Supported catalyst as well as preparation method and application thereof
By loading precious metal and non-precious metal active components on the porous support to form a supported catalyst with characteristic peaks, the complex operation, high cost and poor stability in the hydrodechlorination reaction of silicon tetrachloride is solved, and the three efficient Preparation of chlorosilicon, the conversion rate and selectivity are significantly improved.
Patent Information
- Application Number
- CN202411308186.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
AI Technical Summary
The existing catalytic reaction of silicon tetrachloride hydrodechloride preparation is complicated, high cost, poor stability, poor conversion rate and excessive impurities in the catalytic reaction.
Using a supported catalyst, the catalyst includes precious metal and non-precious metal active components supported on the porous support, the characteristic peaks are displayed by XPS and O17 MQ-MAS-NMR detection, forming chemical bonds of noble metals and carbonyl complexes and Si-O-precious metals. Optimize the distribution of precious and non-precious metals to improve the stability and activity of the catalyst.
Significantly improve the conversion rate of silicon tetrachloride and the selectivity of trichlorosilicon, the stability and activity of catalysts, the conversion rate is not less than 20%, the selectivity is not less than 85%, and it remains highly efficient during long-term use. active.
Smart Images

Figure BDA0005049884200000101 
Figure BDA0005049884200000161 
Figure BDA0005049884200000162
Abstract
Description
Technical Field
[0001] The present invention relates to the field of hydrodechlorination catalysis, and relates to a supported catalyst, a preparation method of the supported catalyst, and application of the supported catalyst in the field of catalysts for preparing trichlorosilane by hydrodechlorination of silicon tetrachloride. Background Art
[0002] As a widely used organic silicon monomer, trichlorosilane is mainly used to produce semiconductor silicon, single crystal silicon, polycrystalline silicon and silane coupling agents, etc. It is widely used in photovoltaic, semiconductor and organic silicon materials. The preparation method of trichlorosilane in industry is mostly Siemens process. In the existing Siemens process, trichlorosilane is generated by catalytic hydrogenation reaction using silicon tetrachloride, silicon powder and hydrogen as raw materials through cold hydrogenation process.
[0003] At present, the catalyst commonly used in catalytic hydrogenation is a transition metal catalyst. For example, CN102350351B discloses a hydrogenation catalyst and a preparation method thereof, wherein the catalyst is prepared by melt atomization, and copper silicon alloy, copper nickel silicon alloy, copper silicon rare earth alloy or copper nickel silicon rare earth alloy is used as an active component, and the conversion rate of silicon tetrachloride can reach up to 25%. However, the operation of the melt atomization method is relatively complicated, and is specifically manifested as being difficult to control the particle size, and larger particles will cause internal wear of the fluidized bed, and smaller particles cannot be recovered. CN102814181B adopts a melting method to prepare a copper nickel alloy catalyst, wherein the mass content of nickel is 10-35%, and the catalyst has excellent high temperature stability, and the catalyst can be directly discharged after the reaction is completed, but the melting method needs to be carried out under high temperature conditions, and the energy consumption is large, which increases the production cost. CN111434382B discloses a carrier-supported vanadium oxide-promoted Rh-based catalyst and its preparation method and application. The invention uses precious metal Rh as an active component and metal V as an additive, wherein the mass percentage of Rh is 1-5%. MCM-41 is used as a carrier to prepare a supported catalyst. The catalyst prepared by this method is evenly dispersed on the surface of the carrier and has a small size. It can be seen from the continuous reaction for 20 hours that the catalyst is relatively stable. In the absence of an additive, the selectivity of the catalyst drops from 11% to 5%, and the conversion rate drops from 3.2% to 0.8%. The method provided by this patent is relatively limited in the selection of active components and modified additives. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of complex operation, high cost, poor stability, poor conversion rate and excessive impurities in the catalytic reaction of preparing trichlorosilane by hydrodechlorination of silicon tetrachloride in the prior art, and to provide a supported catalyst, which has better purity and stability, and a simple preparation method and low cost.
[0005] In order to achieve the above object, the present invention provides a supported catalyst, which includes a porous carrier and an active component supported on the porous carrier; the active component includes a noble metal and a non-noble metal; wherein at least part of the noble metal element is complexed with CO,
[0006] XPS characterization shows that the supported catalyst has characteristic peaks at 300eV-320eV and 840eV-880eV; and / or, 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 35ppm-45ppm.
[0007] The second aspect of the present invention provides a method for preparing the supported catalyst according to the first aspect of the present invention, the method comprising:
[0008] S1: loading a noble metal source and a CO donor on a porous carrier to prepare a first catalyst;
[0009] S2: loading a non-precious metal source on the first catalyst to prepare a second catalyst;
[0010] S3: drying and calcining the second catalyst to prepare a supported catalyst;
[0011] The method enables at least part of the noble metal elements in the obtained supported catalyst to be complexed with CO; and XPS characterization shows that the supported catalyst has characteristic peaks at 300eV-320eV and 840eV-880eV; and / or, 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 35ppm-45ppm.
[0012] The third aspect of the present invention provides a method for preparing trichlorosilane by hydrodechlorination of silicon tetrachloride, wherein the catalyst used in the method is selected from the supported catalyst described in the first aspect of the present invention.
[0013] The fourth aspect of the present invention provides an application of the supported catalyst described in the first aspect of the present invention in the field of catalysts for preparing trichlorosilane by hydrodechlorination of silicon tetrachloride.
[0014] The present invention loads active ingredients containing precious metals and non-precious metals on a porous carrier, and at least part of the precious metal elements are complexed with carbonyl groups, so that the porous carrier and the carbonyl complex form chemical bonds while the non-precious metal can break hydrogen bonds to form hydrogen ions. This not only improves the dispersion of the precious metals and non-precious metals on the carrier surface, but also can firmly fix the precious metals and non-precious metals on the porous carrier, thereby reducing the loss of active components and improving the stability and activity of the catalyst. DETAILED DESCRIPTION
[0015] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0016] The present invention provides a supported catalyst, which comprises a porous carrier and an active component supported on the porous carrier; the active component comprises a noble metal and a non-noble metal; wherein at least part of the noble metal elements are complexed with CO, and the supported catalyst has characteristic peaks at 300eV-320eV and 840eV-880eV as characterized by XPS; and / or 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 35ppm-45ppm.
[0017] In the present invention, the distribution of the precious metal and non-precious metal components on the porous carrier can be optimized as follows, that is, the precious metal is mainly distributed in the inner layer of the porous carrier relative to the non-precious metal, and the non-precious metal is mainly distributed in the sub-surface layer of the porous carrier.
[0018] By adopting this preferred distribution mode, when the obtained catalyst is used to catalyze the hydrodechlorination of silicon tetrachloride to prepare trichlorosilane, the non-precious metal components mainly distributed in the sub-surface layer of the porous carrier will be more conducive to the breaking of hydrogen bonds of hydrogen, and the precious metal components mainly distributed in the relatively inner layer will be able to remove a chlorine molecule more promptly, thereby promoting the rapid binding of active hydrogen to the Si base with broken chlorine bonds, thereby obtaining a higher silicon tetrachloride conversion rate and trichlorosilane selectivity.
[0019] For this purpose, preferably, more than 90wt%, even more than 95wt% of the precious metals are distributed in the inner layer of the porous carrier, and more than 90wt%, even more than 95wt% of the non-precious metals are distributed in the sub-surface layer of the porous carrier. The inner layer of the porous carrier and the sub-surface layer of the porous carrier are defined relative to the porous carrier, wherein the inner layer is more distributed inside the pores of the porous carrier relative to the sub-surface layer, and the sub-surface layer is more distributed outside the pores of the porous carrier rather than the outer surface of the porous carrier. The sub-surface layer can be considered to be, for example, the area from the center of the porous carrier to the outside, 70-95% by volume, and the inner layer can be considered to be the area from the center of the porous carrier to within 50% by volume.
[0020] In a preferred embodiment of the present invention, the porous carrier is in direct contact with the carbonyl noble metal complex to form a Si-O-noble metal chemical bond, which can improve the dispersion of the noble metal on the carrier surface while also firmly fixing the noble metal on the carrier, thereby reducing the loss of active components and further improving the stability and activity of the catalyst. Preferably, the noble metal is selected from one or more of rhodium, platinum, palladium and ruthenium.
[0021] According to the present invention, non-precious metals can be embedded in the sub-surface layer of the porous carrier to fix it on the carrier surface. At the same time, the non-precious metals can effectively activate hydrogen to further increase the hydrogen bond breaking rate. Preferably, the non-precious metals are selected from one or more of nickel, iron, copper and cobalt.
[0022] In the present invention, in order to improve the coordination effect of the noble metal and the non-noble metal, preferably, the molar ratio of the noble metal to the non-noble metal is 1:5-50, preferably 1:8-35.
[0023] In the present invention, the catalyst can be a non-reduced catalyst or a reduced catalyst. For example, when used in the catalytic reaction of preparing trichlorosilane by hydrodechlorination of silicon tetrachloride of the present invention, the catalyst can be subjected to reduction treatment before use to obtain a reduced catalyst. For this purpose, non-precious metals will exist in the form of metals, and at this time, the precious metals mainly exist in the form of oxides, precious metal carbonyl complexes, and Si-O-precious metal chemical bonds.
[0024] In the present invention, the porous carrier can be selected from at least one of silicon oxide, molecular sieve and activated carbon. The molecular sieve can be, for example, TS-1 molecular sieve, SBA-15 molecular sieve, HY molecular sieve, HMS molecular sieve, ZSM-5 molecular sieve, especially ZSM-5 molecular sieve.
[0025] In order to strengthen the stability of the chemical bond formed by the porous carrier and the carbonyl complex, so that the noble metal and the non-noble metal can be better loaded on the porous carrier, preferably, the specific surface area of the porous carrier is 100 to 500 m 2 / g, micropore volume is 0.1-0.5cm 3 / g, and the mesopore volume is 0.1-0.8cm 3 / g, and the mesopore volume accounts for 30-90vt%.
[0026] More preferably, the specific surface area of the porous carrier is 200 to 400 m 2 / g, micropore volume is 0.1-0.3cm 3 / g, and the mesopore volume is 0.2-0.7cm 3 / g, and the mesopore volume accounts for 40-80vt%.
[0027] The second aspect of the present invention provides a method for preparing the supported catalyst according to the first aspect of the present invention, the method comprising:
[0028] S1: loading a noble metal source and a CO donor on a porous carrier to prepare a first catalyst;
[0029] S2: loading a non-precious metal source on the first catalyst to prepare a second catalyst;
[0030] S3: drying and calcining the second catalyst to prepare a supported catalyst;
[0031] The method enables at least part of the noble metal elements in the obtained supported catalyst to be complexed with CO; and XPS characterization shows that the supported catalyst has characteristic peaks at 300eV-320eV and 840eV-880eV; and / or, 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 35ppm-45ppm.
[0032] In the present invention, in order to improve the coordination between the porous carrier and the active component (precious metal, non-precious metal) and to increase the loading rate of the active component, preferably, the method for preparing the supported catalyst further comprises acid-modifying or alkali-modifying the porous carrier.
[0033] In the present invention, in order to make the porous carrier have better loading conditions, preferably, the acid modification treatment includes stirring the porous carrier and the acidic solution at 70-100°C for 10-25h, and then drying at 80-120°C for 8-15h and calcining at 400-600°C for 5-10h; more preferably, the acid in the acidic solution is selected from at least one of hydrochloric acid, sulfuric acid and nitric acid.
[0034] Preferably, the alkali modification treatment comprises stirring the porous carrier and the alkaline solution at 70-100°C for 10-25h, and then drying at 80-120°C for 8-15h and calcining at 400-600°C for 5-10h; more preferably, the alkali in the alkaline solution is selected from at least one of sodium hydroxide, potassium hydroxide and ammonia water.
[0035] In the present invention, preferably, the acid in the acidic solution is selected from at least one of hydrochloric acid, sulfuric acid and nitric acid, and the concentration of the acidic solution can be, for example, 0.5-3 mol / L. Preferably, the alkali in the alkaline solution is selected from at least one of sodium hydroxide, potassium hydroxide and ammonia water, and the concentration of the alkaline solution can be 0.5-3 mol / L.
[0036] According to the present invention, there are many ways to better load the precious metal source and the CO donor on the porous carrier. In the present invention, preferably, the loading method includes: in step S1, a solution of the precious metal source, the CO donor and the porous carrier are first mixed to load the precious metal source and the CO donor on the porous carrier.
[0037] In the present invention, preferably, the reaction conditions of the first mixing treatment include: temperature of 20-80° C. and time of 0.5-4 h.
[0038] In the present invention, the precious metal source can be selected from a variety of precious metal salts. Preferably, the precious metal source is selected from precious metal halides and / or nitrates, such as precious metal chlorides, precious metal bromides, and precious metal nitrates. Specifically, it can be selected from: one or more of rhodium chloride, platinum chloride, palladium chloride, ruthenium chloride, rhodium bromide, platinum bromide, palladium bromide, ruthenium bromide, rhodium nitrate, platinum nitrate, palladium nitrate and ruthenium nitrate, preferably rhodium chloride and / or rhodium nitrate.
[0039] In the present invention, the concentration of the solution of the noble metal source is 0.001 to 0.1 mol / L, preferably 0.002 to 0.008 mol / L. The solution of the noble metal source may be an aqueous solution of the noble metal source.
[0040] In the present invention, the CO donor will be able to provide CO for complexing the precious metal in the porous carrier. Preferably, the CO donor is selected from one or more of formic acid, sodium formate and methyl formate.
[0041] In the present invention, in order to achieve an optimal ratio between the precious metals in the form of oxides, precious metal carbonyl complexes, and Si-O-precious metal chemical bonds in the loading process, and to prepare a loaded catalyst with higher stability and activity, preferably, the molar ratio of the precious metal source calculated as the precious metal element to the CO donor is 1:1-10, preferably 1:1.5-6.
[0042] According to the present invention, there are many ways to better load the non-precious metal source on the porous carrier. In the present invention, preferably, the loading method includes: in step S2, the solution of the non-precious metal source is subjected to a second mixing treatment with the first catalyst to load the non-precious metal source on the porous carrier; the molar ratio of the amount of the precious metal source to the amount of the non-precious metal source is 1:5-50, preferably 1:8-35.
[0043] In the present invention, preferably, the reaction conditions of the second mixing treatment include: temperature of 20-100° C. and time of 1-5 h.
[0044] In the present invention, the non-precious metal source can be selected from a variety of non-precious metal salts. Preferably, the non-precious metal source is selected from non-precious metal halides and / or non-precious metal nitrates, such as non-precious metal chlorides, non-precious metal bromides, and non-precious metal nitrates. Specifically, it can be selected from: nickel chloride, ferric chloride, cupric chloride, cobalt chloride, nickel bromide, ferric bromide, cupric bromide, cobalt bromide, nickel nitrate, ferric nitrate, copper nitrate and cobalt nitrate. One or more of nickel chloride and / or nickel nitrate are preferred.
[0045] In the present invention, preferably, the concentration of the solution of the non-precious metal source is 0.01-0.5 mol / L, preferably 0.15-0.3 mol / L.
[0046] In the present invention, in order to enable the non-precious metal source to be better loaded on the porous carrier, preferably, in step S2, the mixed solution of the non-precious metal source solution and the first catalyst is further adjusted to a pH of 7-12 and a temperature of 60-100° C. Preferably, the reagent for adjusting the pH is selected from at least one of ammonia water, urea and sodium hydroxide.
[0047] In the present invention, preferably, in step S3, the reaction conditions of the drying treatment include: a temperature of 100-120° C. and a time of 10-12 h.
[0048] In the present invention, preferably, the reaction conditions of the calcination treatment include: a temperature of 400-800° C. and a time of 4-8 hours.
[0049] In the present invention, a washing process may be included before the drying process. The washing process may include, for example, washing with water to remove excess pH adjusting agents, and in particular, washing with water until the filtrate is neutral.
[0050] In the present invention, when the non-precious metal exists in the form of metal, it can be better embedded in the sub-surface of the porous carrier and fixed on the carrier surface. At the same time, the non-precious metal in the form of metal can effectively activate hydrogen and accelerate the breaking of hydrogen bonds to produce hydrogen ions. To this end, preferably, the preparation method of the supported catalyst also includes step S4: reducing the supported catalyst.
[0051] In the present invention, preferably, the reaction conditions of the reduction treatment include: introducing a reducing gas at 300-600° C. for 2-5 hours; the reducing gas is preferably hydrogen.
[0052] The third aspect of the present invention provides a method for preparing trichlorosilane by hydrodechlorination of silicon tetrachloride, wherein the catalyst used in the method is selected from the supported catalyst described in the first aspect of the present invention.
[0053] The supported catalyst described in the first aspect of the present invention is loaded with active ingredients containing noble metals and non-noble metals on a porous carrier, and at least part of the noble metal elements are complexed with carbonyl groups, so that the porous carrier and the carbonyl complex form chemical bonds while the non-noble metal can break hydrogen bonds to form hydrogen ions, thereby improving the stability and activity of the catalyst. Therefore, when the supported catalyst is used to prepare trichlorosilane, the conversion rate of silicon tetrachloride (STC conversion rate / %) and the selectivity of trichlorosilane (TCS selectivity / %) can be significantly improved, wherein the STC conversion rate is not less than 20%, and the TCS selectivity is not less than 85%. In particular, under long-term use, the catalytic activity can still be maintained, and a high STC conversion rate and TCS selectivity can be maintained (for example, under 7 days of catalytic use, the STC conversion rate can be maintained at not less than 15%, and the TCS selectivity can be maintained at not less than 90%).
[0054] The fourth aspect of the present invention provides an application of the supported catalyst described in the first aspect of the present invention in the field of catalysts for preparing trichlorosilane by hydrodechlorination of silicon tetrachloride.
[0055] The present invention will be described in detail below through examples.
[0056] In the following examples, ZSM-5 molecular sieve is a commercial product with the brand name ZSM-5 produced by Zoran Environmental Protection Technology (Dalian) Co., Ltd.;
[0057] TS-1 molecular sieve is a commercial product of Zhuoran Environmental Protection Technology (Dalian) Co., Ltd. with the brand name TS-1.
[0058] XPS characterization was performed using an Escalab 250Xi X-ray photoelectron spectrometer.
[0059] O 17 The MQ-MAS-NMR nuclear magnetic resonance detection used a Varian 400MHz nuclear magnetic resonance instrument.
[0060] Preparation Example 1-5:
[0061] Preparation Examples 1-5 are used to illustrate ZSM-5 molecular sieves A1-A5 after acid modification;
[0062] Preparation Example 1: 5 g of ZSM-5 molecular sieve was added to 150 g of hydrochloric acid solution (0.5 mol / L), and stirred at 90° C. for 20 h, then filtered and washed with deionized water, and then dried at 100° C. for 12 h and calcined at 500° C. for 8 h to obtain acid-modified ZSM-5 molecular sieve A1;
[0063] Preparation Example 2: 5 g of ZSM-5 molecular sieve was added to 150 g of hydrochloric acid solution (1 mol / L), and stirred at 90° C. for 20 h, then filtered and washed with deionized water, and then dried at 100° C. for 12 h and calcined at 500° C. for 8 h to obtain acid-modified ZSM-5 molecular sieve A2;
[0064] Preparation Example 3: Add 5 g of ZSM-5 molecular sieve to 150 g of hydrochloric acid solution (2 mol / L), stir and treat at 90°C for 20 h, then filter and wash with deionized water, dry at 100°C for 12 h, and calcine at 500°C for 8 h to obtain acid-modified ZSM-5 molecular sieve A3.
[0065] Preparation Example 4: Add 5 g of ZSM-5 molecular sieve to 300 g of hydrochloric acid solution (0.5 mol / L), stir and treat at 90°C for 20 h, then filter and wash with deionized water, dry at 100°C for 12 h, and calcine at 500°C for 8 h to obtain acid-modified ZSM-5 molecular sieve A4.
[0066] Preparation Example 5: 5 g of ZSM-5 molecular sieve was added to 150 g of hydrochloric acid solution (0.5 mol / L), and stirred at 90° C. for 20 h, and then filtered and washed with deionized water to obtain acid-modified ZSM-5 molecular sieve A5.
[0067] Preparation Example 6
[0068] This preparation example is used to illustrate the base-modified ZSM-5 molecular sieve A6;
[0069] 5 g of ZSM-5 molecular sieve was added to 150 g of sodium hydroxide solution (0.5 mol / L), stirred at 90°C for 20 h, filtered and washed with deionized water, dried at 100°C for 12 h, and calcined at 500°C for 8 h to obtain alkali-modified ZSM-5 molecular sieve A6.
[0070] Preparation Example 7
[0071] This preparation example is used to illustrate the acid-modified TS-1 molecular sieve A7;
[0072] A method similar to that of Preparation Example 1 was adopted, except that TS-1 molecular sieve was used to replace ZSM-5 molecular sieve to obtain acid-modified TS-1 molecular sieve A7.
[0073] Preparation Example 8
[0074] This preparation example is used to illustrate the unmodified ZSM-5 molecular sieve A8.
[0075] The structural characteristic parameters of the molecular sieves prepared in Preparation Examples 1-8 are shown in Table 1.
[0076] Table 1
[0077]
[0078] Example 1
[0079] (1) First, 0.10 g RhCl 3 ·3H 2 O was dissolved in 150 mL of deionized water to prepare RhCl 3 The aqueous solution was then stirred at 70°C for 2 hours with 4g of ZSM-5 molecular sieve A1 prepared in Preparation Example 1, and then 0.09g of formic acid was added dropwise, and the reaction was continued for 0.5h to prepare the first catalyst;
[0080] (2) First, 3.77 g Ni(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water to prepare Ni(NO 3 ) 2 aqueous solution, and then Ni(NO 3 ) 2 The aqueous solution is mixed with the first catalyst, and then 5 wt % ammonia water is added dropwise to the mixed solution when the temperature is raised to 70° C. until the pH value is 12. After the addition is completed, the mixed solution is heated to 90° C. again and reacted for 4 hours to prepare a second catalyst;
[0081] (3) The second catalyst was filtered, washed with deionized water until the filtrate was neutral, dried at 100° C. for 12 h, and calcined at 450° C. for 4 h to obtain a supported catalyst Ia1;
[0082] (4) grinding the supported catalyst Ia1, introducing a reducing gas at 450° C. for 2 h, wherein the reducing gas is high-purity hydrogen of not less than 99.99%, to prepare a supported catalyst IA1;
[0083] Among them, the molar ratio of Rh to formic acid is 1:5; the molar ratio of Rh to Ni is 1:34.
[0084] XPS characterization showed that the supported catalyst IA1 had characteristic peaks at 852.3 eV and 858.4 eV in the Ni 2p3 / 2 region, and had a characteristic peak at 305.9 eV in the Rh 3d5 / 2 region; 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 39.6 ppm.
[0085] Example 2
[0086] (1) First, 0.19 g RhCl 3 ·3H 2 O was dissolved in 150 mL of deionized water to prepare RhCl 3 The aqueous solution was then stirred at 70°C for 3 hours with 4g of ZSM-5 molecular sieve A1 prepared in Preparation Example 1, and then 0.16g of formic acid was added dropwise, and the reaction was continued for 0.5h to prepare the first catalyst;
[0087] (2) First, 3.6 g Ni(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water to prepare Ni(NO 3 ) 2 aqueous solution, and then Ni(NO 3 ) 2 The aqueous solution is mixed with the first catalyst, and then 5 wt % ammonia water is added dropwise to the mixed solution when the temperature is raised to 70° C. until the pH value is 12. After the addition is completed, the mixed solution is heated to 90° C. again and reacted for 4 hours to prepare a second catalyst;
[0088] (3) The second catalyst was filtered, washed with deionized water until the filtrate was neutral, dried at 100° C. for 12 h, and calcined at 450° C. for 4 h to obtain a supported catalyst Ia2;
[0089] (4) grinding the supported catalyst Ia2, introducing a reducing gas at 450° C. for 2 h, wherein the reducing gas is high-purity hydrogen of not less than 99.99%, to prepare a supported catalyst IA2;
[0090] Among them, the molar ratio of Rh to formic acid is 1:2.7; the molar ratio of Rh to Ni is 1:17;
[0091] XPS characterization showed that the supported catalyst IA2 had characteristic peaks at 852.5 eV and 858.1 eV in the Ni 2p3 / 2 region, and had a characteristic peak at 305.8 eV in the Rh 3d5 / 2 region; 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 39.6 ppm.
[0092] Example 3
[0093] (1) First, 0.34 g RhCl 3 ·3H 2 O was dissolved in 150 mL of deionized water to prepare RhCl 3The aqueous solution was then stirred at 70°C for 3 hours with 4g of the molecular sieve A1 prepared in Preparation Example 1 of ZSM-5, and then 0.3g of formic acid liquid was added dropwise, and the reaction was continued for 0.5h to prepare the first catalyst;
[0094] (2) First, 3.30 g Ni(NO 3 ) 2 6H 2 O was dissolved in 150 mL of deionized water to prepare Ni(NO 3 ) 2 aqueous solution, and then Ni(NO 3 ) 2 The aqueous solution is mixed with the first catalyst, and then 5 wt % ammonia water is added dropwise to the mixed solution when the temperature is raised to 70° C. until the pH value is 12. After the addition is completed, the mixed solution is heated to 90° C. again and reacted for 4 hours to prepare a second catalyst;
[0095] (3) The second catalyst was filtered, washed with deionized water until the filtrate was neutral, dried at 100° C. for 12 h, and calcined at 450° C. for 4 h to obtain a supported catalyst Ia3;
[0096] (4) grinding the supported catalyst Ia3, introducing a reducing gas at 450° C. for 2 h, wherein the reducing gas is high-purity hydrogen of not less than 99.99%, to prepare a supported catalyst IA3;
[0097] Among them, the molar ratio of Rh to formic acid is 1:1.5; the molar ratio of Rh to Ni is 1:8;
[0098] XPS characterization showed that the supported catalyst IA3 had characteristic peaks at 852.7 eV and 858.3 eV in the Ni 2p3 / 2 region, and had a characteristic peak at 305.9 eV in the Rh 3d5 / 2 region; 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 39.6 ppm.
[0099] Example 4
[0100] The method of Example 1 was followed, except that the ZSM-5 molecular sieve A2 prepared in Preparation Example 2 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1, to prepare the supported catalyst IA4.
[0101] Example 5
[0102] The method of Example 1 was followed, except that the ZSM-5 molecular sieve A3 prepared in Preparation Example 3 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1, to prepare the supported catalyst IA5.
[0103] Example 6
[0104] The method of Example 1 was followed, except that the ZSM-5 molecular sieve A4 prepared in Preparation Example 4 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1, to prepare the supported catalyst IA6.
[0105] Example 7
[0106] According to the method of Example 1, the ZSM-5 molecular sieve A5 prepared in Preparation Example 5 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1 to prepare the supported catalyst IA7.
[0107] Example 8
[0108] According to the method of Example 1, the ZSM-5 molecular sieve A6 prepared in Preparation Example 6 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1 to prepare the supported catalyst IA8.
[0109] Example 9
[0110] The method of Example 1 was followed, except that the TS-1 molecular sieve A7 prepared in Preparation Example 7 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1, to prepare the supported catalyst IA9.
[0111] Example 10
[0112] The method of Example 1 was followed, except that the unmodified ZSM-5 molecular sieve A8 in Preparation Example 8 was used to replace the ZSM-5 molecular sieve A1 prepared in Preparation Example 1, to prepare the supported catalyst IA10.
[0113] Embodiment 11
[0114] The method of Example 1 was followed, except that an equimolar amount of HPtCl was used. 6 6H 2 O replaces RhCl 3 ·3H 2 O, and the supported catalyst IA11 was prepared.
[0115] Example 12
[0116] The method of Example 1 was followed, except that an equimolar amount of Co(NO 3 ) 2 6H 2 O replaces Ni(NO 3 ) 2 6H 2 O, and the supported catalyst IA12 was prepared.
[0117] Embodiment 13
[0118] The supported catalyst IA13 was prepared according to the method of Example 1, except that the molar ratio of Rh to Ni was 1:5.
[0119] Embodiment 14
[0120] The supported catalyst IA14 was prepared according to the method of Example 1, except that the molar ratio of Rh to Ni was 1:40.
[0121] Embodiment 15
[0122] The supported catalyst IA15 was prepared according to the method of Example 1, except that the molar ratio of Rh to formic acid was 1:1.
[0123] Example 16
[0124] The supported catalyst IA16 was prepared according to the method of Example 1, except that the molar ratio of Rh to formic acid was 1:8.
[0125] Comparative Example 1
[0126] The method of Example 1 is followed, except that step (1) is as follows: first, 0.10 g of acetylacetonato carbonyl rhodium (purchased from Kunming Bosheng Metal Materials Processing Co., Ltd., CAS No. 14284-92-5) is dissolved in 150 mL of deionized water to prepare an acetylacetonato carbonyl rhodium aqueous solution, and then the mixture is stirred at a constant temperature of 70° C. for 2 h with 4 g of the ZSM-5 molecular sieve A1 prepared in Preparation Example 1 to prepare a first catalyst;
[0127] The remaining steps were the same as those in Example 1 to prepare the supported catalyst IB1.
[0128] Comparative Example 2
[0129] The supported catalyst IB2 was prepared according to the method of Example 1, except that the CO donor (formic acid) was not added.
[0130] Test Example 1
[0131] 0.5 g of the supported catalysts IA1-IA16 and IB1-IB2 prepared in Examples 1-16 and Comparative Examples 1-2 were respectively subjected to hydrodechlorination reaction with a mixture of silicon tetrachloride and hydrogen, wherein the hydrodechlorination reaction temperature was 550° C., the pressure was 3.0 MPa, and the H 2 / STC=5, trichlorosilane S1-S16, DS1-DS2 were prepared;
[0132] The real-time silicon tetrachloride conversion rate (STC conversion rate / %) and trichlorosilane selectivity (TCS selectivity / %) in the hydrodechlorination reaction of Examples 1-16 and Comparative Examples 1-2 were calculated, as well as the silicon tetrachloride conversion rate (7-day STC conversion rate / %) and trichlorosilane selectivity (7-day TCS selectivity / %) after the hydrodechlorination reaction was carried out for 7 days, as shown in Table 2.
[0133] Test method:
[0134] 1. The calculation formula of silicon tetrachloride conversion rate (STC conversion rate / %) is:
[0135]
[0136] Where: C 0(STC) is the initial molar concentration of silicon tetrachloride, mol / L; C (STC) is the molar concentration of silicon tetrachloride after the reaction, mol / L.
[0137] 2. The calculation formula of trichlorosilane selectivity (TCS selectivity / %) is:
[0138]
[0139] Where: C (TCS) is the molar concentration of trichlorosilane generated by the reaction, mol / L; and ΣC (i) It is the sum of the molar concentrations of various reaction products converted by hydrogenation of silicon tetrachloride, mol / L.
[0140] Table 2
[0141]
[0142]
[0143] It can be seen from the results of Table 1 that compared with the supported catalysts prepared in Comparative Examples 1-2, the supported catalysts prepared in Examples 1-16 of the present invention have higher STC conversion / % and TCS selectivity / % in the hydrogenation reaction of silicon tetrachloride, and have significantly better selective hydrogenation capabilities. In particular, in Examples 1-12, the STC conversion is not less than 25%, and the TCS selectivity is not less than 95%. In addition, the supported catalysts prepared in the examples of the present application can still maintain catalytic activity under 7 days of catalytic use, maintaining an STC conversion of not less than 15% and a TCS selectivity of not less than 90%.
[0144] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A supported catalyst, characterized in that The supported catalyst comprises a porous carrier and an active component supported on the porous carrier; the active component comprises a noble metal and a non-noble metal; wherein at least part of the noble metal elements are complexed with CO, XPS characterization shows that the supported catalyst has characteristic peaks at 300eV-320eV and 840eV-880eV; and / or, 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 35ppm-45ppm.
2. The supported catalyst according to claim 1, wherein The noble metal is mainly distributed in the inner layer of the porous carrier relative to the non-noble metal, and the non-noble metal is mainly distributed in the sub-surface layer of the porous carrier; Preferably, the noble metal is selected from one or more of rhodium, platinum, palladium and ruthenium; the non-noble metal is selected from one or more of nickel, iron, copper and cobalt; More preferably, the noble metal is selected from rhodium; and the non-noble metal is selected from nickel.
3. The supported catalyst according to claim 1 or 2, wherein The molar ratio of the noble metal to the non-noble metal is 1:5-50, preferably 1:8-35.
4. A supported catalyst according to any one of claims 1 to 3, wherein The non-noble metal is present in metallic form.
5. The supported catalyst according to any one of claims 1 to 4, wherein The porous carrier is selected from at least one of silicon oxide, molecular sieve and activated carbon; Preferably, the specific surface area of the porous carrier is 100 to 500 m 2 / g, micropore volume is 0.1-0.5cm 3 / g, and the mesopore volume is 0.1-0.8cm 3 / g, the mesopore volume accounts for 30-90vt%; More preferably, the specific surface area of the porous carrier is 200 to 400 m 2 / g, micropore volume is 0.1-0.3cm 3 / g, and the mesopore volume is 0.2-0.7cm 3 / g, and the mesopore volume accounts for 40-80vt%.
6. A method for preparing a supported catalyst according to any one of claims 1 to 5, wherein: The method includes: S1: loading a noble metal source and a CO donor on a porous carrier to prepare a first catalyst; S2: loading a non-precious metal source on the first catalyst to prepare a second catalyst; S3: drying and calcining the second catalyst to prepare a supported catalyst; The method enables at least part of the noble metal elements in the obtained supported catalyst to be complexed with CO; and XPS characterization shows that the supported catalyst has characteristic peaks at 300eV-320eV and 840eV-880eV; and / or, 17 MQ-MAS-NMR nuclear magnetic resonance detection results show that the supported catalyst has a characteristic peak at 35ppm-45ppm.
7. The preparation method according to claim 6, wherein: The method further comprises subjecting the porous carrier to an acid modification treatment or an alkali modification treatment; Preferably, the acid modification treatment comprises stirring the porous support and the acidic solution at 70-100°C for 10-25h, and then drying at 80-120°C for 8-15h and calcining at 400-600°C for 5-10h; more preferably, the acid in the acidic solution is selected from at least one of hydrochloric acid, sulfuric acid and nitric acid; Preferably, the alkali modification treatment comprises stirring the porous carrier and the alkaline solution at 70-100°C for 10-25h, and then drying at 80-120°C for 8-15h and calcining at 400-600°C for 5-10h; more preferably, the alkali in the alkaline solution is selected from at least one of sodium hydroxide, potassium hydroxide and ammonia water.
8. The preparation method according to claim 6 or 7, wherein In step S1, a solution of a noble metal source, a CO donor and a porous carrier are subjected to a first mixing treatment so that the noble metal source and the CO donor are supported on the porous carrier; Preferably, the reaction conditions of the first mixing treatment include: temperature of 20-80°C and time of 0.5-4h; More preferably, the noble metal source is selected from noble metal halides and / or nitrates, preferably rhodium chloride and / or rhodium nitrate; the solution concentration of the noble metal source is 0.001 to 0.1 mol / L, preferably 0.002 to 0.008 mol / L.
9. The preparation method according to any one of claims 6 to 8, wherein: The CO donor is selected from one or more of formic acid, sodium formate and methyl formate; Preferably, the molar ratio of the noble metal source calculated as the noble metal element to the CO donor is 1:1-10, preferably 1:1.5-6.
10. The preparation method according to any one of claims 6 to 9, wherein: In step S2, a solution of a non-precious metal source and the first catalyst are subjected to a second mixing treatment so that the non-precious metal source is loaded on a porous carrier; the molar ratio of the amount of the precious metal source to the amount of the non-precious metal source is 1:5-50, preferably 1:8-35; Preferably, the reaction conditions of the second mixing treatment include: temperature of 20-100°C and time of 1-5h; More preferably, the non-precious metal source is selected from non-precious metal halides and / or nitrates, preferably nickel chloride and / or nickel nitrate; the concentration of the solution of the non-precious metal source is 0.01-0.5 mol / L, preferably 0.15-0.3 mol / L.
11. The preparation method according to any one of claims 6 to 10, wherein: In step S2, it also includes adjusting the pH of the mixed solution of the non-precious metal source solution and the first catalyst to 7-12 and the temperature to 60-100° C.; Preferably, the pH adjusting agent is selected from at least one of aqueous ammonia, urea and sodium hydroxide.
12. The preparation method according to any one of claims 6 to 11, wherein: In step S3, the reaction conditions of the drying treatment include: temperature of 100-120°C and time of 10-12h; Preferably, the reaction conditions of the calcination treatment include: a temperature of 400-800° C. and a time of 4-8 hours.
13. The preparation method according to any one of claims 6 to 12, wherein: The method further comprises step S4: subjecting the supported catalyst to reduction treatment; Preferably, the reaction conditions of the reduction treatment include: introducing reducing gas at 300-600° C. for 2-5 hours.
14. A method for preparing trichlorosilane by hydrodechlorination of silicon tetrachloride, wherein: The catalyst used in the method is selected from the supported catalyst described in any one of claims 1 to 5.