Carbon intercalation iron phthalocyanine out-phase junction and preparation method and application thereof
The carbon-intercalated iron phthalocyanine heterojunction addresses the limitations of existing photo-Fenton technology by enhancing the generation of reactive oxygen species, achieving efficient degradation of pollutants through improved carrier separation and charge migration.
Patent Information
- Application Number
- CN202411200347.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing photo-Fenton technologies suffer from low photocatalyst carrier separation efficiency and slow charge migration rates, limiting their effectiveness in degrading pollutants.
A carbon-intercalated iron phthalocyanine heterojunction is prepared by calcining iron phthalocyanine with a nitrogen-containing precursor, forming a twin phase structure with a surface carbon layer to enhance internal carrier excitation and external charge migration through a built-in electric field.
The heterojunction catalyst achieves efficient degradation of pollutants by promoting carrier separation and charge transfer, resulting in high pollutant removal rates and improved catalytic activity.
Smart Images

Figure CN119076058A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of environmental materials, and in particular to a carbon-intercalated iron phthalocyanine heterojunction and a preparation method and application thereof. Background Art
[0002] Photo-Fenton technology uses sustainable clean energy to activate H2O2 to efficiently degrade pollutants, and has broad application prospects in environmental remediation. The excitation transition and migration of carriers on photocatalysts are crucial for the subsequent generation of reactive oxygen species. However, the vast majority (~90%) of photogenerated carriers will recombine and dissipate in the form of heat, which has become a bottleneck for the further application of photo-Fenton technology. Considering that internal carrier excitation transitions and external charge migration to reaction sites are necessary processes for carrier utilization, synchronously enhancing carrier separation and charge transfer is the key to improving the photo-Fenton reaction.
[0003] Junction engineering can introduce a built-in electric field (IEF) to promote the separation of photogenerated carriers, which is mainly divided into heterojunctions and homojunctions. Heterojunctions inherently contain different materials, which can easily lead to lattice mismatch, large contact resistance and band mismatch. The homojunction composed of the same material can effectively avoid the above defects, especially the heterojunction composed of different crystal forms of the same material, which can reduce the contact resistance by forming a semi-coherent interface. In addition, the introduction of a carbon layer on the surface of the heterojunction can improve the conductivity and further promote charge transfer. Therefore, by constructing a built-in electric field and carbon intercalation in the heterojunction, the internal excitation transition and external migration of carriers are simultaneously improved, thereby enhancing the generation of reactive oxygen species.
[0004] The Chinese invention patent application with patent publication number CN11692881A discloses a two-dimensional bismuth ferrite-cadmium sulfide composite photo-Fenton catalyst and its preparation method and application, wherein the heterojunction material composited with CdS nanoparticles and Bi2Fe4O9 nanosheets has a removal rate of only 90% for rhodamine B within 120 minutes, low charge transfer efficiency, and poor pollutant removal effect. The Chinese invention patent application with patent publication number CN 117548112A discloses a CdS@Si-α-Fe2O3 / ZnO heterostructure photo-Fenton catalyst and its preparation method and application, wherein the removal rate of ciprofloxacin by the ternary composite heterojunction catalyst is 95% within 60 minutes, the degradation time is long, and the catalytic activity is low.
[0005] The Chinese invention patent application with the patent publication number CN110743602A discloses a composite photocatalyst. By calcining the phthalocyanine metal monomers under an inert atmosphere, a thermal polymerization reaction occurs between the phthalocyanine metal monomers to generate a phthalocyanine metal polymer with more stable chemical properties; the phthalocyanine metal polymer and the g-C3N4 precursor are calcined twice under an inert atmosphere, and during the calcination process, the g-C3N4 precursor generates g-C3N4 quantum dots and forms a π-π conjugated bond system with the phthalocyanine metal polymer, so that the g-C3N4 quantum dots are evenly dispersed on the surface of the phthalocyanine polymer, preventing the g-C3N4 quantum dots from agglomerating and shielding the active sites; in addition, the metal element (MN4, M represents the metal element) of the phthalocyanine metal polymer skeleton coordinates with the N element in g-C3N4 to form a metal-N chelate (MN4-N), firmly anchoring the metal atoms, making them evenly dispersed in single atoms, effectively solving the problem of easy loss and easy agglomeration of metal ions. However, the problems of slow carrier transmission and high recombination rate still exist. The catalytic performance of the catalyst was evaluated by using the Fenton oxidation degradation method of Rhodamine B. The results showed that the removal rate of Rhodamine B was 99.89% after 90 minutes of reaction. The degradation time was relatively long and the catalytic activity was low. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the existing photo-Fenton technology, such as low photocatalyst carrier separation efficiency and slow charge migration rate, and to provide a carbon intercalation heterogeneous junction photo-Fenton catalyst and a preparation method thereof, which can achieve efficient degradation of pollutants in complex water bodies by simultaneously improving the internal excitation and external migration of photogenerated carriers.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a carbon-intercalated iron phthalocyanine heterogeneous junction, characterized in that iron phthalocyanine and a nitrogen-containing carbon precursor are calcined to induce a crystal phase change of the iron phthalocyanine to form an α-FePc and β-FePc twin phase, and the nitrogen-containing carbon precursor is carbonized to prepare an iron phthalocyanine heterogeneous junction coated with a surface carbon layer. The specific preparation steps include:
[0009] (1) mixing FePc with a nitrogen-containing carbon precursor to obtain a homogeneous mixed powder;
[0010] (2) The obtained mixed powder is placed in a tube furnace and calcined in an inert gas (nitrogen or argon) to obtain a carbon-intercalated iron phthalocyanine heterojunction.
[0011] Preferably, the nitrogen-carbon precursor is selected from any one or more of pyromellitic acid imide, phthalimide, aminophthalimide, nitrophthalimide and naphthalenetetracarboxylic acid imide.
[0012] Preferably, the mass ratio of iron phthalocyanine to the nitrogen-containing carbon precursor is: 1:(1-50).
[0013] Preferably, the calcination temperature is 200-500° C., the calcination time is 1-6 hours, and the heating rate is 1-10° C. / min.
[0014] Another object of the present invention is to provide a carbon-intercalated iron phthalocyanine heterojunction prepared by the method described in the present invention.
[0015] Another object of the present invention is to provide the use of the carbon-intercalated iron phthalocyanine heterojunction as a catalyst in removing organic pollutants in water.
[0016] In a specific application, the carbon intercalated iron phthalocyanine heterojunction is used as a photo-Fenton catalyst to remove pollutants from water.
[0017] In the field of water treatment, photo-Fenton technology can be used to treat various organic pollutants and some inorganic pollutants, such as benzene, phenol, dyes, pesticides, etc. In particular, in the photo-Fenton process, H2O2 produces hydroxyl radicals, which effectively remove pollutants such as pesticides, dyes, drugs, nitrobenzene and chlorophenol. In addition, Fenton reagents are also widely used in the treatment of industrial wastewater, including oily wastewater, printing and dyeing wastewater, coking wastewater, phenolic wastewater, and nitro wastewater.
[0018] In a specific example, the organic pollutants are selected from antibiotics, organic dyes, phenols, etc. For example, tetracycline, macrolide antibiotics, quinolone antibiotics (such as ciprofloxacin, ofloxacin), methylene blue, rhodamine B, methyl orange, phenol.
[0019] The treatment steps are as follows: after mixing the carbon intercalated phthalocyanine iron heterojunction with a solution containing organic pollutants, H2O2 is added, and a light source is turned on for reaction. The mass ratio of the organic pollutants, the carbon intercalated phthalocyanine iron heterojunction and H2O2 is preferably 1:(5-15):(1-20), and the reaction time is 5-40 minutes.
[0020] Technical effect: Compared with the existing technology, it has the following significant advantages:
[0021] (1) Compared with the traditional photo-Fenton catalyst, the carbon intercalation heterojunction photo-Fenton catalyst prepared by the present invention has a higher coordination of the heterojunction interface, which is conducive to the internal excitation transition of the carrier.
[0022] (2) Compared with traditional photo-Fenton catalysts, the carbon intercalation heterogeneous junction photo-Fenton catalyst prepared by the present invention has a surface carbon layer with intrinsic conductivity and can promote charge transfer.
[0023] (3) The carbon-intercalated iron phthalocyanine heterojunction of the present invention drives the internal carrier transition through the built-in electric field of the heterojunction, and at the same time promotes the migration of charges in combination with the surface carbon layer, thereby generating H2O2 through two-step hole oxidation activation. 1 O2 can achieve efficient degradation of various pollutants. The present invention breaks through the shortcomings of high carrier recombination rate and slow transfer rate of traditional photocatalysts, simultaneously improves the internal excitation and external migration of photogenerated carriers, develops efficient photo-Fenton technology, and has comprehensive technical and economic advantages such as high pollutant removal rate and strong anti-interference. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a transmission electron microscope image of the carbon intercalation heterogeneous junction α, β-FePc@C described in the present invention.
[0025] Figure 2 It is the degradation rate of tetracycline by the carbon intercalated heterogeneous α,β-FePc@C of the present invention in the presence of various inorganic salts.
[0026] Figure 3 The degradation rates of tetracycline by α-FePc, β-FePc, α,β-FePc heterojunction and carbon intercalation heterojunction α,β-FePc@C. DETAILED DESCRIPTION
[0027] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiment of the present invention. The various terms and phrases used in the present invention have the general meanings known to those skilled in the art. The present invention generally or specifically describes the materials and test methods used in the test. Although many materials and operating methods used to achieve the purpose of the present invention are well known in the art, the present invention is still described in as much detail as possible. The instruments, reagents, materials, etc. involved in the following embodiments, unless otherwise specified, are conventional instruments, reagents, materials, etc. existing in the prior art, and unless otherwise specified, are conventional experimental methods, detection methods, etc. existing in the prior art.
[0028] Example 1
[0029] a: 90 mg FePc and 450 mg pyromellitic acid diimide were placed in a ball mill at a speed of 3000 r / min for 10 min, and the mixture was ball milled to obtain a homogeneous powder;
[0030] b: The homogeneous powder was placed in a tube furnace, and the temperature was raised to 400°C at a rate of 5°C / min for calcination for 4 hours under the protection of argon atmosphere. After the reaction was completed, the tube furnace was cooled naturally to room temperature to obtain α,β-FePc@C, which was numbered A.
[0031] The transmission electron microscopy of the carbon intercalation heterogeneous α, β-FePc@C photocatalyst obtained in this example is shown in the attached figure. Figure 1 It can be seen that there is a heterogeneous interface composed of flake α-FePc and tubular β-FePc in α,β-FePc@C, and there is a surface carbon layer at the interface.
[0032] In this example, the obtained carbon intercalation heterogeneous α, β-FePc@C photocatalyst was used to degrade tetracycline. The specific experimental conditions were: 10 mg of the catalyst was placed in 50 mL of 20 mg / L tetracycline solution, and the adsorption-desorption equilibrium was reached after 30 minutes. Then 10 mM H2O2 was added and the xenon lamp was turned on to initiate the reaction. The degradation results of tetracycline are shown in FIG. Figure 3 As shown, the degradation rate of tetracycline can reach 96.7% within 15 minutes, and the degradation rate of tetracycline can reach 99.9% within 30 minutes.
[0033] Example 2
[0034] The same as Example 1, except that the calcination temperature was 600° C., and the catalyst obtained was numbered B. Under the same experimental conditions as Example 1, the degradation rate of tetracycline within 30 min was 56.7%.
[0035] Example 3
[0036] Same as Example 1, except that the heating rates were 1 and 10°C / min, respectively, and the obtained catalysts were numbered C and D. Under the same experimental conditions as Example 1, the degradation rates of tetracycline within 30 min were 91.6% and 95.8%, respectively.
[0037] Example 4
[0038] Same as Example 1, except that:
[0039] In step a, 250 mg of FePc and 250 mg of pyromellitic acid diimide were placed in a ball mill, and the resulting catalyst was numbered E. Under the same experimental conditions as in Example 1, the degradation rate of tetracycline within 30 min was 95.2%.
[0040] Example 5
[0041] Same as Example 1, except that:
[0042] In step a, 9 mg of FePc and 450 mg of pyromellitic acid diimide were placed in a ball mill, and the resulting catalyst was numbered F. Under the same experimental conditions as in Example 1, the degradation rate of tetracycline within 30 min was 91.8%.
[0043] Example 6
[0044] Same as Example 1, except that:
[0045] In step a, the carbon precursor is naphthalenetetracarboxylic acid acyl diimide. In step b, the calcination conditions are: heating rate 10°C / min, calcination temperature 500°C, and holding time 2h. The obtained catalyst is numbered G. Under the same experimental conditions as Example 1, the degradation rate of tetracycline within 30min is 97.2%.
[0046] Example 7
[0047] Same as Example 1, except that:
[0048] In step a, the carbon precursor is phthalimide. In step b, the calcination conditions are: heating rate 5°C / min, calcination temperature 350°C, holding time 3h. The obtained catalyst is numbered H. Under the same experimental conditions as Example 1, the degradation rate of tetracycline within 30min is 98.1%.
[0049] Example 8
[0050] Same as Example 1, except that:
[0051] In step a, the carbon precursor is aminophthalimide. In step b, the calcination conditions are: heating rate 1°C / min, calcination temperature 200°C, and holding time 1h. The obtained catalyst is numbered I. Under the same experimental conditions as Example 1, the degradation rate of tetracycline within 30min is 98.9%.
[0052] Example 9
[0053] Same as Example 1, except that:
[0054] In step a, the carbon precursor is nitrophthalimide. The obtained catalyst is numbered J. Under the same experimental conditions as in Example 1, the degradation rate of tetracycline within 30 minutes is 97.5%.
[0055] The degradation rate data of tetracycline by the carbon intercalation heterogeneous junction prepared in Examples 1-9 are shown in Table 1:
[0056] Table 1 Degradation rate of tetracycline by the catalysts prepared in Examples 1-9
[0057]
[0058] The above results show that at a calcination temperature of 200-500°C, 1-6h, and a heating rate of 1-10°C / min, different nitrogen-containing carbon precursors can achieve efficient degradation of tetracycline within 30 minutes. When the calcination temperature exceeds 500°C, the catalytic performance of the calcined product is significantly reduced. It is speculated that the carbon intercalation twin phase heterojunction structure of the present invention cannot be produced at an excessively high calcination temperature, and the built-in electric field of the heterojunction cannot be formed, thereby affecting the internal carrier transition and charge migration.
[0059] Example 10
[0060] Taking the carbon intercalation heterogeneous junction α, β-FePc@C photocatalyst prepared in Example 1 as an example, the degradation effect of ofloxacin in the presence of different inorganic salts was investigated. The degradation experimental conditions were the same as those in Example 1, except that 10 mM Cl - 、SO4 2- 、HCO3 - 、H2PO4 - and NO3 - The results are as follows Figure 2 As shown, the results showed that the degradation rates of tetracycline within 30 minutes were 98.2%, 98.2%, 96.3%, 94.4%, 9 and 98.5%, respectively, indicating that the catalyst can still effectively remove tetracycline in water under the presence of various inorganic salts.
[0061] Embodiment 11
[0062] Taking the carbon intercalated heterogeneous junction α, β-FePc@C photocatalyst prepared in Example 1 as an example, its degradation effect on different organic pollutants was investigated. The degradation experimental conditions were the same as in Example 1, except that the pollutant was changed to any one of ciprofloxacin, ofloxacin, methylene blue, rhodamine B and bisphenol A. Under the same experimental conditions as in Example 1, the degradation rates of ciprofloxacin, ofloxacin, rhodamine B and bisphenol A within 30 minutes were as shown in Table 2, which were 90.9%, 91.5%, 95.9% and 77.1%, respectively, indicating that the catalyst has high efficiency catalytic degradation performance for a variety of organic pollutants.
[0063] Table 2 Degradation rate of various organic pollutants by carbon intercalation heterogeneous junction
[0064] type Ciprofloxacin Ofloxacin Rhodamine B Bisphenol A Degradation rate (%) 90.9% 91.5% 95.9% 77.1%
[0065] Comparative Example 1
[0066] In order to study the difference between the single phase and heterogeneous phase of FePc for catalytic degradation of tetracycline, single phase (β-FePc) and heterogeneous phase (α,β-FePc) catalysts were prepared, and the catalytic effects of original FePc (α-FePc), β-FePc and α,β-FePc were compared. Figure 3 . The preparation method is the same as step b of Example 1 (without the mixing step with the nitrogen-containing carbon precursor), and the calcination temperature is 320°C to obtain α,β-FePc, and 425°C to obtain β-FePc. Under the same experimental conditions as Example 1, the degradation rates of tetracycline by α-FePc, β-FePc and α,β-FePc within 30 minutes of the obtained catalyst are 77.1%, 76.7% and 90.3%, respectively. Compared with the single crystal phase of α-FePc or β-FePc, the heterogeneous junction interface formed by α,β-FePc has the effect of significantly enhancing the internal excitation of photogenerated carriers, greatly improving the efficiency of rapid degradation of organic matter.
[0067] Comparative Example 2
[0068] In order to study the important role played by the surface carbon layer in the carbon intercalation heterogeneous junction α, β-FePc@C photocatalyst in the catalytic degradation of tetracycline, the catalytic effect difference between the heterogeneous junction catalyst without carbon layer (α, β-FePc, preparation method see Comparative Example 1) and the composite catalyst obtained in Example 1 was compared. Under the same experimental conditions as Example 1, the degradation rates of tetracycline by α, β-FePc and α, β-FePc@C within 30 minutes were 90.3% and 99.9%. The results show that the ability of carbon intercalation to promote charge migration can significantly improve the degradation rate of heterogeneous junctions for organic pollutants.
[0069] The above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing a carbon intercalated iron phthalocyanine heterojunction, characterized in that The iron phthalocyanine and the nitrogen-containing carbon precursor are calcined to induce the iron phthalocyanine to undergo a crystal phase change to form an α-FePc and β-FePc twin phase, and the nitrogen-containing carbon precursor is carbonized to prepare an iron phthalocyanine heterophase junction coated with a surface carbon layer. The specific preparation steps include: (1) mixing FePc with a nitrogen-containing carbon precursor to obtain a homogeneous mixed powder; (2) The obtained mixed powder is calcined in an inert gas to obtain a carbon-intercalated iron phthalocyanine heterojunction.
2. The preparation method according to claim 1, characterized in that The nitrogen-containing carbon precursor is selected from any one or more of pyromellitic acid imide, phthalimide, aminophthalimide, nitrophthalimide and naphthalenetetracarboxylic acid imide.
3. The preparation method according to claim 1, characterized in that The mass ratio of iron phthalocyanine to the nitrogen-containing carbon precursor is: 1:(1-50).
4. The preparation method according to claim 1, wherein the calcination temperature is 200-500°C, the calcination time is 1-6 hours, and the heating rate is 1-10°C / min.
5. A carbon intercalated iron phthalocyanine heterojunction, characterized in that The method is prepared by any one of claims 1 to 4.
6. Use of the carbon-intercalated iron phthalocyanine heterojunction according to claim 5 as a catalyst in removing organic pollutants in water.
7. The use according to claim 6, characterized in that The processing steps are as follows: after mixing the carbon-intercalated iron phthalocyanine heterojunction with a solution containing organic pollutants, H2O2 is added, and a light source is turned on to react.
8. The use according to claim 7, characterized in that The mass ratio of organic pollutants, carbon-intercalated phthalocyanine iron heterojunction and H2O2 is 1:(5-15):(1-20), and the reaction time is 5-40 minutes.
9. The use according to claim 8, characterized in that The organic pollutants are selected from antibiotics, organic dyes, and phenols.