Forging method of low-direction sensitive 7085 series aluminum alloy forge piece

Through the forging method combining medium-temperature forging and differential temperature forging, the strong direction sensitivity problem of 7085 aluminum alloy forging in high-temperature forging is solved, and the 7085 aluminum alloy forging with high yield strength and low direction sensitivity is achieved, which improves its Weight loss benefits in aerospace and transportation sectors.

CN119076846AActive Publication Date: 2024-12-06CENT SOUTH UNIV

Patent Information

Application Number
CN202411244901.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-06
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

7085 aluminum alloy forgings have strong directional sensitivity during high-temperature forging, resulting in insufficient rheology performance at the center and inability to produce sufficient deformation during forging, limiting its weight loss benefits in aerospace and transportation fields.

Method used

Using a forging method combining medium-temperature forging and differential temperature forging, the uniform structure and performance of forging parts are achieved by controlling the size and forging temperature of the blank. The specific steps include heating insulation, medium-temperature forging, heating and re-insulation, hot forging and differential temperature forging to ensure The anisotropy of the forgings is reduced and the performance is uniform.

Benefits of technology

It significantly improves the yield strength and elongation of the forgings, reduces anisotropy, ensures consistent performance in different directions, and only slight cracks appear after C-ring stress corrosion, improving the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076846A_ABST
    Figure CN119076846A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of metal material processing, and relates to a forging method and application of a high-strength low-direction-sensitivity large-specification 7085-series aluminum alloy. The forging method comprises the combination of medium-temperature forging and differential-temperature forging. According to the forging method for reducing the direction sensitivity of the 7085 aluminum alloy forge piece and providing the high tensile property, the rheological property of the center of the forge piece can be improved, the recrystallization rate can be greatly increased so that the uniformity of the large-section forge piece in all directions can be improved, the comprehensive performance can be improved, and the direction sensitivity of the forge piece can be reduced. The process designed by the invention is particularly suitable for manufacturing the aluminum alloy material with the large and thick cross section specification, wherein the forging stock specification of the aluminum alloy material is 200mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal material processing and relates to a forging method of a 7085 aluminum alloy forging with high yield strength and extremely low directional sensitivity. Background Art

[0002] 7085 high-strength aluminum alloy is widely used in aerospace, military industry, transportation and other fields. In order to reduce weight, there is an urgent need for large-section thick 7085 series aluminum alloy forgings to support the overall manufacturing of large and complex parts. However, large-section thick 7085 series alloy forgings generally adopt high-temperature forging processes, which are prone to "dead zones", that is, the rheological properties of the central part are insufficient, and sufficient deformation cannot be produced during forging, resulting in strong directional sensitivity of the alloy forgings, which is mainly manifested in the elongation anisotropy index exceeding 50%, and the fracture toughness in different directions differing by more than 30%. At the same time, the high-directional stress corrosion performance is significantly lower than that in other directions, which limits the advantages of longitudinal and lateral performance in the design and restricts the improvement of comprehensive weight reduction benefits. In order to solve the problem of strong directional sensitivity, some research has been done in the prior art. For example, in patent 2023104747198, a multi-directional forging process is used with 7085 aluminum alloy as the processing object, such as: a 100×100×100mm 7085 aluminum alloy blank is not processed. The blank was heated to 460℃, kept warm for 1h, then cooled to 340℃, kept warm for 0.5h, and multi-directional forging was performed at 340℃. The unidirectional deformation in a single upsetting and drawing process was 30%. After forging, the L direction was forged from 100mm to 70mm to obtain a forging. Then, the forging was heated to 460℃, kept warm for 0.5h, and multi-directional forging was performed at 460℃. The temperature difference between the surface and the core was 20℃. The unidirectional deformation in a single upsetting and drawing process was 30%. After forging, the T direction was forged from 70mm to 50mm, and then air-cooled. The T74 forging core obtained by this technology has a tensile strength of 563MPa, a yield strength of 486MPa, and an elongation of 13.4% in the L direction; a tensile strength of 562MPa, a yield strength of 481MPa, and an elongation of 15.0% in the LS direction; and a tensile strength of 548MPa, a yield strength of 458MPa, and an elongation of 12.2% in the ST direction.

[0003] Based on the above research, the present invention has conducted a series of explorations to obtain 7085 forgings with higher yield strength and extremely low directional sensitivity, and has formed the present invention. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention derives for the first time a forging method for 7085 aluminum alloy with large size of E×E×E mm (wherein E ranges from 180 to 220), thereby obtaining an excellent product with high tensile strength, high yield strength, high elongation and extremely low anisotropy.

[0005] The present invention discloses a low-directional-sensitivity 7085 series aluminum alloy free forging, which uses a forging method combining medium-temperature forging and differential-temperature forging to control the forging structure. The alloy material and forging heat treatment include the following steps:

[0006] Step 1: Heating and insulation of forgings

[0007] The blank is heated to A°C, kept warm until the temperature difference between the core and the surface of the blank is less than 5°C, then cooled to B°C, kept warm at B°C until the temperature difference between the core and the surface of the blank is less than 5°C, and a forged part is obtained; the size of the blank is E×E×E mm, where E ranges from 180 to 220,

[0008] The value of A is 440-480, preferably 455-465; the value of B is 320-360, preferably 335-345;

[0009] The material of the blank is 7085 series aluminum alloy;

[0010] Step 2: Warm forging

[0011] The forging piece is subjected to medium temperature forging; during the medium temperature forging, the initial forging temperature is controlled to be B°C, and the forging piece is forged from Emm to Fmm; and a No. 1 intermediate forging piece is obtained; the F is 065 to 0.75E, preferably 0.7E;

[0012] Step 3: Heat and keep warm after medium temperature forging

[0013] The intermediate forging No. 1 obtained in step 2 is heated to C°C, and kept warm until the temperature difference between the core and the surface is less than 5°C; obtaining the intermediate forging No. 2; the value of C is 440-480, preferably 455-465;

[0014] Step 4: Hot forging and differential temperature forging

[0015] The intermediate forging No. 2 obtained in step 3 is subjected to hot forging and differential temperature forging treatment; the hot forging and differential temperature forging treatment are: starting hot forging at C°C, hot forging to 0.45-0.55E, preferably 0.5E; during the hot forging process, spraying coolant on the surface of the forging until the surface temperature reaches D°C, and the temperature of the core of the forging is greater than the temperature of the surface of the forging; the final forging temperature is greater than or equal to D°C; air cooling is performed after forging; and the product is obtained; the value of D is 360-400, preferably 375-385.

[0016] Preferably, the value range of E is 195-205, and more preferably 200.

[0017] The invention discloses a forging method for a low-directionally sensitive 7085 aluminum alloy, wherein the heat preservation time at A°C is 1.5h-2.5h.

[0018] The invention discloses a forging method for a low-directionally sensitive 7085 series aluminum alloy, wherein the heat preservation time at B°C is 1.5h-2.5h.

[0019] The invention discloses a forging method for a low-directionally sensitive 7085 series aluminum alloy, wherein the heat preservation time at C°C is 1.5h-2.5h.

[0020] As a preferred embodiment, the present invention provides a forging method for a low directional sensitive 7085 series aluminum alloy.

[0021] In step 1, the blank is heated to 460°C, kept at this temperature for 2 hours, and then lowered to 340°C and kept at this temperature for 2 hours;

[0022] In step 2, the initial forging temperature of the medium temperature forging is 340°C, and the forging is forged from 200mm to 140mm;

[0023] In step 3, after medium temperature forging, heat to 460°C and keep warm for 2h;

[0024] In step 4, the initial forging temperature of hot forging is 460°C, the forging is forged from 140mm to 100mm, and coolant is sprayed on the upper and lower surfaces during the hot forging process until the surface temperature reaches 380°C, so that the temperature of the central part is relatively high, the final forging temperature is not lower than 380°C, and air cooling is performed after forging. The present invention provides a forging method for a low-directionally sensitive 7085 series aluminum alloy; the product is subjected to heat treatment and aging treatment to obtain a finished product in T74 state; the heat treatment parameters are insulation at 460°C-480°C for 1.5h-2.5h, and water quenching; the T74 aging system is insulation at 110°C-130°C for 4h-10h, and then the temperature is raised to 150°C-170°C for insulation for 8h-12h.

[0025] The present invention discloses a forging method for a 7085 series aluminum alloy with low directional sensitivity; when the forged object is a 7085 aluminum alloy, the forging is subjected to T74 aging to obtain a product;

[0026] The difference in tensile strength between any two of the three directions L, LT and ST of the product is less than or equal to 13MPa; and the tensile strength in any one direction is greater than or equal to 535MPa;

[0027] The difference in yield strength between any two directions of the product in the three directions of L, LT and ST is less than or equal to 12MPa; and the yield strength in any direction is greater than or equal to 510MPa;

[0028] The difference in elongation between any two directions of the product in the three directions of L, LT and ST is less than or equal to 2.1%, and the elongation in any one direction is greater than or equal to 13.1%.

[0029] The invention discloses a forging method for a low-directionally sensitive 7085 series aluminum alloy. When the forged object is a 7085 aluminum alloy, the forging is subjected to T74 aging to obtain a product. After C-ring stress corrosion, only slight cracks are found. The conditions for the C-ring stress corrosion are: a pressure of 290 MPa and a time of 20 days.

[0030] Principles and advantages

[0031] During the forging process, the present invention greatly improves the yield strength of the product and reduces the anisotropy as much as possible through the coordination of size and forging process. The present invention adopts billets within the size range; the method of first medium-temperature forging and then differential temperature forging is adopted to make the forged forging structure and anisotropic properties more uniform; secondly, the surface of the forging after the temperature is reduced during the hot forging process of the present invention is still higher than D℃ (preferably greater than 380℃), ensuring that the surface is prevented from excessive recrystallization in subsequent treatments, resulting in reduced surface material properties. If the operation is not carried out according to the process sequence of the present invention, the performance difference of the final product in each direction will be affected to a certain extent. At the same time, if the size set by the present invention is not followed, even if the process is exactly the same, the anisotropy of the product will increase significantly, and even the strength of the product will decrease.

[0032] The advantages of the present invention are as follows: 1. The uniformity of organizational performance is improved through the recrystallization process; 2. The performance of the surface core is improved simultaneously; 3. The deformation uniformity of each part of the material is improved to reduce the directional sensitivity of the final performance of the material, and no lamellar grain structure with weak grain boundaries will appear in the high direction of the forging; 4. The process combination is simple to operate and can be implemented in industrial production, with production application value; 5. The directional sensitivity and toughness of the forging are significantly superior to those of the same type of forgings or thick plate aluminum alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the process used in Example 1;

[0034] Figure 2 The grain boundary and grain structure orientation difference distribution of the T74 state forging obtained in Example 1.

[0035] from Figure 1 The basic process of the process designed by the present invention can be seen in FIG.

[0036] from Figure 2 It can be seen that there is no lamellar grain structure with weak grain boundaries in the height direction of the forging. DETAILED DESCRIPTION

[0037] The following comparative examples and embodiments are intended to further illustrate the present invention rather than to limit the present invention.

[0038] The room temperature tensile test is carried out according to the national standard GB / T228-2002 to produce relevant standard tensile specimens.

[0039] Comparative Example 1-1:

[0040] Alloy composition: Al-7.28Zn-1.49Mg-1.68Cu-0.11Zr (wt.%)

[0041] The blank is 7085 aluminum alloy with a size of 150×200×200mm. The blank is heated to 460℃, kept at this temperature for 2h, and then put back to 460℃ for multiple hot forgings, forging from 100mm to 70mm; then the forging is heated to 460℃ again, kept at this temperature for 2h, and then forged from 70mm to 50mm, and air-cooled after forging.

[0042] Comparative Example 1-2:

[0043] Alloy composition: Al-7.28Zn-1.49Mg-1.68Cu-0.11Zr (wt.%)

[0044] The blank is 7085 aluminum alloy with a size of 300×300×300mm. The blank is heated to 460℃, kept at this temperature for 2h, then cooled to 340℃, kept at this temperature for 2h, pre-forged at 340℃, forged from 300mm to 210mm; then the forging is heated to 460℃, kept at this temperature for 2h, forged from 210mm to 150mm, and the cooling liquid is evenly sprayed on each surface during the forging process until the surface temperature reaches 380℃, and air-cooled after forging.

[0045] Embodiment 1:

[0046] Alloy composition: Al-7.28Zn-1.49Mg-1.68Cu-0.11Zr (wt.%)

[0047] The blank is 7085 aluminum alloy with a size of 200×200×200mm. The blank is heated to 460℃, kept at this temperature for 2h, then cooled to 340℃, kept at this temperature for 2h, and pre-forged for multiple passes at 340℃, forging from 200mm to 140mm; then the forging is heated to 460℃, kept at this temperature for 2h, and hot forged at 460℃, forging from 140mm to 90mm. During the hot forging process, the upper and lower surfaces are sprayed with coolant until the surface temperature reaches 380℃, and air-cooled after forging.

[0048] The materials prepared in the comparative example and the embodiment were heat treated to the T74 state, and the heat treatment process parameters were 470°C / 2h, water quenching, and after water quenching, the T74 aging system of 120°C / 7h+160°C / 10h was used for double-stage aging. The performance comparison of the materials prepared by the conventional forging process and the invention process in three directions is shown in Table 1.

[0049] Table 1 Comparison of performance in various directions between comparative examples and embodiments

[0050]

Claims

1. A low directional sensitivity 7085 series aluminum alloy free forging, characterized by: The forging method combining medium temperature forging and differential temperature forging is used to control the forging structure. The alloy material and forging heat treatment include the following steps: Step 1: Heating and insulation of forgings The blank is heated to A°C, kept warm until the temperature difference between the core and the surface of the blank is less than 5°C, then cooled to B°C, kept warm at B°C until the temperature difference between the core and the surface of the blank is less than 5°C, and a forged part is obtained; the size of the blank is E×E×Emm, where E ranges from 180 to 220. The value of A is 440-480, preferably 455-465; the value of B is 320-360, preferably 335-345; The material of the blank is 7085 series aluminum alloy; Step 2: Warm forging The forging piece is subjected to medium temperature forging; during the medium temperature forging, the initial forging temperature is controlled to be B°C, and the forging piece is forged from Emm to Fmm; and a No. 1 intermediate forging piece is obtained; the F is 065 to 0.75E, preferably 0.7E; Step 3: Heat and keep warm after medium temperature forging The intermediate forging No. 1 obtained in step 2 is heated to C°C, and kept warm until the temperature difference between the core and the surface is less than 5°C; obtaining the intermediate forging No. 2; the value of C is 440-480, preferably 455-465; Step 4: Hot forging and differential temperature forging The intermediate forging No. 2 obtained in step 3 is subjected to hot forging and differential temperature forging treatment; the hot forging and differential temperature forging treatment are: starting hot forging at C°C, hot forging to 0.45-0.55E, preferably 0.5E; during the hot forging process, spraying coolant on the surface of the forging until the surface temperature reaches D°C, and the temperature of the core of the forging is greater than the temperature of the surface of the forging; the final forging temperature is greater than or equal to D°C; air cooling is performed after forging; and the product is obtained; the value of D is 360-400, preferably 375-385.

2. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 1, characterized in that: The value range of E is 195~205.

3. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 1, characterized in that: The insulation time at A℃ is 1.5h-2.5h.

4. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 1, characterized in that The insulation time at B℃ is 1.5h-2.5h.

5. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 1, characterized in that: The insulation time at C℃ is 1.5h-2.5h.

6. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 1, characterized in that: When the size of the blank is: 200×200×200mm, In step 1, the blank is heated to 460°C, kept at this temperature for 2 hours, and then lowered to 340°C and kept at this temperature for 2 hours; In step 2, the initial forging temperature of the medium temperature forging is 340°C, and the forging is forged from 200mm to 140mm; In step 3, after medium temperature forging, heat to 460°C and keep warm for 2h; In step 4, the initial forging temperature of hot forging is 460°C, the forging is forged from 140 mm to 100 mm, and coolant is sprayed on the upper and lower surfaces during the hot forging process until the surface temperature reaches 380°C, so that the temperature of the center is relatively high, and the final forging temperature is not lower than 380°C.

7. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 6, characterized in that: After forging, the product is air-cooled and then heat-treated and aged to obtain a finished product in T74 state; the heat treatment parameters are: keeping at 460℃-480℃ for 1.5h-2.5h, and water quenching; the T74 aging system is: keeping at 110℃-130℃ for 4h-10h, and then heating to 150℃-170℃ for 8h-12h.

8. The low directional sensitivity 7085 series aluminum alloy free forging according to claim 7, characterized in that: When the forging object is 7085 aluminum alloy, it is aged by T74 after forging; Get the product; The difference in tensile strength between any two of the three directions L, LT and ST of the product is less than or equal to 13MPa; and the tensile strength in any one direction is greater than or equal to 535MPa; The difference in yield strength between any two directions of the product in the three directions of L, LT and ST is less than or equal to 12MPa; and the yield strength in any direction is greater than or equal to 510MPa; The difference in elongation between any two directions of the product in the three directions of L, LT and ST is less than or equal to 2.1%, and the elongation in any one direction is greater than or equal to 13.1%.

Citation Information

Patent Citations

  • Forging method of 7000 series aluminum alloy

    CN108856614A

  • Forming method for improving three-direction performance of aluminum alloy

    CN112439857A

  • Forging method and application of low-direction sensitive 7xxx series aluminum alloy

    CN113441665A

  • Forging method and application of high-toughness low-anisotropy 7-series aluminum alloy

    CN116511392A

Cited By

  • Forging method and application of exfoliation-corrosion-resistant 7-series aluminum alloy