Preparation method and application of composite membrane material for adsorbing and filtering micro-plastics
Through the composite film material of polymer water-absorbing resin and filler, combined with hydrophobic surface and adsorption base, the problem of microplastic adsorption on the equipment wall in microplastic detection is solved, and efficient and convenient microplastic recycling and detection is achieved, improving the detection results accuracy and safety.
Patent Information
- Application Number
- CN202411221020.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, when detecting microplastics, vacuum suction filtration method easily leads to adsorption of small-particle-sized microplastics on the equipment wall, causing low target substance loss and detection results, and complex operation, making it difficult to process microplastics of different particle sizes at the same time.
The composite membrane material that combines polymer water-absorbing resin and filler is designed to form an autonomous adsorption material to avoid solution overflowing, and filter with a uniform capillary driving force, combining the adsorption base and water-absorbing High-permeable water materials that modify the pattern to achieve effective interception and recycling of microplastics.
It effectively reduces the loss of microplastics, shortens detection time, improves recovery rate, avoids solution spillage, and realizes high-throughput and convenient sample pretreatment without chemical reagents, which is safe and environmentally friendly.
Smart Images

Figure CN119075700A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite membrane materials, and in particular to a composite membrane material for adsorbing and filtering microplastics, and a preparation method and application thereof. Background Art
[0002] As human beings become more and more dependent on plastic products, the amount of plastic waste in the environment is also increasing year by year. At the same time, a new pollutant, microplastics, has been generated. Microplastics are plastic fragments or plastic particles with an average particle diameter of less than 5 mm. Microplastics are now widely present in the atmosphere, water bodies, food, soil, human body, etc., and can exist for a long time. Microplastics are broken into smaller nanoplastics under physical, mechanical, biological degradation or ultraviolet light. After entering the human body, microplastics may interact with proteins and have potential adverse effects on human blood cells.
[0003] At present, when people detect the content of microplastics in samples, they usually use vacuum filtration to shorten the filtration time. However, this method can easily cause small-sized microplastics to be adsorbed on the wall of the equipment, resulting in the loss of the target substance. In addition, for microplastics of different particle sizes, different specifications of filter membranes need to be replaced, which is complicated and time-consuming, and can easily cause the loss of microplastics, thereby underestimating the content of microplastics in the test samples.
[0004] Self-filtration technology utilizes uniform and effective capillary driving force to avoid operational errors caused by external negative pressure. It has a high recovery rate, stable and reproducible results, and is convenient for simultaneous operation of multiple samples, which can meet the needs of high-throughput and convenient sample pre-treatment. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a composite membrane material for adsorbing and filtering microplastics, and a preparation method and application thereof. The present invention utilizes the high water absorption of a polymer water-absorbing resin, combined with a certain proportion of fillers, to prepare a self-adsorbing material, which is assembled with a filter membrane having a super-hydrophobic surface, and the contact angle between the hydrophobic region filter membrane surface of the obtained composite membrane material and water is greater than 160°, so that the droplets of the digestion solution or extraction solution based on water are anchored on the filter membrane inside the hydrophobic region, and the solution does not overflow during filtration, which can solve the problem in the prior art that the target separation is attached to the inner wall of the container, the external pressure causes uneven local filtration, and the microplastic detection result is low.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a composite membrane material for adsorbing and filtering microplastics comprises the following steps:
[0008] (1) A paper-based O-ring is adhered to the hydrophobic material a with an adhesive, dried at 80° C. for 5 min, a filler and a water-absorbent resin are mixed evenly, and spread flatly in the paper-based O-ring, and then covered with a circular water-soluble film material, and the water-soluble film material is heated along the O-ring with a heated metal rod to achieve sealing, and a limiting sponge pad is adhered to the high permeability material with an adhesive, and covered on the hydrophobic material a to obtain an adsorption base;
[0009] (2) The hydrophobic material b is heated and printed on both sides of the high permeability water material to form an O-ring hydrophobic modification pattern, and then dried to obtain a high permeability water material with a hydrophobic modification pattern; so that the droplets of the digestion solution or the extraction solution based on water are confined on the filter membrane inside the hydrophobic area, and the solution does not overflow during self-filtration;
[0010] (3) The adsorption base described in step (1) and the high permeability material with hydrophobic modified patterns described in step (2) are assembled together by a binder and dried to obtain a finished self-adsorption and filtration microplastic pretreatment composite membrane.
[0011] Further, the paper-based O-ring in step (1) comprises any one of glass fiber paper and qualitative filter paper, with an outer diameter of 42-50 mm, an inner diameter of 32-35 mm, and a thickness of 1.0-1.5 mm. It is used to limit and fix the water-absorbing resin and calcium carbonate, and cannot affect the expansion of the water-absorbing resin. Further preferably, any one of glass fiber O-ring (outer diameter 47 mm, inner diameter 33 mm, thickness 1.2 mm) and qualitative filter paper O-ring (outer diameter 48 mm, inner diameter 34 mm, thickness 1.0 mm).
[0012] Furthermore, the hydrophobic material a in step (1) includes any one of sulfuric acid paper, oil wax paper, paraffin paper, coated paper, and glassine paper.
[0013] Furthermore, the filler in step (1) includes any one of calcium carbonate, fumed silica, tricalcium phosphate or microcrystalline cellulose powder, and further preferably, the filler in step (1) is any one of calcium carbonate or tricalcium phosphate. The filler has a large specific surface area, excellent filling and anti-agglomeration properties, and helps to improve the gel blocking problem caused by insufficient cross-linking between hydrophilic resin particles, so that the hydrophilic resin particles can be evenly dispersed after absorbing water.
[0014] During the filtration process, the adsorption base is used to adsorb the digestion solution, and the hypertonic water material with hydrophobic modified patterns is used to intercept all solutes including microplastics in the solution to be filtered.
[0015] The present invention uses the combined effect of the adsorption base and the high permeability material with hydrophobic modified lines to trap microplastics in the hydrophilic area. On the one hand, it can reduce the observation range of subsequent instruments and effectively shorten the detection time; on the other hand, it can prevent the overflow of the digestion solution during filtration and reduce the loss of microplastic particles.
[0016] Furthermore, the water-absorbing resin includes but is not limited to at least one of sodium polyacrylate, polyacrylamide, acrylic acid, and acrylamide copolymer.
[0017] Furthermore, in step (1), the mass ratio of the filler to the water-absorbing resin is 0.10-0.20:0.50-1.00, and further preferably, the mass ratio of the filler to the water-absorbing resin is 0.10-0.16:0.50-0.80, and more preferably, the mass ratio of the filler to the water-absorbing resin is 0.12:0.60. 。
[0018] Furthermore, before covering the highly permeable water material in step (1), a water-soluble film material is first covered on the surface of the mixture, and the water-soluble film material includes any one of PVA water-soluble film, PVP water-soluble film, PVOH water-soluble film, and hydroxypropyl methylcellulose water-soluble film. The paper-based O-ring is used to seal the water-absorbent powder material, and can be dissolved in water in a short time without affecting the expansion of the water-absorbent resin. Further preferably, PVA water-soluble film (diameter 47mm, thickness 25μm).
[0019] Further, the hypertonic water material in step (1) includes any one of a paper towel, a hydrophilic non-woven fabric, a mixed cellulose membrane or a glass fiber filter membrane. Further preferably, the paper towel is selected from Qingfeng (120mm*91mm*2ply), a non-woven fabric (50 grams, 115mm*91mm), and the glass fiber filter membrane is selected from any one of whatman GF / A square glass fiber filter paper (1.6μm pore size, 115mm*90mm). The hypertonic water material is used to accelerate the permeation rate of the diversion filtration solution between the filter membrane with hydrophobic modified texture and the adsorption base. The hypertonic water material in step (2) includes any one of a mixed cellulose membrane or a glass fiber filter membrane. Further preferably, the glass fiber filter membrane is selected from any one of Whatman GF / A (1.6μm pore size, 25mm diameter), Whatman GF / B (1.0μm pore size, 25mm diameter), and Whatman GF / C (1.2μm pore size, 25mm diameter). The filtered membrane can be placed in instruments such as an optical microscope, Fourier transform infrared spectrometer, and micro-Raman tester for further qualitative or quantitative analysis of microplastics.
[0020] Furthermore, the hydrophobic material b in step (2) includes but is not limited to any one of paraffin wax and polydimethylsiloxane. The hydrophobic material is used to prepare a hydrophobic ring that inhibits overflow of the filtered solution.
[0021] Furthermore, the printing in step (2) is replaced by spraying or printing.
[0022] Furthermore, the printing refers to fixing the hydrophobic material on the pattern of the seal, and the seal includes a copper seal, and the printing surface of the copper seal is engraved with a pattern.
[0023] Furthermore, the drying temperature is 80-100° C., the drying time is 10-20 min, and the inner ring diameter of the limiting sponge pad is equal to or slightly smaller than the diameter of the high water permeability material in step (2).
[0024] Further, the limiting sponge pad (thickness 1.5mm-2.5mm, outer arc length 100mm-130mm, inner arc length 70mm-100mm, width 40mm-60mm, inner ring diameter 23mm-25mm), further preferably, the limiting sponge pad (thickness 2.0mm, outer arc length 110mm, inner arc length 90mm, width 50mm, inner ring diameter 24mm). The limiting sponge pad is used to fix the high permeability material with hydrophobic modified lines.
[0025] Furthermore, the drying equipment is an air drying oven or a vacuum drying oven.
[0026] Furthermore, the paper-based O-ring and the hydrophobic material a, the high-permeability material with hydrophobic modified patterns and the adsorption base are bonded together by an adhesive, and the adhesive includes but is not limited to any one of sodium carboxymethyl cellulose, polyvinyl pyrrolidone, hot melt adhesive or acrylic resin. Further preferably, the adhesive is 2% sodium carboxymethyl cellulose.
[0027] The present invention also provides a composite membrane material prepared according to the method, and application of the composite membrane material in the adsorption and filtration of microplastics in seafood digestion liquid.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The composite membrane material prepared by the present invention can effectively improve the shortcomings of slow filtration speed and long time consumption in traditional vacuum filtration, and has the characteristics of less time consumption, high recovery rate, and not easily affected by environmental factors.
[0030] 2) Using a seal heated at high temperature and coated with a hydrophobic material, the hydrophobic material a is applied to the surface of the high permeability material in a printing manner. The contact angle between the surface of the membrane material prepared by the present invention and water is greater than 160° as measured by a contact angle tester, which can effectively prevent the solution from overflowing. Take 0.5g of clam sample, add 5mL of 10% KOH solution, ultrasonicate for 10min, put it in a 50℃, 150r / min environment for 4h, and adjust the clarified digestion solution to neutrality with a 10% HCl solution. This solution can be processed by the lower layer of adsorption material in a self-filtration manner within 10-30min.
[0031] 3) The process of the present invention is simple, and can solve the problem in the prior art that microplastic particles adhere to the inner wall of the container, resulting in low measurement results. The composite membrane self-filtration technology provided by the present invention utilizes a uniform and effective capillary driving force to avoid operational errors caused by external negative pressure, has a high recovery rate, stable and reproducible results, is convenient for simultaneous operation of multiple samples, and can meet the needs of high-throughput and convenient sample pretreatment. It can also achieve efficient collection of full-size microplastics. The present invention does not require the use of chemical reagents, is safe and environmentally friendly, and provides a new method for the adsorption and filtration of microplastics in seafood digestion solutions. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The present invention is a process flow chart for preparing composite membrane materials.
[0033] Figure 2 The weighing paper with a glass fiber O-ring prepared in Example 1 of the present invention.
[0034] Figure 3 The water-absorbent powder prepared in Example 1 of the present invention is spread flat in a paper-based O-ring.
[0035] Figure 4 It is the water-absorbent powder in the PVA water-soluble film sealing paper-based O-ring prepared in Example 1 of the present invention.
[0036] Figure 5 It is the adsorption base prepared in Example 1 of the present invention.
[0037] Figure 6 It is the glass fiber filter membrane with hydrophobic modified patterns prepared in Example 1 of the present invention.
[0038] Figure 7 This is the self-adsorption and filtration microplastic pretreatment composite membrane prepared in Example 1 of the present invention (top view).
[0039] Figure 8 This is the self-adsorption and filtration microplastic pretreatment composite membrane prepared in Example 1 of the present invention (left view).
[0040] Fig. 9This is a comparison chart of the recovery rates of nine types of microplastics, including polypropylene (PP-500μm / PP-150μm), polystyrene (PS-500μm), polyethylene terephthalate (PET-500μm / PET-150μm), polyethylene low-density particles (LDPE-500μm), polyvinyl chloride (PVC-500μm), polyamide (PA-500μm), and acrylonitrile-butadiene-styrene copolymer (ABS-500μm), using the composite film material of Example 1 of the present invention.
[0041] Fig.10 This is a comparison chart of the recovery rates of nine types of microplastics, including polypropylene (PP-500μm / PP-150μm), polystyrene (PS-500μm), polyethylene terephthalate (PET-500μm / PET-150μm), polyethylene low-density particles (LDPE-500μm), polyvinyl chloride (PVC-500μm), polyamide (PA-500μm), and acrylonitrile-butadiene-styrene copolymer (ABS-500μm), using the composite film material of Example 2 of the present invention.
[0042] Fig.11 This is a comparison chart of the recovery rates of nine types of microplastics, including polypropylene (PP-500μm / PP-150μm), polystyrene (PS-500μm), polyethylene terephthalate (PET-500μm / PET-150μm), polyethylene low-density particles (LDPE-500μm), polyvinyl chloride (PVC-500μm), polyamide (PA-500μm), and acrylonitrile-butadiene-styrene copolymer (ABS-500μm), using the composite film material of Example 3 of the present invention. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0044] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the raw materials and auxiliary agents are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.
[0045] Example 1
[0046] A method for preparing a composite membrane material for adsorbing and filtering microplastics, the specific steps are as follows:
[0047] (1) Stick the glass fiber O-ring on the weighing paper with 2% sodium carboxymethyl cellulose and dry it at 80°C for 5 minutes. Add calcium carbonate to sodium polyacrylate with a mass ratio of 0.12:0.6 and stir until the mixture is evenly mixed to obtain a water-absorbing powder material, which is spread flat on the paper-based O-ring. Cover the circular PVA water-soluble film on the paper-based O-ring, and use a heated metal rod to heat the PVA water-soluble film along the O-ring to achieve sealing. Stick the limiting sponge pad on the Qingfeng paper towel (120mm*91mm*2ply) with an adhesive and cover it on the weighing paper to obtain an adsorption base;
[0048] (2) solid paraffin and a copper seal with hydrophobic modified patterns were heated to 170°C, and the obtained liquid paraffin was applied to the hydrophobic pattern of the copper seal with a tool, and then quickly printed on a glass fiber filter membrane (1.2 μm, Whatman GF / C). After maintaining for 20 seconds, the copper seal was removed, and the operation was repeated on the other side, followed by drying in a drying oven at 80°C for 10 minutes to obtain a glass fiber filter membrane with hydrophobic modified patterns;
[0049] (3) The adsorption base and the filter membrane with hydrophobic modified texture were adhered together using a 2% sodium carboxymethyl cellulose solution, and then dried in a drying oven at 80°C for 10 minutes to obtain a self-adsorption and filtration microplastic pretreatment composite membrane.
[0050] Recovery test:
[0051] Weigh 30 particles each of polypropylene (PP-500μm / PP-150μm), polystyrene (PS-500μm), polyethylene terephthalate (PET-500μm / PET-150μm), polyethylene low-density particles (LDPE-500μm), polyvinyl chloride (PVC-500μm), polyamide (PA-500μm), and acrylonitrile-butadiene-styrene copolymer (ABS-500μm), and add them to seafood. Digest them with 10% KOH solution, and drain the neutralized digestion solution through a glass rod onto the self-adsorption filtration microplastic pretreatment composite membrane. Use an optical microscope (10×~40×) to magnify and observe the particles in the intercepted hydrophilic area and count them, and calculate the recovery rate of the standard microplastic sample.
[0052] The experimental results show that the average recovery rate of spiked samples is (93.9±3.27)%, and the recovery rate of single type microplastics is between 90.00% and 96.67%. Figure 8 shown.
[0053] Example 2
[0054] A method for preparing a composite membrane material for adsorbing and filtering microplastics, the specific steps are as follows:
[0055] (1) Stick the glass fiber O-ring on the weighing paper with 2% sodium carboxymethyl cellulose and dry it at 80°C for 5 minutes. Add calcium carbonate to sodium polyacrylate with a mass ratio of 0.2:1.0 and stir until the mixture is uniform to obtain a water-absorbing powder material, which is spread flat on the paper-based O-ring. Cover the circular PVA water-soluble film on the paper-based O-ring, and use a heated metal rod to heat the PVA water-soluble film along the O-ring to achieve sealing. Stick the limiting sponge pad on the Qingfeng paper towel (120mm*91mm*2ply) with an adhesive and cover it on the weighing paper to obtain an adsorption base;
[0056] (2) solid paraffin and a copper seal with hydrophobic modified patterns were heated to 170°C, and the obtained liquid paraffin was applied to the hydrophobic pattern of the copper seal with a tool, and then quickly printed on a glass fiber filter membrane (1.2 μm, Whatman GF / C). After maintaining for 20 seconds, the copper seal was removed, and the operation was repeated on the other side, followed by drying in a drying oven at 80°C for 10 minutes to obtain a glass fiber filter membrane with hydrophobic modified patterns;
[0057] (3) The adsorption base and the filter membrane with hydrophobic modified texture were adhered together using a 2% sodium carboxymethyl cellulose solution, and then dried in a drying oven at 80°C for 10 minutes to obtain a self-adsorption and filtration microplastic pretreatment composite membrane.
[0058] Recovery test:
[0059] Weigh 30 particles each of polypropylene (PP-500μm / PP-150μm), polystyrene (PS-500μm), polyethylene terephthalate (PET-500μm / PET-150μm), polyethylene low-density particles (LDPE-500μm), polyvinyl chloride (PVC-500μm), polyamide (PA-500μm), and acrylonitrile-butadiene-styrene copolymer (ABS-500μm), and add them to seafood. Digest them with 10% KOH solution, and drain the neutralized digestion solution through a glass rod onto the self-adsorption filtration microplastic pretreatment composite membrane. Use an optical microscope (10×~40×) to magnify and observe the particles in the intercepted hydrophilic area and count them, and calculate the recovery rate of the standard microplastic sample.
[0060] The experimental results show that the average recovery rate of spiked samples is (95.6±4.05)%, and the recovery rate of single type microplastics is between 88.33% and 96.67%. Fig.10 shown.
[0061] Example 3
[0062] A method for preparing a composite membrane material for adsorbing and filtering microplastics, the specific steps are as follows:
[0063] (1) Stick the glass fiber O-ring on the weighing paper with 2% sodium carboxymethyl cellulose and dry it at 80°C for 5 minutes. Add tricalcium phosphate to sodium polyacrylate with a mass ratio of tricalcium phosphate to sodium polyacrylate of 0.12:0.6 and stir until the mixture is uniform to obtain a water-absorbing powder material, which is spread flat on the paper-based O-ring. Cover the circular PVA water-soluble film on the paper-based O-ring, and use a heated metal rod to heat the PVA water-soluble film along the O-ring to achieve sealing. Stick the limiting sponge pad on the Qingfeng paper towel (120mm*91mm*2ply) with an adhesive and cover it on the weighing paper to obtain an adsorption base;
[0064] (2) solid paraffin and a copper seal with hydrophobic modified patterns were heated to 170°C, and the obtained liquid paraffin was applied to the hydrophobic pattern of the copper seal with a tool, and then quickly printed on a glass fiber filter membrane (1.2 μm, Whatman GF / C). After maintaining for 20 seconds, the copper seal was removed, and the operation was repeated on the other side, followed by drying in a drying oven at 80°C for 10 minutes to obtain a glass fiber filter membrane with hydrophobic modified patterns;
[0065] (3) The adsorption base and the filter membrane with hydrophobic modified texture were adhered together using a 2% sodium carboxymethyl cellulose solution, and then dried in a drying oven at 80°C for 10 minutes to obtain a self-adsorption and filtration microplastic pretreatment composite membrane.
[0066] Recovery test:
[0067] Weigh 30 particles each of polypropylene (PP-500μm / PP-150μm), polystyrene (PS-500μm), polyethylene terephthalate (PET-500μm / PET-150μm), polyethylene low-density particles (LDPE-500μm), polyvinyl chloride (PVC-500μm), polyamide (PA-500μm), and acrylonitrile-butadiene-styrene copolymer (ABS-500μm), and add them to seafood. Digest them with 10% KOH solution, and drain the neutralized digestion solution through a glass rod onto the self-adsorption filtration microplastic pretreatment composite membrane. Use an optical microscope (10×~40×) to magnify and observe the particles in the intercepted hydrophilic area and count them, and calculate the recovery rate of the standard microplastic sample.
[0068] The experimental results show that the average recovery rate of spiked samples is (93.3±2.62)%, and the recovery rate of single type microplastics is between 88.33% and 98.33%. Fig.11 shown.
[0069] Comparative Example 1
[0070] Christina J. Thiele et al. added 30 particles of 9 different sizes of microplastics (PS, PP, PET, PA, PVC, LDPE, acrylonitrile, particle size <600μm) to seafood, digested them with 10% KOH solution, and the neutralized digestion solution was vacuum filtered through a glass fiber (1.2μm, WhatmanGF / C) filter membrane and dried, and then magnified and observed under an optical microscope (10×~60×) and counted.
[0071] The experimental results show that the average recovery rate of spiked samples is (86.2±7.9)%, and the recovery rate of a single type of microplastics is between 77.5% and 91.6%.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a composite membrane material for adsorbing and filtering microplastics, characterized in that: The following steps are involved: (1) A paper-based O-ring is adhered to the hydrophobic material a with an adhesive, dried at 80° C. for 5 min, a filler and a water-absorbent resin are mixed evenly, and spread flatly in the paper-based O-ring, and then covered with a circular water-soluble film material, and the water-soluble film material is heated along the O-ring with a heated metal rod to achieve sealing, and a limiting sponge pad is adhered to the high permeability material with an adhesive, and covered on the hydrophobic material a to obtain an adsorption base; (2) heating and printing the hydrophobic material b on both sides of the high water permeability material to form an O-ring hydrophobic modification pattern, and drying the pattern to obtain a high water permeability material with hydrophobic modification patterns; (3) The adsorption base described in step (1) and the high permeability material with hydrophobic modified patterns described in step (2) are assembled together by a binder and dried to obtain a finished self-adsorption and filtration microplastic pretreatment composite membrane.
2. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The paper-based O-ring in step (1) comprises any one of glass fiber paper and qualitative filter paper.
3. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The hydrophobic material a in step (1) comprises any one of sulfuric acid paper, oil wax paper, paraffin paper, coated paper, and glassine paper.
4. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The filler in step (1) comprises any one of calcium carbonate, fumed silica, tricalcium phosphate or microcrystalline cellulose, the water-absorbing resin comprises at least one of sodium polyacrylate, polyacrylamide, acrylic acid, and acrylamide copolymer, and the mass ratio of the filler to the water-absorbing resin is 0.10-0.20:0.50-1.
00.
5. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The water-soluble membrane material in step (1) includes any one of PVA water-soluble membrane, PVP water-soluble membrane, PVOH water-soluble membrane, and hydroxypropyl methylcellulose water-soluble membrane. The high permeability water material in step (1) includes any one of paper towel, hydrophilic non-woven fabric, mixed cellulose membrane or glass fiber filter membrane.
6. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The high water permeability material in step (2) includes any one of a mixed cellulose membrane or a glass fiber filter membrane, and the hydrophobic material b in step (2) includes any one of paraffin and polydimethylsiloxane.
7. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The printing in step (2) is replaced by spraying or printing.
8. The method for preparing a composite membrane material for adsorbing and filtering microplastics according to claim 1, characterized in that: The drying temperature is 80-100° C., the drying time is 10-20 min, the binder used is 2% sodium carboxymethyl cellulose solution, and the inner ring diameter of the limiting sponge pad is equal to or slightly smaller than the diameter of the high permeability material in step (2).
9. The composite membrane material prepared according to the method according to any one of claims 1 to 8.
10. Use of the composite membrane material prepared by the method according to any one of claims 1 to 8, or the composite membrane material according to claim 9 in the adsorption and filtration of microplastics in seafood digestion liquid.