cloth thickness (μm) 8.0 8.0 5.7 8.4 8.0 9.2 Degree of reduction of delay time difference A A A A B A Glass cloth yarn width stability A A A B A A Glass cloth productivity OK OK OK OK OK OK

[0169] Pt;{(Bt / (Dt×Ft))×Bt / (25000 / Wt)} 1 / 2 ×(Dt×Ft) / (25000 / Wt)}

[0170] Py;{(By / (Dy×Fy))×By / (25000 / Wy)} 1 / 2 ×(Dy×Fy) / (25000 / Wy)}

[0171] [Table 2]

[0172] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Reference Example 1 Warp yarn filament diameter (μm); Dt 3.6 3.6 3.6 3.6 5.0 3.6 Number of warp filaments (pieces); Ft 496 496 2500 160 689 38 Warp yarn weaving density (root / 25m); Wt 28.0 14.0 2.8 43.4 7.3 105 Average warp yarn width (μm); Bt 890 1155 8750 540 3250 137 Warp filament number / warp filament diameter; Rt 137.8 137.8 694.4 44.4 137.8 10.6 Warp yarn opening efficiency coefficient; Pt 1.410 0.647 0.984 0.937 0.952 0.436 Weft yarn filament diameter (μm); Dy 3.6 3.6 3.6 3.6 5.0 3.6 Number of weft filaments (roots); Fy 496 496 2500 160 689 38 Weft yarn weaving density (root / 25m); Wy 28.0 14.0 2.8 43.4 7.3 110 Average weft yarn width (μm); 892 1160 8760 560 3250 185 Weft yarn filament number / weft yarn filament diameter; Ry 137.8 137.8 694.4 44.4 137.8 10.6 Weft yarn opening efficiency coefficient; Py 1.413 0.650 0.985 0.972 0.952 0.632 <![CDATA[(Pt×Py) 1 / 2 ]]> 1.411 0.648 0.984 0.955 0.952 0.525 Glass cloth thickness (μm) 9.5 8.0 9.5 8.0 13.5 10.0 Degree of reduction of delay time difference C C C A A C Glass cloth yarn width stability A A B A A - Glass cloth productivity OK OK OK NG OK -

[0173] Pt;{(Bt / (Dt×Ft))×Bt / (25000 / Wt)} 1 / 2 ×(Dt×Ft) / (25000 / Wt)}

[0174] Py;{(By / (Dy×Fy))×By / (25000 / Wy)} 1 / 2 ×(Dy×Fy) / (25000 / Wy)}

[0175] As apparent from Table 1, according to the glass cloths of Examples 1 to 6 of the present invention, the yarn widths of the warp and weft yarns are stable, the delay time difference of the printed wiring board is reduced, the degradation of signal quality can be suppressed, and high productivity can be achieved.

[0176] On the other hand, as is apparent from Table 2, the glass cloths of Comparative Examples 1 and 2, whose warp yarn opening efficiency coefficient Pt and weft yarn opening efficiency coefficient Py do not satisfy the above formula (3), have a degree of reduction in the delay time difference comparable to that of the glass cloth of Reference Example 1.

[0177] In addition, it is clear that the glass cloth of Comparative Example 3 in which Rt and Ry exceed 555.5 has a degree of reduction in delay time difference comparable to that of the glass cloth of Reference Example 1 and has poor stability in glass cloth yarn width.

[0178] In addition, it is clear that the glass cloth of Comparative Example 4 in which Rt and Ry are less than 68.6 has a problem of poor productivity of the glass cloth.

[0179] In addition, it is clear that the glass cloth of Comparative Example 5, in which the filament diameter Dt of the glass filaments constituting the warp yarns and the filament diameter Dy of the glass filaments constituting the weft yarns exceed 4.5 μm, has a thickness exceeding 10.0 μm.

Claims

1. A glass cloth, which is composed of warp yarns and weft yarns respectively formed by bundling a plurality of glass filaments, wherein the glass cloth is characterized in that: The filament diameter Dt of the glass filaments constituting the warp yarn and the filament diameter Dy of the glass filaments constituting the weft yarn are each independently within a range of 0.5 μm or more and 4.5 μm or less, The number of glass filaments Ft constituting the warp yarn and the number of glass filaments Fy constituting the weft yarn are independently in the range of 150 or more and 3000 or less, The weaving density Wt of the warp yarns and the weaving density Wy of the weft yarns are independently within a range of 1.0 yarn / 25 mm or more and 50.0 yarn / 25 mm or less, The average yarn width Bt of the warp yarn and the average yarn width By of the weft yarn are each independently within a range of 550 μm or more and 10000 μm or less, The warp yarn opening efficiency coefficient Pt obtained by the following formula (1) from the Dt, the Ft, the Wt and the Bt is in the range of 0.600 to 1.500, and the weft yarn opening efficiency coefficient Py obtained by the following formula (2) from the Dy, the Fy, the Wy and the By is in the range of 0.600 to 1.500, The ratio Ft / Dt (Rt) of the number of glass filaments Ft constituting the warp yarn to the filament diameter Dt of the glass filaments constituting the warp yarn, and the ratio Fy / Dy (Ry) of the number of glass filaments Fy constituting the weft yarn to the filament diameter Dy of the glass filaments constituting the weft yarn are independently in the range of 68.6 or more and 555.5 or less, The Pt and the Py satisfy the following formula (3), the thickness of the glass cloth is less than 10.0 μm, Pt={(Bt / (Dt×Ft))×Bt / (25000 / Wt)} 1 / 2 ×{(Dt×Ft) / (25000 / Wt)}…(1), Py={(By / (Dy×Fy))×By / (25000 / Wy)} 1 / 2 ×{(Dy×Fy) / (25000 / Wy)}…(2), 0.770≤(Pt×Py) 1 / 2 ≤1.200 … (3)。 2. The glass cloth according to claim 1, characterized in that: The filament diameter Dt of the glass filaments constituting the warp yarn and the filament diameter Dy of the glass filaments constituting the weft yarn are independently in the range of 2.0 μm or more and 3.8 μm or less, and Pt and Py satisfy the following formula (4): 0.890≤(Pt×Py) 1 / 2 ≤0.970 … (4)。 3. A prepreg, characterized in that: The glass cloth according to claim 1 or 2 is included.

4. A printed wiring board, characterized in that The glass cloth according to claim 1 or 2 is included.

Citation Information

Patent Citations

  • Glass cloth for printed wiring board

    CN102482809A

  • Glass cloth

    CN107709642A

  • Glass Cloth

    CN107896498A

  • Prepreg, metal foil-clad laminate, and printed circuit board

    CN108503868A

  • Glass cloth, prepreg and print circuit board

    JP2019019431A