Anti-cracking preparation process and mold for easy-to-tear cover

By forming a boss with pre-stretched mold and punching and curing on the easy-tear cover, the fracture problem caused by excessive tensile coefficient of the easy-tear cover mold in the prior art is solved, and the production success rate and product quality are improved .

CN119076778APending Publication Date: 2024-12-06HANGZHOU PANJI INTELLIGENT DEVICE CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202311289971.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-10-07
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the production process of easy-tear cover, due to the limitation of the tensile coefficient of the metal material, the stretch coefficient of the easy-tear cover mold in the prior art causes the inner hole to break, affecting production efficiency and product quality.

Method used

The boss is formed by a pre-stretched mold, and the removal opening and flange are formed on the boss through a punching mold, and the arc-shaped edge is curled by a pressing arc mold and a rolling mold to avoid the material under extremely small flange operation. Break, improve production success rate.

Benefits of technology

After pre-stretching and punching treatment, material breakage is avoided, the production success rate and product quality of the easy-to-tear cover are improved, and the stability and efficiency of the production process are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076778A_ABST
    Figure CN119076778A_ABST
Patent Text Reader

Abstract

The invention innovatively provides an anti-cracking preparation process of an easy-to-tear cover, which comprises the following steps of: forming a boss which protrudes outwards from a basic cover through tensile deformation; a cover ring with a central taking-out opening is formed on the boss through stamping machining, and a flange is formed between the cover ring and the edge of the boss; the flange is pressed towards the side where the boss is located to form an arc-shaped curled edge; and the arc-shaped curled edge is curled to form a curled part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of filtering equipment, and more particularly to a preparation process and a mold for preventing cracking of an easy-tear cover. Background Art

[0002] In the production process of the tear-off cover, the inner circle of the tear-off cover is punched, stretched and rolled, and then covered and sealed. In the rolling process, the cut surface is rolled, and a section is generated when the tool punches the inner hole of the tear-off cover. The inner hole passes through a stretching die to reach the arc required for rolling, and then the fracture surface is rolled inward by a rolling die. Since the tensile coefficient of the metal material has a limit, when the tensile coefficient of the tear-off cover die is too large, the fracture of the inner hole of the tear-off cover will be torn, and defective products will be easily produced during the rolling process, affecting the production efficiency of the tear-off cover. Summary of the invention

[0003] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a preparation process and a mold for preventing cracking of an easy-tear cover, so as to overcome the above-mentioned defects in the prior art.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A preparation process for preventing an easy-tear cover from cracking, comprising:

[0006] The base cover is stretched and deformed to form a boss that protrudes outward;

[0007] A cover ring having a central removal opening is formed by stamping on the boss, and a flange is formed between the cover ring and the edge of the boss;

[0008] Pressing the flange toward the side where the boss is located to form an arc-shaped curling edge;

[0009] The arc-shaped curled edge is rolled up to form a rolled portion.

[0010] Preferably, the angle between the boss and the edge of the base cover is 93.5°-95°, and the stretching height is 3.7-4.2 mm.

[0011] Preferably, the flange width is 0.7 mm.

[0012] Preferably, the radius of the rolled portion is 0.6-0.8 mm.

[0013] Preferably, the base cover is pre-punched before being stretched and deformed, and the pre-punched hole has a diameter smaller than the removal opening.

[0014] Preferably, it comprises a pre-stretching die, a punching die, an arc pressing die and a rolling die, and the pre-stretching die, the punching die, the arc pressing die and the rolling die are all located on the same production line.

[0015] Preferably, the pre-stretching die comprises an upper stretching die, a lower stretching die and a stretching platen, the upper stretching die is slidably arranged in the stretching platen, and stretching inclined surfaces are arranged relatively on the upper stretching die and the lower stretching die.

[0016] Preferably, the punching die comprises an upper punching die, a lower punching die and a punching plate, the upper punching die is slidably arranged on the punching plate, and the inner wall of the lower punching die is annularly provided with a first step surface, and the inner wall of the first step surface matches the upper punching die.

[0017] Preferably, the arc pressing mold includes an upper arc pressing mold, a lower arc pressing mold and an arc pressing plate, the upper arc pressing mold is slidably arranged in the arc pressing plate, the lower arc pressing mold is provided with an annular groove, and the upper arc pressing mold is provided with an annular protrusion, and the annular groove and the annular protrusion are arranged opposite to and matched with each other.

[0018] Preferably, the rolling mold comprises an upper rolling mold, a lower rolling mold and a rolling pressure plate, the lower rolling mold is slidably arranged in the rolling pressure plate, and a second step surface is annularly arranged on the upper surface of the lower rolling mold.

[0019] Beneficial effects of the present invention: The method for producing an easy-tear cover adopted by the present invention is to perform punching, arc pressing and curling after pre-stretching the inner hole of the base cover. During the pre-stretching process of the base cover, since there is no fracture surface, the material will not break within a certain tensile strength. The stretched base cover is punched, and the excess material on the stretched boss is cut off to form a removal opening, and the flange is curled to form a rolled-up portion. During the arc pressing and curling process, since only a very small flange is operated, it will not crack within the tensile coefficient inherent in the metal characteristics of the cross-section, thereby improving the success rate of easy-tear cover production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a basic cover structure diagram of the present invention;

[0021] Figure 2 It is a structural diagram of a stretching die of the present invention;

[0022] Figure 3 It is a structural diagram of the punching die of the present invention;

[0023] Figure 4 It is a structural diagram of the arc pressing die of the present invention;

[0024] Figure 5 It is a structural diagram of a rolling mold of the present invention.

[0025] Figure numerals: 1. base cover; 12. boss; 13. removal opening; 14. flange; 15. rolling portion; 21. upper stretching die; 211. stretching inclined surface; 22. lower stretching die; 23. stretching pressure plate; 31. upper punching die; 311. first step surface; 32. lower punching die; 33. punching pressure plate; 41. upper arc pressing die; 411. annular groove; 42. lower arc pressing die; 421. annular protrusion; 43. arc pressing pressure plate; 51. upper rolling die; 52. lower rolling die; 521. second step surface; 53. rolling pressure plate. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may also be a component centered. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may also be a component centered. When a component is considered to be "set on" another component, it may be directly set on the other component or there may also be a component centered. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0029] The embodiments of the present invention are further described in detail below with reference to the accompanying drawings:

[0030] like Figure 1-5As shown, the present invention provides a preparation process for preventing an easy-tear cover from cracking, comprising: using a pre-stretching die to stretch and deform a basic cover 1 to form an outwardly protruding boss 12 to achieve a pre-stretching effect; after the basic cover 1 is pre-stretched, a punching die is used to stamp and process the boss 12 to form a cover ring, that is, a removal opening 13 is punched in the center of the boss 12, and a flange 14 is provided between the removal opening 13 and the edge of the boss 12, ensuring that the flange 14 is provided between the removal opening 13 and the side wall of the boss 12, and an arc pressing die is used to press the flange 14 toward the side where the boss 12 is located, thereby forming an arc-shaped curling edge, which is convenient for rolling up the flange 14; using a rolling die, the arc-shaped curling edge is rolled up to form a rolled-up portion, and a rolling portion 15 is used to achieve the setting of the easy-tear cover while preventing the edge of the removal opening 13 from being too sharp, causing the removal opening 13 to scratch the user during use.

[0031] In the production process of the easy-tear cover, the base cover 1 is first pre-stretched to form a boss 12. In the pre-stretching process, since the base cover 1 has no fracture surface, the material will not easily break within a certain tensile coefficient. After the stretching is completed, a punching die is used to punch holes to flush out excess material to form a removal opening 13. The base cover 1 is pre-stretched before punching, which solves the problem that the traditional easy-tear cover is easily broken in the process of punching first and then stretching and curling, thereby improving the success rate of the easy-tear cover production.

[0032] The inclination angle between the boss 12 and the edge of the base cover 1 is 93.5°-95°. At the same time, the stretching height is 3.7-4.2 mm. While ensuring a certain height between the boss 12 and the base cover 1, there is a certain deflection angle between the boss 12 and the base cover 1.

[0033] The width of the flange 14 is 0.7 mm. During the punching process, there is a 0.7 mm flange 14 between the removal opening 13 and the edge of the boss 12. The flange 14 can be curled to prevent the edge of the removal opening 13 from scratching the user during use and affecting the use effect.

[0034] The radius of the rolled portion 15 is 0.6-0.8 mm. After the flange 14 is rolled, the side of the flange 14 is close to the boss 12 to achieve the rolling. While the side of the flange 14 is hidden to avoid scratches, the rolled portion 15 is used to cover the easy-tear film.

[0035] The base cover 1 is pre-punched before being stretched and deformed, and the diameter of the pre-punched hole is smaller than the removal opening 13. Before the base cover 1 is stretched, the base cover 1 is pre-punched, and the diameter of the pre-punched hole is smaller than the removal opening 13. In the production process of the easy-tear cover, the base cover 1 is stretched after being pre-punched. During the stretching process, cracks may exist around the pre-punched hole. The cracked part is cut off by punching to prevent the rolled-up part 15 from cracking.

[0036] A preparation mold for preventing an easy-tear cover from cracking comprises a pre-stretching mold, a punching mold, an arc pressing mold and a rolling mold, wherein the pre-stretching mold, the punching mold, the arc pressing mold and the rolling mold are sequentially arranged on a production line, and a conveyor belt for transmitting a basic cover 1 is provided, which passes through different molds in sequence to realize the production of the basic cover 1.

[0037] like Figure 2 As shown, the pre-stretching die includes an upper stretching die 21, a lower stretching die 22 and a stretching platen 23. The upper stretching die 21 is slidably arranged on the stretching platen 23. During use, the base cover 1 is placed on the lower stretching die 22, and the stretching platen 23 is placed on the lower stretching die 22. The lower stretching die 22 and the stretching platen 23 are used to fix the base cover 1 in the pre-stretching die. At the same time, the upper stretching die 21 is driven to slide in the stretching platen 23 to stretch the base cover 1 and form a boss 12. The bottom of the upper stretching die 21 is provided with a chamfer, and the chamfer radius is between 0.35-0.5mm. The lower stretching die 22 includes an upper chamfer and a lower chamfer, the upper chamfer radius is 0.4mm, and the lower chamfer radius is between 0.6-0.7mm. The upper stretching die 21 is provided with a chamfer, and the lower chamfer radius is between 0.6-0.7mm. Both the stretching die 21 and the lower stretching die 22 are provided with chamfers. The chamfers are used to ensure that after the boss 12 is stretched, the boss 12 is provided with chamfers to avoid affecting the usability due to overly sharp corners; the upper stretching die 21 and the lower stretching die 22 are relatively provided with stretching inclined planes 211, and the inclination angle of the stretching inclined plane 211 is 93.5°-95°. The stretching inclined plane 211 is used to ensure that there is a certain angle between the boss 12 and the base cover 1 during the stretching process; and in the mold closing process, a stretching die gap of 0.23-0.25mm is retained between the upper stretching die 21 and the lower stretching die 22. The stretching die gap is used to ensure the formation of the boss 12 during the stretching process. At the same time, it is avoided that the gap between the two is too small, resulting in deformation or too thinness of the boss 12, affecting the use effect.

[0038] like Figure 3As shown, the punching die includes an upper punching die 31, a lower punching die 32 and a punching plate 33. The upper punching die 31 is slidably arranged on the punching plate 33. A first step surface 311 is annularly arranged on the inner wall of the lower punching die 32, and the interior of the first step surface 311 matches the upper punching die 31. During use, the upper punching die 31 is driven to move downward and enter into the first step surface 311 to squeeze and punch the boss 12 to achieve the formation of the removal opening. The outer wall of the punching plate 33 matches the inner wall size of the boss 12. During use, the punching plate 33 is pressed on the inner wall of the boss 12 to fix the base cover 1, and there is a matching gap of 0.1 mm between the upper punching die 31 and the punching plate 33. While the punching plate 33 is used to limit the upper punching die 31, it does not affect the up and down movement of the upper punching die 31 in the punching plate 33.

[0039] like Figure 4 As shown, the arc pressing mold includes an upper arc pressing mold 41, a lower arc pressing mold 42 and an arc pressing plate 43. The upper arc pressing mold 41 is slidably set in the arc pressing plate 43. The lower arc pressing mold 42 is provided with an annular groove 411, and the upper arc pressing mold 41 is provided with an annular protrusion 421. The annular groove 411 and the annular protrusion 421 are arranged opposite to each other and matched. During use, the annular protrusion 421 is matched with the annular groove 411, and the annular protrusion 421 is pressed downward to achieve curling of the flange 14.

[0040] like Figure 5 As shown, the rolling mold includes an upper rolling mold 51, a lower rolling mold 52 and a rolling pressure plate 53. The lower rolling mold 52 is slidably set in the rolling pressure plate 53. The upper surface of the lower rolling mold 52 is annularly provided with a second step surface 521; a groove matching the annular protrusion 421 is provided on the second step surface 521. During the rolling process, the arc curling edge is set in the groove. During use, the arc curling edge is driven to move by pushing the lower rolling mold 52 to the side where the upper rolling mold 51 is located, thereby realizing the rolling of the arc portion.

[0041] The above are only preferred embodiments of the present invention. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A preparation process for preventing cracking of an easy-tear cover, characterized in that: include, The base cover (1) is stretched and deformed to form a boss (12) protruding outward; A cover ring having a central removal opening (13) is formed by stamping on the boss (12), and a flange (14) is formed between the cover ring and the edge of the boss (12); Pressing the flange (14) toward the side where the boss (12) is located to form an arc-shaped curling edge; The arc-shaped curled edge is rolled up to form a rolled portion (15).

2. The process for preparing the anti-cracking easy-tear cover according to claim 1, characterized in that: The edge angle between the boss (12) and the base cover (1) is 93.5°-95°, and the stretching height is 3.7-4.2 mm.

3. The process for preparing the anti-cracking easy-tear cover according to claim 1, characterized in that: The flange (14) has a width of 0.7 mm.

4. The process for preparing the anti-cracking easy-tear cover according to claim 1, characterized in that: The radius of the rolled portion (15) is 0.6-0.8 mm.

5. The process for preparing the anti-cracking easy-tear cover according to claim 1, characterized in that: Before the base cover (1) is stretched and deformed, it is pre-punched, and the diameter of the pre-punched hole is smaller than the removal opening (13). A preparation mold for preventing an easy-tear cover from cracking, characterized in that it comprises a pre-stretching mold, a punching mold, an arc pressing mold and a rolling mold, wherein the pre-stretching mold, the punching mold, the arc pressing mold and the rolling mold are all located on the same production line.

6. A mold for preventing cracking of an easy-tear cover according to claim 6, characterized in that: The pre-stretching die comprises an upper stretching die (21), a lower stretching die (22) and a stretching pressing plate (23); the upper stretching die (21) is slidably arranged in the stretching pressing plate (23); and stretching inclined surfaces (211) are arranged relatively on the upper stretching die (21) and the lower stretching die (22).

7. A mold for preventing cracking of an easy-tear cover according to claim 6, characterized in that: The punching die comprises an upper punching die (31), a lower punching die (32) and a punching plate (33); the upper punching die (31) is slidably arranged on the punching plate (33); and the inner wall of the lower punching die (32) is annularly provided with a first step surface (311); the inner wall of the first step surface (311) matches the upper punching die (31).

8. A mold for preventing the easy-tear cover from cracking according to claim 6, characterized in that: The arc pressing mold comprises an upper arc pressing mold (41), a lower arc pressing mold (42) and an arc pressing plate (43); the upper arc pressing mold (41) is slidably arranged in the arc pressing plate (43); the lower arc pressing mold (42) is provided with an annular groove (411); the upper arc pressing mold (41) is provided with an annular protrusion (421); the annular groove (411) and the annular protrusion (421) are arranged opposite to and matched with each other.

9. A mold for preventing cracking of an easy-tear cover according to claim 6, characterized in that: The rolling mold comprises an upper rolling mold (51), a lower rolling mold (52) and a rolling pressure plate (53); the lower rolling mold (52) is slidably arranged in the rolling pressure plate (53); and a second step surface (521) is annularly arranged on the upper surface of the lower rolling mold (52).

Citation Information

Patent Citations

  • Manufacturing method for tear-open lids, involves providing lid ring blank, which has beading and flange adjoined to beading flank, where flange with cutting edge borders opening of lid ring blank

    CH705595A1

  • Punch stretching mould

    CN101028638A

  • Method and device for producing tear-off lids and tear-off lid

    CN110366457A

  • Molding process of beer can screw cap

    CN110576116A

  • Method for producing a rolled edge

    CN111372700A