Ultrafine polyimide nanofiber membrane prepared at high voltage and application thereof in high-temperature filtration
The preparation of polyimide nanofiber membranes through metal wire needle-free electrospinning process solved the problems of low filtration efficiency of polyimide in PM0.3 and complex electrospinning process, achieving high-efficiency and stable high-temperature filtration performance and low resistance.
Patent Information
- Application Number
- CN202411388551.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-30
AI Technical Summary
Polyimide materials are still poor in filtration efficiency of PM0.3, and the electrospinning time is long and complex in traditional electrospinning technology, which affects the economical and scalability of the industrial application of materials.
The metal wire needleless electrospinning process is adopted to increase the voltage range from 60kV to 80kV, and a thinner nanofiber membrane is prepared, which simplifies the electrospinning process and improves the filtration performance.
The PM0.3 filtration efficiency of 99.98% was achieved under high temperature conditions and the filtration efficiency of 99.95% was maintained, demonstrating excellent stability and hydrophobic properties, reducing filtration resistance.
Smart Images

Figure CN119075714A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of separation membranes, in particular to high-voltage preparation of ultrafine polyimide nanofiber membranes and high-temperature filtration applications thereof. Background Art
[0002] The emission of fine particulate matter (PM2.5-0.3) caused by industrialization and urbanization has become an urgent environmental problem. PM2.5-0.3 mainly comes from the burning of fossil fuels, biomass and garbage, which are common in industry, transportation, agriculture and home heating. PM has a complex composition, including inorganic substances such as silicates, sulfates, nitrates, and organic substances such as organic carbon and elemental carbon, and may carry up to 791 bacterial genera, increasing the risk of allergies and infections. The negative charge characteristics of PM affect its behavior in the atmosphere.
[0003] PM poses a serious threat to human health. Due to its small size, PM2.5 is easier to enter the human body and cause more serious diseases such as asthma, cardiovascular disease and lung inflammation. Studies have shown that PM2.5 concentrations exceeding 200μg / m 3 PM0.3, due to its smaller particle size, may cause cardiovascular disease, respiratory disease, diabetes, and lung cancer.
[0004] Industrial dust collectors are effective against large particles, but not against particles smaller than 2.5μm. Electrostatic precipitators are expensive, and their removal efficiency is affected by PM characteristics. Nanofiber filters have higher filtration efficiency and lower pressure drop than general ultrafine fiber filters due to the "slip effect" that reduces resistance to airflow, and show potential in the removal of particles smaller than 2.5μm. Polyimide (PI) exhibits excellent mechanical properties due to its rigid segments, strong intermolecular interactions, and high binding energy. Its highly conjugated and highly aromatic structure gives PI good thermal stability, and its high dipole moment (6.2D) enhances its adsorption capacity for particulate matter, making PI the preferred high-performance material in the field of air filtration.
[0005] In the article "High Temperature Resistant Polyimide / Polyethersulfone Nano-Fibers Membrane for Removal of PM", the PI / PES nanofiber membrane developed by Wei-Ting Chen and Yi-Hung Lai achieved a PM2.5 filtration efficiency of 99.54% within 20 minutes of spinning time, a pressure drop of 92 Pa, and significant thermal stability of about 500°C. In the article "Electrospun Polyimide / Metal-Organic Framework Nanofibrous Membrane with Superior Thermal Stability for Efficient PM2.5 Capture", the PI-ZIF nanofiber membrane prepared by Zhimin Hao's team combining PI and metal organic framework (ZIF-8) achieved a PM2.5 filtration efficiency of 96.6% ± 2.9% at 300°C, showing good thermal stability and low pressure drop.
[0006] Although polyimide has made significant progress in PM2.5 filtration, there is still room for improvement in PM0.3 filtration efficiency. In addition, the electrospinning time of electrospun PI nanofiber membranes in traditional electrospinning technology usually ranges from 10kV to 40kV, and the electrospinning time often exceeds 60min. The complexity of the preparation process also affects the economy and scalability of the material in industrial applications. Summary of the invention
[0007] The purpose of the present invention is to provide a high-voltage preparation of ultrafine polyimide nanofiber membranes and their high-temperature filtration applications, in order to solve the problem that the above-mentioned polyimide materials are still poor in PM0.3 filtration efficiency and the preparation process is relatively complicated. The present invention adopts a metal wire needleless electrospinning process to electrospin PI nanofiber membranes. Compared with the needle-type electrospinning process, the needleless electrospinning scheme avoids the problems of needle clogging and wear. The present invention uses a voltage of 60kV to 80kV to enhance the droplet splitting ability and generate nanofibers with finer diameters, thereby improving the filtration performance for high-temperature filtration. Compared with composite materials, the present invention prepares fine-diameter nanofiber membranes by adjusting the electrospinning voltage to improve the filtration performance of PI nanofiber membranes, which is more convenient. With the support of the metal wire needleless electrospinning process, the fine-diameter PI nanofiber membrane can be electrospun in 8 to 12 minutes to obtain a high-efficiency filtration membrane.
[0008] To achieve the above object, the present invention provides a method for preparing an ultrafine polyimide nanofiber membrane in a first aspect, comprising the following steps:
[0009] (1) Preparation of polyamic acid solution
[0010] Dissolving 4,4'-diaminodiphenyl ether in N,N-dimethylacetamide, and obtaining a transparent 4,4'-diaminodiphenyl ether / N,N-dimethylacetamide solution after 4,4'-diaminodiphenyl ether (ODA) is completely dissolved; adding pyromellitic acid anhydride monomer to the 4,4'-diaminodiphenyl ether / N,N-dimethylacetamide solution in multiple portions, stirring to allow 4,4'-diaminodiphenyl ether and pyromellitic acid anhydride monomer to fully react, and standing to obtain a polyamic acid solution;
[0011] (2) electrospinning polyamic acid solution using a metal wire needle-free process;
[0012] (3) After the electrospinning is completed, the PAA nanofiber membrane is obtained by drying, and then thermal imidization is performed to obtain a polyimide nanofiber membrane.
[0013] Preferably, the solution preparation process in step (1) is carried out under nitrogen protection conditions at 0-5°C.
[0014] Preferably, the 4,4'-diaminodiphenyl ether (ODA), N,N-dimethylacetamide (DMAc), and pyromellitic dianhydride (PMDA) monomers in step (1) are vacuum dried at 120°C for 1 to 5 hours to remove residual solvent and moisture.
[0015] In the present invention, PAA is polyamic acid, SE is an electrospinning electrode, CE is a collecting electrode, PMDA is pyromellitic dianhydride, ODA is 4,4'-diaminodiphenyl ether, and DMAC is N,N-dimethylacetamide.
[0016] Preferably, in step (1), the molar ratio of ODA to PMDA is 1:1 to 1.02.
[0017] Preferably, the concentration of the PAA solution in step (1) is 15-20 wt %.
[0018] More preferably, the concentration of the PAA solution in step (1) is 16 to 18 wt %.
[0019] Preferably, in the metal wire needle-free electrospinning process in step (2), the voltage is 60-80 kV, the distance from the electrospinning electrode to the carrier is 240 mm, and the distance from the collecting electrode to the carrier is 20 mm; the operating distance of the transfer vehicle is 350 mm, the cycle time is 6 s, and the electrospinning time is 8-12 min; the spinning temperature is 15° C. to 25° C., and the humidity is 30% to 50%.
[0020] Preferably, the drying temperature in step (3) is 100-120° C. and the drying time is 8-15 hours.
[0021] Preferably, the specific steps of thermal imidization in step (3) are:
[0022] The dried PAA nanofiber membrane was placed in a muffle furnace and heated at a rate of 1 to 2°C / min under air conditions from room temperature to 350 to 400°C, and kept at 100°C, 200°C, 300°C, and 350°C for 1 hour, and then naturally cooled to room temperature to obtain a polyimide nanofiber membrane.
[0023] The second aspect of the present invention provides an ultrafine polyimide nanofiber membrane, which is prepared by the above-mentioned preparation method.
[0024] Preferably, the average fiber diameter of the polyimide nanofiber membrane is 100-400 nm.
[0025] The third aspect of the present invention provides an application of an ultrafine polyimide nanofiber membrane, specifically an application of the polyimide nanofiber membrane in filtering high-temperature fine particles.
[0026] Preferably, the particle size of the fine particles is 0.3 μm.
[0027] Therefore, the present invention adopts the above-mentioned high voltage to prepare ultrafine polyimide nanofiber membrane and its high temperature filtration application, which has the following beneficial effects:
[0028] (1) The present invention adopts metal wire needle-free electrospinning technology to electrospin polyimide (PI) material, and prepares a nanofiber membrane with an average fiber diameter of 122 nm under a high electrospinning voltage of 80 kV for 10 minutes.
[0029] (2) The fine-diameter PI nanofiber membrane prepared by the present invention has a filtration efficiency of 99.98% for PM0.3, while operating at a low resistance of 189.18 Pa. After continuous treatment at a high temperature of 390°C for one hour, the filtration efficiency of the fine-diameter PI nanofiber membrane for PM0.3 remains above 99.95%, and it is able to achieve complete filtration of PM2.5. This proves that the fine-diameter PI nanofiber membrane has excellent stability and reliability under extreme temperature conditions.
[0030] (3) The membrane prepared in the present invention also exhibits excellent hydrophobic properties, with a static hydrophobic angle measurement of 130±3°, which helps to maintain its filtration performance in a humid environment.
[0031] (4) The fine-diameter PI nanofiber membrane studied in this invention provides a new preparation strategy for PM filtration in high-temperature environments and provides new insights into its ultimate performance.
[0032] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] FIG. 1( a ) is a flow chart of the preparation process of the polyimide nanofiber membrane of the present invention;
[0034] FIG1( b ) is a schematic diagram of the spinning process of the polyimide nanofiber membrane of the present invention;
[0035] Figure 2 The characterization results of Examples 1-5, wherein (a) is a Fourier transform infrared spectrometer (FTIR) image of PAA and PI, (b) is a tensile tension-strain curve graph, (c) is a comparison of the appearance before and after bending, and (d) is a schematic diagram of the slip flow effect;
[0036] Figure 3 Scanning electron microscope (SEM) images and diameter distribution statistical graphs of the polyimide nanofiber membranes prepared in Examples 1-3 and Example 6, wherein (a) and (b) are SEM images of PI15-80-10, (c) is a SEM image of PI16-80-10, (d) is a diameter distribution statistical graph of PI16-80-10, (e) is a SEM image of PI17-80-10, (f) is a diameter distribution statistical graph of PI17-80-10, (g) is a SEM image of PI18-80-10, and (h) is a diameter distribution statistical graph of PI18-80-10;
[0037] Figure 4 The filtration performance of Examples 1-3 and Examples 7-10, wherein (a) is a graph showing the filtration efficiency of the PI nanofiber membranes prepared in Examples 1-3 and Examples 7-10 for PM0.3, (b) is a graph showing the filtration efficiency of the PI nanofiber membranes prepared in Examples 1-3 and Examples 7-10 for PM0.5-2.5, (c) is a graph showing the filtration efficiency of Example 1 and commercial glass fiber for PM0.3, and (d) is a graph showing the filtration efficiency of Example 1 and commercial glass fiber for PM0.5-2.5;
[0038] Figure 5 The high temperature resistance, filtration performance and hydrophobic performance of Example 1, Examples 3-5 and Examples 11-14, wherein (a) is a thermogravimetric analysis (TG) graph, a differential thermogravimetric analysis (DTG) curve and a differential scanning calorimetry (DSC) curve of the fine-diameter PI nanofiber membrane of Example 3, (b) is a PM0.3 filtration efficiency graph of the fine-diameter PI nanofiber membrane of Example 3 and commercial glass fiber after treatment at different temperatures, (c) is a PM0.5-2.5 filtration efficiency graph of the fine-diameter PI nanofiber membrane of Examples 1, 4-5 and 11-14, and (d) is a comparison graph of the water contact angles of the fine-diameter PI nanofiber membrane and commercial glass fiber after treatment at different temperatures;
[0039] Figure 6SEM images and statistical distribution diagrams of fiber diameters of PI nanofiber membranes prepared in Example 1 and Example 4-5, wherein (a) is the SEM image of PI350, (b) is the statistical diagram of the diameter distribution of PI350, (c) is the SEM image of P380, (d) is the statistical diagram of the diameter distribution of P380, (e) is the SEM image of P400, and (f) is the statistical diagram of the diameter distribution of P400. DETAILED DESCRIPTION
[0040] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.
[0041] Example 1
[0042] As shown in FIG. 1( a ) and FIG. 1( b ), a method for preparing an ultrafine polyimide nanofiber membrane comprises the following steps:
[0043] (1) Preparation of PAA solution
[0044] The ODA, DMAc, and PMDA monomers were dried under vacuum at 120 °C for 1 to 5 h to remove residual solvent and water;
[0045] Under nitrogen protection, ODA was dissolved in DMAc, with a molar ratio of ODA to PMDA of 1:1. After ODA was completely dissolved, a transparent ODA / DMAc solution was obtained.
[0046] At 2°C, PMDA monomer was added to the ODA / DMAc solution three times, each time with an interval of 30 minutes, and stirred to allow the ODA and PMDA monomers to react fully, and then allowed to stand to obtain a PAA solution; the concentration of the PAA solution was 18wt%;
[0047] (2) Electrospinning of PAA solution
[0048] Electrospinning parameters: voltage 80 kV, distance from SE to carrier 240 mm, distance from CE to carrier 20 mm; spinning carriage running distance 350 mm, cycle time 6 s, electrospinning time 10 min; spinning temperature 20 ° C, humidity 40%;
[0049] (3) After the electrospinning is completed, it is dried at 120°C for 12 h to obtain a PAA precursor. The dried PAA precursor is placed in a muffle furnace and heated at a rate of 1.66°C / min under air conditions from room temperature to 350°C. It is kept at 100°C, 200°C, 300°C, and 350°C for 1 h, and then naturally cooled to room temperature. The PAA precursor is thermally imidized to form a PI nanofiber membrane. The obtained polyimide nanofiber membrane is recorded as PI18-80-10 or PI350.
[0050] Example 2
[0051] The difference between this embodiment and embodiment 1 is that the concentration of the PAA solution is different. In this embodiment, the concentration of the PAA solution is 17 wt %, and the obtained polyimide nanofiber membrane is recorded as PI17-80-10.
[0052] Example 3
[0053] The difference between this embodiment and embodiment 1 is that the concentration of the PAA solution is different. In this embodiment, the concentration of the PAA solution is 16 wt %, and the obtained polyimide nanofiber membrane is recorded as PI16-80-10.
[0054] Example 4
[0055] The difference between this embodiment and embodiment 1 is that the temperature of thermal imidization is different. In this embodiment, the temperature of the muffle furnace is raised from room temperature to 380° C., and the obtained polyimide nanofiber membrane is recorded as PI380.
[0056] Example 5
[0057] The difference between this embodiment and embodiment 1 is that the temperature of thermal imidization is different. In this embodiment, the temperature of the muffle furnace is raised from room temperature to 400° C., and the obtained polyimide nanofiber membrane is recorded as PI400.
[0058] Example 6
[0059] The difference between this embodiment and embodiment 1 is that the concentration of the PAA solution is different. In this embodiment, the concentration of the PAA solution is 15 wt %, and the obtained polyimide nanofiber membrane is recorded as PI15-80-10.
[0060] Example 7
[0061] The difference between this embodiment and embodiment 3 is that the electrospinning time is different. The electrospinning time of this embodiment is 12 minutes, and the obtained polyimide nanofiber membrane is recorded as PI16-80-12.
[0062] Example 8
[0063] The difference between this embodiment and embodiment 3 is that the electrospinning time is different. The electrospinning time of this embodiment is 8 minutes, and the obtained polyimide nanofiber membrane is recorded as PI16-80-8.
[0064] Example 9
[0065] The difference between this embodiment and embodiment 3 is that the electrospinning voltage is different. The electrospinning voltage of this embodiment is 70 kV, and the obtained polyimide nanofiber membrane is recorded as PI16-70-10.
[0066] Example 10
[0067] The difference between this embodiment and embodiment 3 is that the electrospinning voltage is different. The electrospinning voltage of this embodiment is 60 kV, and the obtained polyimide nanofiber membrane is recorded as PI16-60-10.
[0068] Embodiment 11
[0069] The difference between this embodiment and embodiment 1 is that the temperature of thermal imidization is different. In this embodiment, the temperature of the muffle furnace is raised from room temperature to 360° C., and the obtained polyimide nanofiber membrane is recorded as PI360.
[0070] Example 12
[0071] The difference between this embodiment and embodiment 1 is that the temperature of thermal imidization is different. In this embodiment, the temperature of the muffle furnace is raised from room temperature to 370° C., and the obtained polyimide nanofiber membrane is recorded as PI370.
[0072] Example 13
[0073] The difference between this embodiment and embodiment 1 is that the temperature of thermal imidization is different. In this embodiment, the temperature of the muffle furnace is raised from room temperature to 390° C., and the obtained polyimide nanofiber membrane is recorded as PI390.
[0074] Embodiment 14
[0075] The difference between this embodiment and embodiment 1 is that the temperature of thermal imidization is different. In this embodiment, the temperature of the muffle furnace is raised from room temperature to 410° C., and the obtained polyimide nanofiber membrane is recorded as PI410.
[0076] Test example
[0077] (1) The polyimide nanofiber membranes prepared in Examples 1-5 were characterized by FTIR and SEM.
[0078] The molecular structure of the synthesized material was characterized using the Thermo Fisher Scientific Nicolet iS20 Fourier transform infrared spectrometer from the United States. Fourier transform infrared spectroscopy (FTIR) is used to identify the functional groups and chemical bonds present in the material and determine whether the target nanofiber membrane has been obtained.
[0079] The chemical composition of PAA nanofibers and their thermal imidization PI nanofiber membranes was analyzed in detail by FTIR. Figure 2 As shown in (a), the characteristic absorption peak of PAA is located at 1718.95 cm -1 (Asymmetric stretching vibration of C=O in COOH), 1649.49 cm -1 (C=O symmetric stretching vibration in CONH), 1497.62 cm -1 (benzene ring skeleton stretching vibration) and 1233.38cm -1 (CO-NH symmetric stretching vibration), which is consistent with the PAA structure. After thermal imidization, the characteristic absorption peak of PI appears at 1717.18 cm -1 (asymmetric stretching vibration of C=O on the imide ring), 1775.13 cm -1 (symmetric stretching vibration of C=O) and 1374.76 cm -1 (stretching vibration of CNC on the imide ring), and 1242.36 cm -1 (ether bond vibration) and 722.08cm -1 (-C=O bending vibration in the imide ring). In addition, 2600cm -1 Up to 3500cm -1 The absorption peaks at are attributed to -COOH and -NH- of PAA, which disappeared in the FTIR spectrum of PI, indicating that PAA was completely converted into PI after thermal imidization.
[0080] The morphology of the samples was examined using a Czech TESCAN MIRA LMS scanning electron microscope (SEM). Before SEM imaging, the samples were sputtered with platinum for 45 seconds (current 10 mA) using an Oxford Quorum SC7620 sputter coater to enhance the resolution and contrast of the image. SEM analysis provides a detailed view of the sample surface morphology and microstructure.
[0081] The surface morphology of the nanofiber membranes prepared from PAA solutions with different concentrations was analyzed by scanning electron microscopy (SEM). Figure 3 As shown in (c), (e) and (g), when the PAA solution concentration is 16wt.% to 18wt.%, the surface of the obtained fine diameter PI nanofiber membrane is very smooth and no beaded fibers are observed, which indicates that the optimization of electrospinning process parameters is helpful to obtain uniform fiber morphology. Figure 3(a) and (b) showed spindle-like structures and bonding on the fiber surface, which was due to the unstable fiber formation caused by the low solution concentration. Further statistical analysis quantified the SEM images and the results showed that the average diameter of the nanofibers increased with the increase of PAA solution concentration. Figure 3 As shown in (d), (f) and (h), the diameter distribution of the nanofibers is an inverse Gaussian distribution, and the average diameters of the PI16-80-10, PI17-80-10 and PI18-80-10 nanofibers are 139.28 nm, 150.90 nm and 174.27 nm, respectively. The membrane obtained by the present invention exhibits a finer fiber diameter, which has a positive effect on improving the filtration performance.
[0082] The surface morphology of the thin-diameter PI nanofiber membranes treated at different temperatures was analyzed by SEM. Figure 6 (a), (c) and (e) show that even after further treatment at high temperature, the fiber surface remains smooth without any structural damage caused by bending or curling. Further statistical analysis shows that the average diameter of the nanofibers increases with the increase of treatment temperature. Specifically, Figure 6 As shown in (b), (d) and (f), the average diameters of PI350, PI380 and PI400 nanofibers are 139.28 nm, 151.41 nm and 165.65 nm, respectively, and their diameter distributions all show anti-Gaussian characteristics.
[0083] (2) The thin-diameter PI nanofiber membrane samples were cut into uniform sizes, i.e. rectangular specimens with a length of 30 mm and a width of 10 mm. This standardized sample size helps ensure the consistency and comparability of the test results. Subsequently, a tensile test was performed on an INSTRON 8872 testing machine. During the test, the sample was uniformly stretched at a strain rate of 2 mm / min until it broke.
[0084] like Figure 2 As shown in (b), with the increase of PAA concentration from 16wt.% to 18wt.%, the tensile strength of the thin-diameter PI nanofiber membrane increased significantly. Specifically, the PI18-80-10 sample showed the highest tensile strength, reaching 8.893MPa, which was 28.53% higher than the 6.355MPa of the PI16-80-10 sample. This result shows that increasing the PAA concentration is an effective way to improve the mechanical strength of the PI nanofiber membrane. Further analysis shows that Figure 3As shown in (c), (e) and (g), as the concentration of PAA increases, the amount of filaments produced during the electrospinning process increases, resulting in an increase in the thickness of the nanofiber membrane produced within the same electrospinning time. In addition, the increase in PAA concentration also leads to a decrease in the diameter of the nanofibers, which affects the tensile strength of the fine-diameter PI nanofiber membrane. The tensile strength of the fine-diameter PI nanofiber membrane obtained by the present invention is 5 to 8 MPa.
[0085] In addition, the Knudsen number (K n ) can be calculated by the following formula:
[0086] Kn=2λ / d f
[0087] where λ and d f are the mean free path of air molecules (λ=65.3nm) and the fiber diameter, respectively.
[0088] The corresponding K values of PI16-80-10, PI17-80-10, and PI18-80-10 nanofiber membranes n The values are 0.937, 0.865, and 0.749, respectively. The airflow around the thin-diameter PI nanofibers belongs to the transitional flow region. Figure 2 (d) According to the principle of slip flow phenomenon, when the fiber diameter is close to 65.3 nm, the airflow velocity on the surface of a single fiber is not zero. Therefore, the resistance of the airflow can be significantly reduced, and it is reasonable to assume that the thin-diameter PI nanofiber membrane exhibits the characteristics of the lip effect, especially for PI16-80-10.
[0089] The calculated K n The airflow characteristics of PI16-80-10, PI17-80-10, and PI18-80-10 nanofiber membranes were evaluated. n The values are 0.937, 0.865, and 0.749, respectively, indicating that the airflow around the thin-diameter PI nanofibers is in the transitional flow region. Based on the principle of slip flow phenomenon, it is expected that the airflow velocity on the surface of a single fiber will not tend to zero when the fiber diameter is close to the mean free path of air molecules.
[0090] from Figure 2 From the perspective of mechanical properties shown in (b), the increase in ambient temperature is accompanied by an increase in the diameter of the nanofibers, where the tensile strength of PI400 reaches 7.721MPa, which is 21.49% higher than 6.355MPa of PI16-80-10. However, the elongation at break of PI400 decreases from 25.60% of PI16-80-10 to 19.02%, a decrease of 25%. The appearance comparison before and after bending is shown in Figure 2 (c).
[0091] (3) The thermal properties of the material, including stability and phase change, were determined using a German Netzsch STA449F3 Jupiter synchronous thermal analyzer. The sample was heated from 30°C to 800°C under a nitrogen atmosphere at a heating rate of 20°C / min without insulation. This method allows the thermal degradation behavior of the material to be evaluated and any phase changes that occur during heating to be identified.
[0092] When discussing the basic issues of particulate matter filtration in high temperature environments, thermal stability is one of the key factors. Figure 5 As shown in (a), the fine-diameter PI nanofiber membrane was characterized by thermogravimetric analysis (TGA), and the results revealed that the mass of the membrane changed slightly in the temperature range of 30 to 180°C, which was attributed to the removal of residual organic solvents. When the temperature rose to 553.40°C, a significant mass loss occurred, which was due to the self-crosslinking, cyclization and dehydrogenation reactions of the membrane. The differential thermogravimetric analysis (DTG) curve showed that the main weight loss temperature of the fine-diameter PI nanofiber membrane was 610°C, which was mainly caused by the oxidation of the continuously released carbon and carbon monoxide. Therefore, the fine-diameter PI nanofiber membrane exhibited good thermal stability below 550°C. The differential scanning calorimetry (DSC) curve did not have a clear peak between 300°C and 500°C, further confirming the excellent thermal stability of the fine-diameter PI nanofiber membrane. However, as a filter material, its ability to maintain filtration efficiency and avoid failure at high temperatures is more practical.
[0093] (4) The temperature resistance filtration test was conducted using a KJ-T1200-S6010-wQ vacuum tube furnace from Zhengzhou Kejia Electric Furnace Co., Ltd. To simulate real high temperature conditions, the sample was heated to 410°C in air at a rate of 10°C / min, and isothermally kept at 10°C for 1 h in the range of 350°C to 400°C. The filtration efficiency and resistance were then measured at different temperatures from 350°C to 410°C.
[0094] The filtration performance of the membrane was evaluated on the LZC-K1 filter material comprehensive performance test bench of Huada Instrument Equipment Co., Ltd. in Suzhou, Jiangsu, China. The membrane was placed in a circular fixture with a diameter of 11 cm, and its filtration efficiency and resistance were measured by adjusting the flow rate at different wind speeds. The filtration efficiency of the filter was calculated by the following formula:
[0095]
[0096] Where, η is the filtration efficiency; C down , C up are the particle number concentrations downstream and upstream of the filter, respectively.
[0097] When analyzing the filtration performance of the fine-diameter PI nanofiber membrane, the filtration efficiency of PM0.3 is mainly analyzed. Figure 4 (a) and Figure 4 As shown in (b), the PI16-80-10 sample showed significant superiority. The filtration efficiency of PI16-80-10 reached 99.98753%, compared with 99.989% of PI18-80-10 sample and 99.97466% of PI17-80-10 sample. All three were greater than 99.95%, achieving efficient filtration of PM0.3, and the filtration efficiency of PM2.5 could achieve complete filtration. However, PI16-80-10 has an advantage in resistance. In terms of filtration resistance, the resistance of PI16-80-10 sample was 189.18Pa, compared with 348.86667Pa of PI18-80-10 sample and 238.74Pa of PI17-80-10 sample, the filtration resistance of PI16-80-10 sample was the smallest. The PI15-80-10 sample was also tested. Due to the spindle-like structure of PI15-80-10 and the large amount of fiber bonding and flaky covering on the surface, its filtration efficiency reached 99.99%, and the filtration resistance was extremely high, reaching 500Pa+. Due to the testing instrument, the upper limit of the test was 500Pa.
[0098] Further comparison of samples under different electrospinning times (such as PI16-80-12) and different electrospinning voltages (such as PI16-70-10) showed that the extension of electrospinning time did not improve efficiency, but increased resistance. Samples under different voltages, such as PI16-70-10, achieved a filtration efficiency of 99.92495%, but its resistance was 178.74Pa.
[0099] When exploring the performance of fine-diameter PI nanofiber membranes in practical applications, a series of filtration efficiency tests were conducted under wind speed conditions and compared with commercial glass fiber filter media. Figure 4 As shown in (c) and (d), at a wind speed of 1 cm / s, the PM0.3 filtration efficiency of the fine-diameter PI nanofiber membrane (PI16-80-10) reached 99.9993%, slightly higher than the 99.9924% of the glass fiber filter. As the wind speed increases, the filtration efficiency of the fine-diameter PI nanofiber membrane decreases slightly, but even at a wind speed of 10 cm / s, its PM0.3 efficiency remains at a high level of 99.9736%. In contrast, the efficiency of the glass fiber filter drops from 99.9924% at 1 cm / s to 99.9317% at 10 cm / s.
[0100] In terms of filtration resistance, the resistance of PI16-80-10 at a wind speed of 1 cm / s is 40.7 Pa, while the resistance of glass fiber filter material is 72.5 Pa, indicating that the thin diameter PI nanofiber membrane has lower airflow resistance under low wind speed conditions. As the wind speed increases, the resistance of PI16-80-10 increases to 351.0 Pa, but it is still lower than the 500.5+Pa resistance value of glass fiber filter material at the same wind speed.
[0101] The temperature limit of fine-diameter PI nanofiber membranes to maintain high-efficiency filtration was explored, and the fine-diameter PI nanofiber membranes were compared with commercial glass fibers under the same conditions, which can clarify the gap between fine-diameter PI nanofiber membranes and commercial high-temperature filtration materials. In the experiment, the fine-diameter PI nanofiber membranes (PI16-80-10) and commercial glass fibers were heated to 410°C at a rate of 10°C / min, and isothermally kept for 1 hour at intervals of 10°C in the range of 350°C to 400°C. Figure 5 As shown in (b), the filtration resistance of glass fiber increases slightly from 302.63 Pa to 310.6 Pa between 350°C and 400°C. The filtration resistance of the fine-diameter PI nanofiber membrane reaches a peak of 205.3 Pa at 360°C, but drops to 195.7 Pa at 400°C. As the temperature increases, the filtration resistance decreases.
[0102] In terms of filtration efficiency, as the temperature increases, the filtration efficiency of glass fiber and fine-diameter PI nanofiber membranes both decrease. The filtration efficiency of glass fiber decreases from 99.98% at 28°C to 99.92% at 400°C, a change of 0.06%. The filtration efficiency of fine-diameter PI nanofiber membranes decreases from 99.99% at 28°C to 99.77% at 400°C, a change of 0.21%. Figure 5 (c) Although the fine-diameter PI nanofiber membrane has been working at a high temperature of more than 350°C for 6 hours at 400°C, its filtration efficiency has dropped to the point where it cannot achieve high-efficiency filtration of PM0.3 particles, but it can still guarantee complete filtration of PM2.5. When the temperature reaches 410°C, PI410 still has a filtration efficiency of 99.96% for PM2.5.
[0103] (5) Surface contact angle The surface wettability of the membrane was evaluated using a JCY-2 contact angle meter from Shanghai Fangrui Instrument Co., Ltd. The membrane was cut into 1×1 cm 2 The film was placed in a rectangular shape and dried in a drying oven at 60°C for 2 hours. A 2 μL water droplet was dropped on the film surface to measure the contact angle (CA), which is an indicator of the hydrophobicity or hydrophilicity of the material. Each test was performed in triplicate to ensure the accuracy and repeatability of the results.
[0104] like Figure 5As shown in (d), the glass fiber (GF) exhibits excellent hydrophobicity, with an initial contact angle of 128.53°. As time goes by, the contact angle slightly decreases to 126.29° at 300 seconds, indicating that its hydrophobic performance has slightly degraded but remains stable overall. For the fine-diameter PI nanofiber membrane, the initial contact angles of the samples at different heat treatment temperatures are close to 130°, showing extremely strong hydrophobicity. The decrease in the contact angle during the observation time is small, indicating that the hydrophobic performance of PI is relatively stable. In particular, the contact angle of the PI400 sample is stable at 126.00°, which is slightly lower than the 127.23° of the PI16-80-10 sample, but the decrease is not large. Despite the slight difference in the initial contact angle, the PI samples at different heat treatment temperatures show similar hydrophobic properties, suggesting that the heat treatment temperature has little effect on the hydrophobic properties of PI. The enhanced hydrophobicity of the fine-diameter PI nanofiber membrane is attributed to the high-temperature imidization treatment at 350°C, which removes the hydrophilic -NH- groups and thus increases the hydrophobic angle. On the other hand, as the heat treatment temperature increases, although the diameter of the nanofibers increases, their diameter range remains between 120nm and 165nm. The finer nanofibers in the present invention lead to the formation of smaller fiber pore sizes. The smaller pore size causes the water droplets to be subjected to greater tension on the surface of the nanofibers, thereby significantly improving the surface water contact angle of the fine-diameter PI nanofiber membrane compared to the 100° to 110° observed in other studies.
[0105] Therefore, the present invention adopts a preparation method and application of a polyimide nanofiber membrane with the above structure. The prepared polyimide nanofiber membrane has the advantages of high filtration efficiency, low resistance, good thermal stability and hydrophobicity, so that it has broad application prospects in the field of high-temperature PM filtration.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing an ultrafine polyimide nanofiber membrane, characterized in that: The following steps are involved: (1) Preparation of polyamic acid solution Dissolving 4,4'-diaminodiphenyl ether in N,N-dimethylacetamide, and obtaining a transparent 4,4'-diaminodiphenyl ether / N,N-dimethylacetamide solution after 4,4'-diaminodiphenyl ether (ODA) is completely dissolved; adding pyromellitic acid anhydride monomer to the 4,4'-diaminodiphenyl ether / N,N-dimethylacetamide solution in multiple portions, stirring to allow 4,4'-diaminodiphenyl ether and pyromellitic acid anhydride monomer to fully react, and allowing to stand to obtain a polyamic acid solution; (2) The polyamic acid solution is electrospun using a metal wire needle-free process; (3) After the electrospinning is completed, the PAA nanofiber membrane is obtained by drying, and then thermal imidization is performed to obtain a polyimide nanofiber membrane.
2. The method for preparing an ultrafine polyimide nanofiber membrane according to claim 1, characterized in that: The solution preparation process in step (1) is carried out under nitrogen protection at 0~5°C.
3. The method for preparing an ultrafine polyimide nanofiber membrane according to claim 1, characterized in that: The concentration of the polyamic acid solution in step (1) is 15-20 wt %.
4. The method for preparing an ultrafine polyimide nanofiber membrane according to claim 1, characterized in that: In step (2), the metal wire needle-free electrospinning process: the voltage is 60-80 kV, the distance from the electrospinning electrode to the carrier is 240 mm, and the distance from the collecting electrode to the carrier is 20 mm; the operating distance of the transfer vehicle is 350 mm, the cycle time is 6 s, and the electrospinning time is 8-12 min; the spinning temperature is 15°C-25°C, and the humidity is 30%-50%.
5. The method for preparing an ultrafine polyimide nanofiber membrane according to claim 1, characterized in that: The specific steps of thermal imidization in step (3) are: The dried PAA nanofiber membrane was placed in a muffle furnace and heated at a rate of 1-2°C / min under air conditions from room temperature to 350-400°C, and kept at 100°C, 200°C, 300°C, and 350°C for 1 h, and then naturally cooled to room temperature to obtain a polyimide nanofiber membrane.
6. An ultrafine polyimide nanofiber membrane, characterized in that: Prepared by the preparation method according to any one of claims 1 to 6.
7. The ultrafine polyimide nanofiber membrane according to claim 6, characterized in that: The average fiber diameter of the polyimide nanofiber membrane is 100~400nm.
8. An application of an ultrafine polyimide nanofiber membrane, characterized in that: Application of ultrafine polyimide nanofiber membrane in high-temperature fine particle filtration.
Citation Information
Patent Citations
Polyimide electrospun nanofiber and preparation method thereof
CN115821416A
Preparation method of reusable multifunctional PI-based nanofiber filtering membrane
CN117717919A