Preparation method and application of evaporator based on biomass hybrid hydrogel

A biomass hybrid hydrogel evaporator, using biochar and polyzwitterionic hydrogel with tetrahydrazide foam stabilization, addresses high energy consumption and salt crystallization issues in saline environments, achieving efficient and cost-effective water evaporation.

CN119075845AActive Publication Date: 2024-12-06HARBIN INSTITUTE OF TECHNOLOGY (SHENZHEN) (INSTITUTE OF SCIENCE AND TECHNOLOGY INNOVATION HARBIN INSTITUTE OF TECHNOLOGY SHENZHEN)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411218350.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing water resource methods such as reverse osmosis, multi-stage flash evaporation, and membrane distillation face high energy consumption, pollution, and equipment costs, while solar interfacial evaporation technologies lack efficient materials for low-cost, high-efficiency water evaporation, especially in saline environments.

Method used

A biomass hybrid hydrogel evaporator is prepared by converting waste biomass into biochar, combining it with polyzwitterionic hydrogel and tetrahydrazide polydimethylsiloxane foam to enhance light-to-heat conversion and water retention, stabilized with a pH regulator, and floated on water surfaces for solar-driven evaporation.

Benefits of technology

The biomass hybrid hydrogel evaporator reduces evaporation enthalpy, improves hydrophilicity, and enhances evaporation efficiency, effectively addressing salt crystallization and evaporation difficulties in saline water bodies, with a simple, cost-effective, and sustainable process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075845A_ABST
    Figure CN119075845A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solar photo-thermal conversion and water treatment, in particular to a preparation method and application of an evaporator based on biomass hybrid hydrogel. The preparation method comprises the following steps of S1, preparation of a solar absorbent; S2, preparation of the hydrogel evaporator. The prepared biomass hybrid hydrogel evaporator is applied to purification of saline water resources; the biomass hybrid hydrogel evaporator prepared by the method has the advantages of evaporation enthalpy reduction, material hydrophilicity improvement, excellent light absorption and thermal conversion capability, high evaporation efficiency, stable combination with the polyelectrolyte resistance effect of zwitterionic hydrogel, and solving of the problems of salt crystallization and difficult evaporation of salt-containing water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar thermal conversion and water treatment, and in particular to a preparation method and application of a biomass hybrid hydrogel evaporator. Background Art

[0002] Water is one of the most abundant resources on earth, but the available fresh water resources are very limited. The existing common water resource methods mainly include reverse osmosis, multi-stage flash evaporation and membrane distillation, but they all have the disadvantages of high energy consumption, serious pollution and expensive equipment. Solar interfacial evaporation technology uses solar energy to separate water and impurities by evaporation with the help of an evaporator. It can use sustainable energy and potential fresh water resources to alleviate water shortages. It has the advantages of low energy consumption, green environmental protection, simplicity and high efficiency. Water in hydrogels exists in three states: free water, intermediate water and bound water. Among them, intermediate water can reduce the energy demand for water evaporation. At the same time, hydrogels are hydrophilic polymers with three-dimensional network structures and highly adjustable physicochemical properties. They are considered to be promising solar evaporators. In particular, polyzwitterionic hydrogels have a unique anti-polyelectrolyte effect in high salinity environments. This unique salt response can decompose its relatively collapsed cohesive state into chain expansion and greater water absorption, which helps to coordinate more salt species and achieve more stretched conformations for water capture in hydrogels.

[0003] The core of interfacial evaporation is to select a suitable solar absorber to efficiently convert light energy into the heat energy required for steam to achieve efficient evaporation. Compared with light-to-heat conversion materials such as metals and semiconductors, carbon-based materials have the advantages of natural broadband light absorption and abundant sources, such as graphene and carbon nanotubes. Among them, biochar is low in cost, simple to prepare, and has a wide absorption band, and can be used as an effective absorber of the solar spectrum. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a preparation method and application of a biomass hybrid hydrogel evaporator. The technical solution of the present invention is: a preparation method based on a biomass hybrid hydrogel evaporator, comprising the following steps:

[0005] S1. Preparation of solar absorber

[0006] S1-1, drying the waste biomass and placing it in a porcelain boat, then transferring it to a tube furnace, heating the tube furnace from room temperature to 400-800°C at a heating rate of 5-10°C / min under a protective atmosphere and maintaining it for 1 hour, cooling it to room temperature and then taking it out, grinding it to obtain a biochar material;

[0007] S1-2, the obtained biochar material is acid-washed with a HNO3 solution with a mass concentration of 3-5%, kept for 12-15 hours, and then washed with water 3-5 times until the water flow is neutral, taken out and dried at 30-50°C, and ball-milled for 10-12 hours until it passes through a 100-200 mesh sieve to obtain a solar absorber;

[0008] S2. Preparation of hydrogel evaporator

[0009] S2-1, dissolving the polyzwitterionic hydrogel in deionized water at a mass ratio of 2-4:6-8, stirring evenly until transparent, to obtain solution A;

[0010] S2-2, preparing an initiator according to a mass ratio of initiator to solution A of 0.04 to 0.06:10, and then preparing a cross-linking agent according to a volume ratio of cross-linking agent to solution A of 1:100 to 130, and then adding the initiator and the cross-linking agent to the solution A obtained in S2-1, mixing, and ultrasonicating for 10 to 20 minutes under the conditions of an ultrasonic temperature of 15°C, an ultrasonic frequency of 40kHz, and an ultrasonic power of 360W to obtain a hydrogel precursor solution;

[0011] S2-3, dispersing the solar absorber obtained in S1-2 in deionized water to obtain solution B;

[0012] S2-4, adding the solution B obtained in S2-3 to the hydrogel precursor solution obtained in S2-2 at a volume ratio of 1:10, mixing and ultrasonicating for 12 to 17 minutes under the conditions of an ultrasonic temperature of 15°C, an ultrasonic frequency of 40kHz, and an ultrasonic power of 360W to obtain a mixed solution, and then adding tetramethylethylenediamine at a volume ratio of 40 to 50 μL:100 mL of the mixed solution, and passing nitrogen gas for aeration for 25 to 35 minutes to obtain liquid C;

[0013] S2-5. Liquid C is injection molded and sealed at 85-95° C., reacted for 3.5-4.5 hours to obtain a hydrogel, and then soaked in deionized water for 20-24 hours, and dried to obtain a biomass hybrid hydrogel evaporator.

[0014] Further, in step S1-1, the waste biomass is coconut shell, sorghum straw or sludge;

[0015] Note: The above biomass is a type of carbon-rich natural resource with the characteristics of sustainability, renewable, biodegradable and low cost.

[0016] Further, in step S1-2, the polyzwitterionic hydrogel is [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl)ammonium hydroxide, the initiator is ammonium persulfate, and the cross-linking agent is polyethylene glycol diacrylate;

[0017] Description: Polyzwitterionic hydrogel has a good anti-polyelectrolyte effect. It can capture and retain water more effectively when treating salt water resources, while reducing the salt crystallization threshold, thereby improving the recovery efficiency of water resources. Ammonium persulfate as an initiator can improve the efficiency of the polymerization reaction and the completeness of the monomer reaction to a certain extent. Polyethylene glycol diacrylate as a cross-linking agent can react with the hydrogel monomer to form a more stable and tough hydrogel network structure, thereby improving its water absorption performance, water retention capacity and mechanical strength.

[0018] Further, in step S2-3, the mass ratio of the solar absorber to deionized water is 1:10;

[0019] Note: The addition of solar absorber in the above proportion makes the gel have better light-to-heat conversion ability, improves the state of water molecules inside the gel, and increases evaporation efficiency.

[0020] Furthermore, in step S2-5, the liquid C is stabilized before the gelation reaction.

[0021] The stabilization treatment method comprises: injecting nitrogen with a purity of 99.9-99.99% into a high-pressure container containing liquid tetrahydrazide polydimethylsiloxane at a volume ratio of 18-22:1, adjusting the temperature of the high-pressure container to 85-95°C and the pressure to 5-15MPa, stirring and diffusing for 3-6h until bubbles are generated, then reducing the pressure in the container at a rate of 0.25-0.5MPa / min until the bubbles are solidified to obtain tetrahydrazide polydimethylsiloxane foam, ultrasonically immersing the tetrahydrazide polydimethylsiloxane foam in liquid C at a mass ratio of 0.3-0.5:1 and mixing for 15-30min, finally dripping a pH adjuster until the pH of the solution is 4.5-5.5, and mixing to obtain stabilized liquid C;

[0022] Among them, the nitrogen injection speed is 900-1000Nm 3 / h, the ultrasonic immersion temperature is 25-30°C, the ultrasonic frequency is 10-12kHz, and the ultrasonic power is 160-180W;

[0023] Description: Low surface tension tetrahydrazide polydimethylsiloxane foam helps to lower the energy threshold of water evaporation, making it easier for water molecules to change from liquid to gas. Mixing liquid C with low surface tension tetrahydrazide polydimethylsiloxane foam can effectively increase the evaporation rate of the evaporator. Tetrahydrazide polydimethylsiloxane foam has a low thermal conductivity, which can reduce heat loss on the surface of the hydrogel evaporator and help maintain a high temperature environment inside the evaporator, thereby accelerating the evaporation of water. By adjusting the pH value of the solution to 4.5-5.5, the swelling rate of the hydrogel can be improved. This optimization helps the hydrogel evaporator maintain stable performance during long-term use, thereby achieving more efficient and stable water evaporation.

[0024] Furthermore, the pH regulator is a hydroxyethylidene diphosphonic acid solution with a concentration of 80 to 100 mg / L or a sodium hydroxide solution with a concentration of 0.5 to 2 mol / L;

[0025] Description: The hydroxyethylidene diphosphonic acid solution is selected as the regulator because, firstly, the anions formed after the dissociation of hydroxyethylidene diphosphonic acid in water form stable complexes or chelates with metal ions such as calcium and magnesium, thereby preventing these metal ions from forming precipitation during the concentration process; secondly, hydroxyethylidene diphosphonic acid can change the kinetic process of crystal growth, making it difficult for crystals to form or the formed crystals are relatively loose and difficult to adhere to the evaporator surface.

[0026] Furthermore, the prepared biomass hybrid hydrogel evaporator is applied to the purification of salt water resources;

[0027] Description: The biomass hydrogel evaporator prepared by the present invention has the advantages of reducing evaporation enthalpy, improving material hydrophilicity, excellent light absorption and heat conversion capabilities, high evaporation efficiency, and better salt crystallization evaporation ability, which can effectively solve the problems of salt crystallization and evaporation difficulty in saline water bodies.

[0028] Furthermore, the application method is: the biomass hybrid hydrogel evaporator is floated on the water surface through an isolation layer, and the solar-driven interface evaporation can be performed under sunlight; the isolation layer is PVA sponge or foam;

[0029] Description: The use of the isolation layer can effectively prevent the hydrogel evaporator from direct contact with the water body, reduce the heat loss of the water body during the evaporation process, and thus improve the efficiency of the evaporator. At the same time, the isolation layer can also serve as a supporting material to keep the position of the hydrogel evaporator stable and prevent it from moving or deforming due to water flow or other factors during the evaporation process.

[0030] PVA sponge or foam is used as an isolation layer, which itself has a certain ability to absorb and retain water. This material can continuously provide water for the hydrogel evaporator and promote the transfer of water molecules to the surface of the evaporator through its pore structure. This water transfer ability can ensure that the evaporator can maintain a stable evaporation rate under continuous light. By floating the hydrogel evaporator on the water surface and performing solar-driven evaporation, this technology can be applied to a wider range of water environments, such as lakes, rivers, seawater, etc. This technology is not only suitable for the recovery and purification of freshwater resources, but can also be used in fields such as seawater desalination.

[0031] Furthermore, the isolation layer is wrapped with a hydrophilic material;

[0032] Description: Hydrophilic materials can quickly absorb and transfer water to the surface of the hydrogel evaporator, which helps to form a uniform and continuous water film on the surface of the evaporator; the uniform distribution of the water film helps to improve the evaporation efficiency of the evaporator because water molecules can more effectively contact solar radiation and convert into water vapor; and hydrophilic materials usually have good thermal conductivity, which can help heat transfer to the evaporator surface faster, thereby accelerating the evaporation of water.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The biomass hybrid hydrogel evaporator prepared by the present invention has the advantages of reducing evaporation enthalpy, improving material hydrophilicity, and excellent light absorption and heat conversion capabilities, high evaporation efficiency, and can stably combine the anti-polyelectrolyte effect of zwitterionic hydrogel, solving the problems of salt crystallization and difficult evaporation of saline water bodies; at the same time, the preparation process of the present invention is simple, easy to operate, and low in price, and can be promoted and applied on a large scale. It is a green and efficient new method with industrial application prospects.

[0035] (2) The present invention combines biochar as an absorbent with polyzwitterionic hydrogel to collect sunlight and convert it into thermal energy, which is then used in situ for the evaporation of water contained in the molecular network. At the same time, the unique anti-polyelectrolyte effect can effectively address the problem of salt in potential freshwater resources and alleviate the occurrence of salt crystallization. Waste biomass is used as the raw material of the absorbent, which is widely available, easy to obtain, and environmentally friendly, thus realizing the "resourceization" of waste disposal and achieving the purpose of "treating waste with waste".

[0036] (3) The present invention stabilizes liquid C before gelation, and utilizes tetrahydrazide polydimethylsiloxane foam with low surface tension to effectively reduce the energy threshold of water evaporation, thereby effectively improving the evaporation rate of the evaporator. The low thermal conductivity of tetrahydrazide polydimethylsiloxane foam is utilized to effectively reduce the heat loss on the surface of the hydrogel evaporator, maintain the high temperature environment inside the evaporator, and thus accelerate the evaporation of water. By preparing a pH regulator with excellent photothermal conversion performance and excellent biological contamination resistance, the swelling rate of the hydrogel is effectively improved, thereby optimizing the hydrogel evaporator to maintain stable performance during long-term use, and at the same time, it also plays a certain role in limiting the deposition of salt, thereby achieving more efficient and stable water evaporation. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a comparison diagram of the evaporation rate of the hydrogel evaporator obtained by carbonizing sorghum straw at 400°C, 600°C, 800°C and without biochar hybridization;

[0038] Figure 2 It is a comparison chart of the evaporation rates of the hydrogel evaporator prepared by carbonization of different biomasses at 600°C, conventional solar evaporation without the aid of an evaporator, and without biochar hybridization;

[0039] Figure 3 is a comparison chart of the long-period evaporation rate of the hydrogel evaporator in Example 1 of the present invention;

[0040] Figure 4 It is a comparison chart of the evaporation rates of the biomass hybrid hydrogel evaporators prepared by Examples 1 to 24 and Control Groups 1 to 5 of the present invention. DETAILED DESCRIPTION

[0041] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.

[0042] Example 1: A method for preparing a biomass hybrid hydrogel evaporator, comprising the following steps:

[0043] S1. Preparation of solar absorber

[0044] S1-1, drying the waste biomass and placing it in a porcelain boat, then transferring it to a tube furnace, heating the tube furnace from room temperature to 600°C at a heating rate of 5°C / min and maintaining it for 1 hour under a protective atmosphere, cooling it to 26°C and then taking it out, grinding it to obtain a biochar material; wherein the protective atmosphere is argon gas; and the waste biomass is sorghum straw;

[0045] S1-2, the obtained biochar material was acid-washed with a 4% HNO3 solution, kept for 14 hours, and then washed with water 7 times until the water flow was neutral, taken out and dried at 40°C, and ball-milled for 12 hours until it passed through a 100-mesh sieve to obtain a solar absorber;

[0046] S2. Preparation of hydrogel evaporator

[0047] S2-1, dissolving the polyzwitterionic hydrogel in deionized water at a mass ratio of 3:7, stirring evenly until transparent, to obtain solution A; the polyzwitterionic hydrogel is [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl) ammonium hydroxide;

[0048] S2-2, preparing an initiator according to a mass ratio of initiator to solution A of 0.05:10, and then preparing a cross-linking agent according to a volume ratio of cross-linking agent to solution A of 1:160, and then adding the initiator and the cross-linking agent to the solution A obtained in S2-1, mixing, and ultrasonicating for 15 minutes under the conditions of an ultrasonic temperature of 15°C, an ultrasonic frequency of 40kHz, and an ultrasonic power of 360W to obtain a hydrogel precursor solution; the initiator is ammonium persulfate, and the cross-linking agent is polyethylene glycol diacrylate;

[0049] S2-3, dispersing the solar absorber obtained in S1-2 in deionized water to obtain solution B; the mass ratio of the solar absorber to the deionized water is 1:10;

[0050] S2-4, adding the solution B obtained in S2-3 to the hydrogel precursor solution obtained in S2-2 at a volume ratio of 1:101, mixing, and ultrasonically treating for 15 min under the conditions of an ultrasonic temperature of 15°C, an ultrasonic frequency of 40 kHz, and an ultrasonic power of 360 W to obtain a mixed solution, and then adding tetramethylethylenediamine at a volume ratio of 45 μL:100 mL of tetramethylethylenediamine: the mixed solution, and passing nitrogen for aeration for 30 min to obtain liquid C;

[0051] S2-5, injection molding liquid C in a sealed state at 90° C., reacting for 4 hours to obtain a hydrogel, and then soaking it in deionized water for 22 hours to obtain a biomass hybrid hydrogel evaporator;

[0052] This embodiment also provides an application method, in which the prepared biomass hybrid hydrogel evaporator is applied to the purification of salt water resources;

[0053] The application method is: the biomass hybrid hydrogel evaporator is floated on the water surface through an isolation layer, and the solar-driven interface evaporation can be carried out under the sunlight; the isolation layer is a PVA sponge; the isolation layer is wrapped with a hydrophilic material; in this embodiment, the hydrophilic material is dust-free paper.

[0054] Example 2: Different from Example 1, in step S1-1, the waste biomass is coconut shell.

[0055] Example 3: Different from Example 1, in step S1-1, the waste biomass is sludge.

[0056] Example 4: Different from Example 1, in step S1-1, the temperature of the tubular furnace is increased from room temperature to 400°C at a heating rate of 5°C / min.

[0057] Example 5: Different from Example 1, in step S1-1, the temperature of the tubular furnace is increased from room temperature to 800°C at a heating rate of 5°C / min.

[0058] Example 6: Different from Example 1, in step S1-2, the obtained biochar material is acid-washed with a HNO3 solution with a mass concentration of 3%, kept for 12 hours, and then washed with water 7 times until the water flow is neutral, taken out and dried at 30°C.

[0059] Example 7: Different from Example 1, in step S1-2, the obtained biochar material is acid-washed with a HNO3 solution with a mass concentration of 5%, kept for 15 hours, and then washed with water 9 times until the water flow is neutral, taken out and dried at 50°C.

[0060] Example 8: Different from Example 1, in step S2-1, the polyzwitterionic hydrogel is dissolved in deionized water at a mass ratio of 2:8.

[0061] Example 9: Different from Example 1, in step S2-1, the polyzwitterionic hydrogel is dissolved in deionized water at a mass ratio of 4:6.

[0062] Example 10: Different from Example 1, in step S2-2, the initiator is prepared according to the mass ratio of initiator: solution A of 0.04:10, and the cross-linking agent is prepared according to the volume ratio of cross-linking agent: solution A of 1:150. Then the initiator and cross-linking agent are added to the solution A obtained in S2-1, mixed and ultrasonicated for 10 minutes.

[0063] Example 11: Different from Example 1, in step S2-2, the initiator is prepared at a mass ratio of initiator: solution A of 0.06:10, and the cross-linker is prepared at a volume ratio of cross-linker: solution A of 1:200. Then the initiator and cross-linker are added to the solution A obtained in S2-1, mixed and ultrasonicated for 20 minutes.

[0064] Example 12: Different from Example 1, in step S2-4, solution B obtained in S2-3 is added to the hydrogel precursor solution obtained in S2-2 at a volume ratio of 1:9, mixed and then ultrasonically treated for 12 minutes to obtain a mixed solution, and then tetramethylethylenediamine is added at a volume ratio of 40 μL:100mL of tetramethylethylenediamine: mixed solution, and nitrogen is passed through for aeration for 25 minutes to obtain liquid C.

[0065] Example 13: Different from Example 1, in step S2-4, solution B obtained in S2-3 is added to the hydrogel precursor solution obtained in S2-2 at a volume ratio of 1:11, mixed and then ultrasonically treated for 17 minutes to obtain a mixed solution, and then tetramethylethylenediamine is added at a volume ratio of 50 μL:100mL of tetramethylethylenediamine: mixed solution, and nitrogen is passed through for aeration for 35 minutes to obtain liquid C.

[0066] Example 14: Different from Example 1, in step S2-5, liquid C is injection molded and sealed at 85°C, reacted for 3.5 hours to obtain a hydrogel, and then soaked in deionized water for 20 hours to obtain a biomass hybrid hydrogel evaporator.

[0067] Example 15: Different from Example 1, in step S2-5, liquid C is injection molded and sealed at 95°C, reacted for 4.5 hours to obtain a hydrogel, and then soaked in deionized water for 24 hours to obtain a biomass hybrid hydrogel evaporator.

[0068] Example 16: Different from Example 1, in step S2-5, the liquid C is stabilized before the gelation reaction.

[0069] The stabilization treatment method is as follows: nitrogen gas with a purity of 99.95% is injected into a high-pressure container containing liquid tetrahydrazide polydimethylsiloxane at a volume ratio of 20:1, the temperature of the high-pressure container is adjusted to 90°C and the pressure is 10MPa, and the mixture is stirred and diffused for 4.5 hours until bubbles are generated, and then the pressure in the container is reduced at a rate of 0.35MPa / min until the bubbles are solidified to obtain tetrahydrazide polydimethylsiloxane foam, and the tetrahydrazide polydimethylsiloxane foam is ultrasonically immersed in liquid C at a mass ratio of 0.4:1 and mixed for 22 minutes. In this embodiment, the pH value of the solution is measured to be 6, and finally a pH adjuster is added dropwise until the pH value of the solution is 5.0, and the stabilized liquid C is obtained by mixing; the pH adjuster is a 90mg / L hydroxyethylidene diphosphonic acid solution;

[0070] Among them, the nitrogen injection speed is 950Nm 3 / h, the ultrasonic immersion temperature was 27°C, the ultrasonic frequency was 14kHz, and the ultrasonic power was 170W.

[0071] Example 17: Different from Example 16, nitrogen with a purity of 99.9% is heated at 900 Nm 3 The mixture is injected into a high-pressure container containing liquid tetrahydrazide polydimethylsiloxane at an injection rate of / h.

[0072] Example 18: Different from Example 16, nitrogen with a purity of 99.99% is heated at a speed of 1000 Nm 3 The mixture is injected into a high-pressure container containing liquid tetrahydrazide polydimethylsiloxane at an injection rate of / h.

[0073] Example 19: Different from Example 16, the temperature of the high-pressure container is adjusted to 85°C and the pressure is 5 MPa, and the mixture is stirred and diffused for 3 hours until bubbles are generated, and then the pressure in the container is reduced at a rate of 0.25 MPa / min until the bubbles solidify.

[0074] Example 20: Different from Example 16, the temperature of the high-pressure container is adjusted to 95°C and the pressure is 15 MPa, and the mixture is stirred and diffused for 6 hours until bubbles are generated, and then the pressure in the container is reduced at a rate of 0.5 MPa / min until the bubbles solidify.

[0075] Example 21: Different from Example 16, the tetrahydrazide polydimethylsiloxane foam is ultrasonically immersed in liquid C and mixed for 15 minutes, and finally a pH adjuster is added dropwise until the solution pH is 4.5, and the stabilized liquid C is obtained by mixing; wherein, the ultrasonic immersion temperature is 25°C, the ultrasonic frequency is 10kHz, and the ultrasonic power is 160W.

[0076] Example 22: Different from Example 16, the tetrahydrazide polydimethylsiloxane foam is ultrasonically immersed in liquid C and mixed for 30 minutes, and finally a pH adjuster is added dropwise until the solution pH is 5.5, and the stabilized liquid C is obtained by mixing; wherein, the ultrasonic immersion temperature is 30°C, the ultrasonic frequency is 12kHz, and the ultrasonic power is 180W.

[0077] Example 23: Different from Example 16, the pH regulator is a hydroxyethylidene diphosphonic acid solution with a concentration of 80 mg / L.

[0078] Example 24: Different from Example 16, the pH regulator is a 100 mg / L hydroxyethylidene diphosphonic acid solution.

[0079] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and is intended to illustrate the practical application effect of the present invention.

[0080] The hydrogel evaporator was floated in a beaker containing 100 mL of 10 wt% NaCl salt water through a PVA sponge. The beaker was placed on an electronic balance and directly below a solar simulator equipped with an AM1.5G filter. The distance between the surface of the evaporation layer hydrogel of the evaporator and the light source was measured and calibrated by a solar power meter so that the light intensity received on the surface was 1 standard sunlight intensity (1 kW / m 2 ), the test was carried out at a room temperature of 25±1℃ and a humidity of about 50%. During the evaporation process, the electronic balance data was recorded every 10 minutes to obtain the mass loss under light. At the same time, a dark evaporation experiment was carried out, that is, the analytical balance was wrapped with tin foil, and the mass loss under dark evaporation was recorded in the same way in a completely light-proof environment. After the evaporation process stabilized, the steady-state evaporation rate V was obtained by the following calculation formula:

[0081]

[0082] Where: M is the net total mass loss (mass loss under light minus mass loss under dark evaporation, kg); A is the area of ​​the evaporation layer hydrogel (m 2 ); T is the total evaporation time (h).

[0083] Figure 1 In the figure, Control is the evaporation rate of the hydrogel evaporator without biochar hybridization; So400-PZH represents the evaporation rate of the hydrogel evaporator prepared by carbonizing sorghum straw at a temperature of 400°C, i.e., Example 4; So600-PZH represents the evaporation rate of the hydrogel evaporator prepared by carbonizing sorghum straw at a temperature of 600°C, i.e., Example 1; So800-PZH represents the evaporation rate of the hydrogel evaporator prepared by carbonizing sorghum straw at a temperature of 600°C, i.e., Example 5; Figure 1 It can be seen that the evaporation rate of the biomass hybrid hydrogel evaporator prepared at 600°C is the best, so Example 1 is selected as the optimal solution;

[0084] Figure 2 In the above, Pure Water is the traditional solar evaporation without the aid of an evaporator; Control is the evaporation rate of the hydrogel evaporator without biochar hybridization; Co600-PZH represents the evaporation rate of the hydrogel evaporator made of coconut shell at a carbonization temperature of 600°C, i.e., Example 2; So600-PZH represents the evaporation rate of the hydrogel evaporator made of sorghum straw at a carbonization temperature of 600°C, i.e., Example 1; Sw600-PZH represents the evaporation rate of the hydrogel evaporator made of sludge at a carbonization temperature of 600°C, i.e., Example 3; Figure 2It can be seen that the evaporation rate of the hydrogel evaporator obtained after carbonization of coconut shell and sorghum straw at 600°C is better, and the evaporation rate of the hydrogel evaporator obtained after carbonization of sludge at 600°C is smaller than that of the hydrogel evaporator obtained after carbonization of coconut shell and sorghum straw at 600°C, but it is improved compared with traditional solar evaporation and hydrogel evaporator without biochar hybridization. It can be seen that the evaporation effect of the hydrogel evaporator after biomass hybridization is better.

[0085] Figure 3 In the experiment, the hydrogel evaporator prepared in Example 1 was used for 7 consecutive evaporations, and it was found that the evaporation rate did not change much and was relatively stable;

[0086] 1. Investigate the effect of the preparation method of the hydrogel evaporator on the evaporation performance of the obtained hydrogel evaporator

[0087] Control group 1: Different from Example 1, the polyzwitterionic hydrogel uses commercially available 3-[(3-acrylamidopropyl)dimethylammonium]propionate polymer.

[0088] Control group 2: Different from Example 1, the mass ratio of the solar absorber to deionized water is 1:9.

[0089] Control group 3: Different from Example 16, liquid C was not mixed with tetrahydrazide polydimethylsiloxane.

[0090] Control group 4: Different from Example 16, the tetrahydrazide polydimethylsiloxane was not subjected to foaming treatment.

[0091] Control group 5: Different from Example 16, a commercially available nitric acid solution with a concentration of 90 mg / L was used as the pH adjuster.

[0092] Conclusion: Figure 4From the comparison of Examples 1 to 24, it can be seen that the parameter changes during the preparation method of the hydrogel evaporator have little effect on the evaporation performance of the hydrogel evaporator. From the comparison of Examples 1, 8 to 9 and Control Group 1, it can be seen that the polyzwitterionic hydrogel is selected. Although the acrylamide-based polymer can form an interpenetrating double network structure to improve the mechanical strength, this structure may cause the flexibility of the hydrogel to decrease. The reduced flexibility of the hydrogel may reduce its surface area or change its shape, thereby affecting the surface area and efficiency of water evaporation. A larger surface area usually contributes to faster water evaporation, and the reduction in flexibility may limit this advantage of the hydrogel. In addition, the reduced flexibility may change the surface absorbance of the hydrogel, thereby affecting its absorption and utilization of solar radiation, thereby indirectly affecting the evaporation efficiency; [2-(Methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl) ammonium hydroxide (SBMA) as a zwitterionic monomer can provide physical crosslinking through its strong dipole and the association between molecular chains to enhance the mechanical properties of the hydrogel. The mechanical reinforcement of the hydrogel helps to reduce rupture during the evaporation process. or deformation, thereby indirectly helping to maintain a high evaporation efficiency; and the methacryloyl compound can not only improve the mechanical strength of the hydrogel, but also has good water retention, frost resistance, self-healing and transparency, etc. Good water retention can maintain a moist state for a longer time, thereby continuously carrying out the evaporation process; good frost resistance, then it can maintain a liquid or stable structure at low temperatures and continue to evaporate; excellent self-healing, can quickly restore its structure and function after slight damage, thereby maintaining the stability of evaporation performance, high transparency can more fully absorb sunlight, thereby improving evaporation efficiency; from the comparison of Example 1 and Control Group 2, it can be seen that a too high proportion of solar absorber will cause the evaporation performance of the hydrogel evaporator to be weakened. Although the solar absorber can improve the hydrogel's ability to absorb sunlight, a too high proportion may cause the absorber to aggregate, forming an area with low light-to-heat conversion efficiency, thereby reducing the overall evaporation efficiency. A too high proportion of solar absorber will also destroy the network structure of the hydrogel, reduce its water retention capacity, and further cause the hydrogel to lose water too quickly during the evaporation process, thereby reducing its evaporation efficiency and durability;

[0093] From the comparison of Examples 1 to 15 and Examples 16 to 24, it can be seen that Examples 16 to 24 perform stabilization treatment on liquid C, and the evaporation performance of the hydrogel evaporator is significantly improved compared with that of Example 1, which can be explained that the stabilization treatment can effectively reduce the adhesion of salt and other pollutants on the evaporation interface, improve the sustainable use of the evaporator, and further improve the evaporation efficiency of the hydrogel evaporator. From the perspective of economy, Example 16 is the best solution;

[0094] From the comparison between Example 16 and Control Group 3 and Control Group 4, it can be seen that since tetrahydrazide polydimethylsiloxane can form reversible covalent bonds (such as acylhydrazone bonds) with other components in the hydrogel, this helps to construct a self-repairing system. When the hydrogel evaporator is damaged during use, these reversible covalent bonds can prompt the hydrogel to self-repair, thereby maintaining the stability and durability of its evaporation performance, thereby improving the evaporation rate and evaporation efficiency of the hydrogel evaporator; however, from the comparison between Example 16 and Control Group 4, it can be seen that the evaporation performance of tetrahydrazide polydimethylsiloxane after foaming is better. The main reason is that the tetrahydrazide polydimethylsiloxane after foaming has a larger specific surface area, which helps to increase the contact area between the hydrogel evaporator and the air, thereby improving the evaporation efficiency. The foam structure can effectively disperse the liquid and make the hydrogel evaporate more evenly. and high efficiency, and since the tetrahydrazide polydimethylsiloxane foam itself has good thermal stability and thermal conductivity, when mixed with the hydrogel precursor solution, these properties can be transferred to the hydrogel, so that it can remain stable at a higher temperature and transfer heat more efficiently, thereby further promoting water evaporation; and from the comparison of Example 16, Example 23 to Example 24 and Control Group 5, it can be seen that the use of a 90 mg / L hydroxyethylidene diphosphonic acid solution as a pH regulator has a significant improvement on the evaporation performance of the hydrogel evaporator compared with the direct use of a 90 mg / L nitric acid solution, the main reason being that the anions formed after the dissociation of hydroxyethylidene diphosphonic acid in water can prevent the metal ions in the evaporator from forming precipitation during the concentration process; and hydroxyethylidene diphosphonic acid can change the kinetic process of crystal growth, making it difficult for the crystal to adhere to the surface of the evaporator.

[0095] In summary, the stabilization treatment of liquid C according to the method provided in the present application before gelation has a more prominent effect on the evaporation performance of the hydrogel evaporator. At the same time, the foaming treatment of tetrahydrazide polydimethylsiloxane also has a good improvement effect on the evaporation performance of the hydrogel evaporator.

Claims

1. A preparation method based on biomass hybrid hydrogel evaporator, It is characterized in that The following steps are involved: S1. Preparation of solar absorber S1-1, drying the waste biomass and placing it in a porcelain boat, then transferring it to a tube furnace, heating the tube furnace from room temperature to 400-800°C at a heating rate of 5°C / min under a protective atmosphere and maintaining it for 1 hour, cooling it to room temperature and then taking it out, grinding it, and obtaining a biochar material; S1-2, the obtained biochar material is treated with HNO with a mass concentration of 3-5%. 3 The solution is acid-washed, maintained for 12 to 15 hours, and then washed with water 7 to 9 times until the water flow is neutral, taken out and dried at 30 to 50° C., and ball-milled for 10 to 12 hours until it passes through a 100 to 200 mesh sieve to obtain a solar absorber; S2. Preparation of hydrogel evaporator S2-1, dissolving the polyzwitterionic hydrogel in deionized water at a mass ratio of 2-4:6-8, stirring evenly until transparent, to obtain solution A; S2-2, preparing an initiator according to a mass ratio of initiator to solution A of 0.04 to 0.06:10, and then preparing a cross-linking agent according to a volume ratio of cross-linking agent to solution A of 1:150 to 200, and then adding the initiator and the cross-linking agent to the solution A obtained in S2-1, mixing, and ultrasonicating for 10 to 20 minutes under the conditions of an ultrasonic temperature of 15°C, an ultrasonic frequency of 40kHz, and an ultrasonic power of 360W to obtain a hydrogel precursor solution; S2-3, dispersing the solar absorber obtained in S1-2 in deionized water to obtain solution B; S2-4, adding the solution B obtained in S2-3 to the hydrogel precursor solution obtained in S2-2 at a volume ratio of 1:10, mixing and ultrasonicating for 12 to 17 minutes under the conditions of an ultrasonic temperature of 15°C, an ultrasonic frequency of 40kHz, and an ultrasonic power of 360W to obtain a mixed solution, and then adding tetramethylethylenediamine at a volume ratio of 40 to 50 μL:100 mL of the mixed solution, and passing nitrogen gas for aeration for 25 to 35 minutes to obtain liquid C; S2-5. Liquid C is injection molded and sealed at 85-95° C., reacted for 3.5-4.5 hours to obtain a hydrogel, and then soaked in deionized water for 20-24 hours to obtain a biomass hybrid hydrogel evaporator.

2. A method for preparing a biomass hybrid hydrogel evaporator according to claim 1, It is characterized in that In step S1-1, the waste biomass is coconut shell, sorghum straw or sludge.

3. A method for preparing a biomass hybrid hydrogel evaporator according to claim 1, It is characterized in that In step S1-2, the polyzwitterionic hydrogel is [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonic acid propyl)ammonium hydroxide, the initiator is ammonium persulfate, and the cross-linking agent is polyethylene glycol diacrylate.

4. The method for preparing a biomass hybrid hydrogel evaporator according to claim 1, It is characterized in that In step S2-3, the mass ratio of the solar absorber to deionized water is 1:

10.

5. The method for preparing a biomass hybrid hydrogel evaporator according to claim 1, It is characterized in that In step S2-5, the liquid C is stabilized before the gelation reaction. The stabilization treatment method comprises: injecting nitrogen with a purity of 99.9-99.99% into a high-pressure container containing liquid tetrahydrazide polydimethylsiloxane at a volume ratio of 18-22:1, adjusting the temperature of the high-pressure container to 85-95°C and the pressure to 5-15MPa, stirring and diffusing for 3-6h until bubbles are generated, then reducing the pressure in the container at a rate of 0.25-0.5MPa / min until the bubbles are solidified to obtain tetrahydrazide polydimethylsiloxane foam, ultrasonically immersing the tetrahydrazide polydimethylsiloxane foam in liquid C at a mass ratio of 0.3-0.5:1 and mixing for 15-30min, finally dripping a pH adjuster until the pH of the solution is 4.5-5.5, and mixing to obtain stabilized liquid C; Among them, the nitrogen injection speed is 900~1000Nm 3 / h, the ultrasonic immersion temperature is 25-30°C, the ultrasonic frequency is 10-12kHz, and the ultrasonic power is 160-180W.

6. A method for preparing a biomass hybrid hydrogel evaporator according to claim 5, It is characterized in that The pH regulator is a hydroxyethylidene diphosphonic acid solution with a concentration of 80 to 100 mg / L or a sodium hydroxide solution with a concentration of 0.5 to 2 mol / L.

7. Application of the biomass hybrid hydrogel evaporator prepared by the method according to any one of claims 1 to 6, It is characterized in that It is applied in the purification of salt water resources.

8. The use of a biomass hybrid hydrogel evaporator as claimed in claim 7, It is characterized in that The application method is as follows: the biomass hybrid hydrogel evaporator is floated on the water surface through an isolation layer, and the evaporation of the solar-driven interface can be carried out under the irradiation of sunlight; the isolation layer is PVA sponge or foam.

9. The use of a biomass hybrid hydrogel evaporator as claimed in claim 7, It is characterized in that The isolation layer is wrapped with a hydrophilic material.

Citation Information

Patent Citations

  • Graphene-Carbon Hybrid Foam

    CN108602046A

  • Preparation method of biomass carbon material for solar evaporated water and application of biomass carbon material

    CN109734148A

  • Photo-thermal hydrogel, preparation method and application thereof, and photo-thermal conversion evaporator

    CN114456308A

  • Boron carbide bilayer foam solar evaporator and method for preparing thereof

    US20220082302A1