Additive manufacturing precipitation strengthening type medium / high-entropy alloy with high dislocation density and preparation method

Through the combination of cyclic deep-cooling prefatigue and heat treatment, combined with specific scanning strategies, the problem of weakening of the strengthening mechanism caused by dislocation recovery in additive manufacturing is solved, and the high dislocation density and alloy strength are significantly improved, achieving good strength and plasticity. Combined.

CN119076977APending Publication Date: 2024-12-06INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411208017.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In additive manufacturing, the formation of secondary reinforcement phase depends on long-term heat treatment, resulting in dislocation recovery and weakening of the reinforcement mechanism. Plastic processing methods such as forging will destroy the shape of the part, making it difficult to maintain alloy strength while maintaining high dislocation density. .

Method used

By adopting a combination of cyclic deep-cooling prefatigue treatment and heat treatment, the dislocation density is improved by introducing a large number of dislocations into the alloy and suppressing its recovery, and combining the scanning strategy of each layer with an angle of 90° to the previous layer, ensuring that Thermal stability and alloy strength of dislocations.

Benefits of technology

It significantly improves the dislocation density and strength of the alloy, maintains good thermal stability and strong plasticity combination, avoids shape damage, and is suitable for additive manufacturing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076977A_ABST
    Figure CN119076977A_ABST
Patent Text Reader

Abstract

The invention discloses a high-dislocation-density additive manufacturing precipitation strengthening type medium / high-entropy alloy and a preparation method, and belongs to the field of metal material manufacturing. According to the method, on the basis of a pre-fatigue deformation strategy, cyclic cryogenic pre-fatigue treatment is conducted on the additive manufacturing alloy before heat treatment, dislocation is promoted to proliferate massively, and dense cross faults are introduced. And the dislocation is pinned by the cross-layer dislocation, so that extremely high thermal stability is shown, almost all the dislocation is reserved in the thermal treatment process, and the dislocation density in the alloy is greatly improved. According to the strategy, the dislocation strengthening effect of the metal material is fully exerted, and the strength of the alloy is greatly improved. In addition, the method is easy to operate, has no damage to the appearance of the material, and is adaptive to an additive manufacturing technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metal material manufacturing, and in particular to a method for preparing an additively manufactured precipitation-strengthened alloy with a high dislocation density. Background Art

[0002] Additive manufacturing is a material preparation technology based on the discrete-stacking principle, which is driven by the three-dimensional data of parts to directly manufacture parts. Compared with traditional preparation methods, it has incomparable advantages in forming complex structural parts, saving costs and reducing preparation cycles. During the forming process, the large temperature gradient and high cooling rate cause the additive manufacturing alloy to form ultra-high density dislocations, stimulate the dislocation strengthening mechanism, and greatly improve the strength of the additive manufacturing alloy. Precipitation-strengthened medium / high entropy alloy is a new type of metal material designed based on the second phase precipitation strengthening strategy. It shows an excellent combination of strength and plasticity. In the future, it will become one of the most important structural materials in the fields of aerospace, shipbuilding and precision instruments. The use of additive manufacturing technology to prepare precipitation-strengthened medium / high entropy alloys is expected to perfectly combine the advantages of additive manufacturing technology with the excellent performance of materials, achieving the effect of "1+1>2".

[0003] In order to achieve this goal, a key problem needs to be solved. That is, the formation of secondary strengthening phases depends on long-term heat treatment. In this process, dislocations in additive manufacturing alloys are annihilated on a large scale due to static recovery, which greatly weakens the dislocation strengthening mechanism, which will inevitably cause serious loss of alloy strength. Although plastic processing methods such as forging and rolling can introduce high-density dislocations into the alloy to make up for the loss of dislocation strengthening effect, they will destroy the shape of the parts. Therefore, a preparation method for additive manufacturing precipitation-strengthened medium / high entropy alloys that does not affect the dimensional accuracy of the alloy and can maintain a high dislocation density is urgently needed. Summary of the invention

[0004] In this context, the present invention starts from the two perspectives of "increasing source" and "saving cost" and provides a method for preparing additively manufactured precipitation-strengthened medium / high entropy alloys with high dislocation density. By introducing a large number of dislocations into the alloy and suppressing the dislocation recovery process, the dislocation density in the alloy is effectively increased, the dislocation strengthening effect is enhanced, and a huge improvement in the strength of the alloy is achieved.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a high dislocation density additively manufactured precipitation-strengthened alloy comprises the following steps:

[0007] Step 1: Preparation of precipitation-strengthened alloy by additive manufacturing;

[0008] Step 2: After the alloy obtained in step 1 is cooled to room temperature, it is immediately subjected to cyclic deep-cold pre-fatigue treatment;

[0009] Step 3: heat treating the alloy obtained in step 2.

[0010] Preferably, the additively manufactured precipitation-strengthened alloy in step 1 is prepared by adopting a scanning strategy in which the scanning direction of each layer forms an angle of 90° with the previous layer.

[0011] Preferably, the cyclic deep cooling pre-fatigue treatment in step 2 comprises the following steps:

[0012] (1) cooling the alloy to -150°C to -196°C (preferably -170°C to -196°C, more preferably -185°C to -196°C), and keeping the temperature for 5 to 7 hours (preferably 6 to 7 hours, more preferably 6 to 6.5 hours);

[0013] (2) After the insulation is completed, the alloy is immediately placed in a drying oven at 90-120°C (preferably 100-110°C) and heated for 5-10 minutes (preferably 5-6 minutes);

[0014] (3) Repeat steps (2) and (3) for 3 to 6 times to complete the cyclic deep cryogenic pre-fatigue treatment.

[0015] Preferably, the heat treatment temperature in step three is 700-900°C (preferably 700-800°C, more preferably 700-750°C), the holding time is 180-240min (preferably 180-200min), and water quenching is performed after completion.

[0016] Preferably, the dislocation density in the alloy subjected to cyclic deep cold pre-fatigue treatment is not less than 6.8×10 14 m -2 , the cross stacking fault density is not less than 3.9×10 14 m -2 .

[0017] Preferably, after heat treatment, the dislocation density in the alloy is not less than 6.3×10 14 m -2 , the volume fraction of the precipitated phase is not less than 15%.

[0018] The constituent elements of the medium entropy alloy include two or more of Al, Ti, Ta, and V and two or more of Co, Cr, and Ni; the constituent elements of the high entropy alloy include two or more of Al, Ti, Ta, and V and three or more of Fe, Co, Cr, Ni, and Cu.

[0019] The nominal atomic percentage of the medium entropy alloy is three or more of Co 31.33at.%, Cr 31.33at.%, Ni31.33at.%, Al 3.01at.%, and Ti 3at.%; the nominal atomic percentage of the high entropy alloy is five or more of Fe 23.75at.%, Co 23.75at.%, Cr 23.75at.%, Ni 23.75at.%, Al2.5at.%, and Ti2.5at.%.

[0020] The dislocation density of the alloy after cyclic deep cold pre-fatigue treatment is not less than 6.8×10 14 m -2 , the cross stacking fault density is not less than 3.9×10 14 m -2 ; After heat treatment, the dislocation density in the alloy is not less than 6.3×10 14 m -2 , the volume fraction of the precipitated phase is not less than 15%.

[0021] The additive manufacturing precipitation-strengthened neutral and / or high entropy alloy with high dislocation density prepared by the preparation method of the present invention.

[0022] This method is based on the pre-fatigue deformation strategy. Before heat treatment, the additive manufacturing alloy is subjected to cyclic deep cold pre-fatigue treatment, which promotes the proliferation of dislocations and introduces dense cross-stacked faults. The dislocations are pinned by cross-stacked faults, showing extremely high thermal stability, and can be almost completely retained during the heat treatment process, thereby greatly increasing the dislocation density in the alloy. This strategy gives full play to the dislocation strengthening effect of metal materials and greatly improves the strength of the alloy. In addition, this method is simple to operate, non-destructive to the material shape, and is suitable for additive manufacturing technology.

[0023] The advantages and beneficial effects of the present invention are as follows:

[0024] (1) The method of the present invention adopts a scanning strategy in which the scanning direction of each layer is at a 90° angle to the previous layer. The additive manufacturing precipitation-strengthened high-entropy alloy is prepared, which effectively avoids the superposition and concentration of residual stresses and can introduce dislocations and cross-stack faults more uniformly and densely.

[0025] (2) The method described in the present invention is simple to operate. A large number of dislocations and cross-stacking faults are introduced into the alloy without damaging the alloy's appearance. The cross-stacking faults have a pinning effect on dislocations, thereby improving the thermal stability of the alloy and inhibiting the recovery of dislocations. The strength of the additively manufactured precipitation-strengthened alloy is greatly improved, and a good combination of strength and plasticity is achieved.

[0026] (3) The method described in the present invention can introduce a large number of crystal defects into the alloy, thereby promoting the formation of the second phase, enhancing the precipitation strengthening effect, and further strengthening the alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the scanning path used in additive manufacturing of the present invention.

[0028] Figure 2 (CoCrNi) in step 1 of Example 1 94 Transmission electron microscopy (TEM) image of Al3Ti3 alloy.

[0029] Figure 3 For step 2 (CoCrNi) in Example 1 94 Transmission electron microscopy (TEM) image of Al3Ti3 alloy.

[0030] Figure 4 For step 3 (CoCrNi) in Example 1 94 Transmission electron microscopy (TEM) image of Al3Ti3 alloy.

[0031] Figure 5 For Example 1 (CoCrNi) 94 X-ray diffraction (XRD) pattern and scanning electron microscope (SEM) image of Al3Ti3 alloy.

[0032] Figure 6 For Example 1 (CoCrNi) 94 Room temperature tensile stress-strain curve of Al3Ti3 alloy.

[0033] Figure 7 For Comparative Example 1 (CoCrNi) 94 Transmission electron microscope image of Al3Ti3 alloy.

[0034] Figure 8 For Comparative Example 1 (CoCrNi) 94 X-ray diffraction (XRD) pattern and scanning electron microscope (SEM) image of Al3Ti3 alloy.

[0035] Fig. 9 For Comparative Example 1 (CoCrNi) 94 Room temperature tensile stress-strain curve of Al3Ti3 alloy.

[0036] Fig.10 For Comparative Example 2 (CoCrNi) 94 Transmission electron microscope image of Al3Ti3 alloy.

[0037] Fig.11For Comparative Example 2 (CoCrNi) 94 Room temperature tensile stress-strain curve of Al3Ti3 alloy. DETAILED DESCRIPTION

[0038] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, so as to better understand the principles and advantages of the present invention.

[0039] Example 1

[0040] This example prepares a high dislocation density additive manufacturing L12 phase precipitation strengthening (CoCrNi) 94 Al3Ti3 medium entropy alloy, comprising the following steps:

[0041] Step 1: Using 304 stainless steel as the substrate, additive manufacturing (CoCrNi) is performed layer by layer using a Direct Energy Deposition (DE) device equipped with a YDFL-4000CO2 fiber laser. 94 Al3Ti3 medium entropy alloy. The nominal atomic percentage of the medium entropy alloy is Co31.33at.%, Cr 31.33at.%, Ni 31.33at.%, Al3.01at.%, Ti 3at.%. The process parameters of the direct energy deposition are: laser power 800W, scanning speed 480mm / min, spot diameter 2.8mm, powder feeding rate 10g / min, overlap rate of adjacent scanning paths on each layer is 40%, layer thickness is 0.3mm, scanning path see Figure 1 a (one layer is moved back and forth in the length direction, and the next layer is moved back and forth in the width direction, alternately, and the scanning directions of the two adjacent layers are perpendicular, that is, the scanning direction of each layer is at a 90° angle to the previous layer.) The size of the prepared medium-entropy alloy is 70mm×50mm×30mm (length×width×thickness).

[0042] Step 2: After the alloy obtained in step 1 is cooled to room temperature, it is immediately subjected to cyclic deep cooling pre-fatigue treatment, and the specific operation includes the following steps:

[0043] S1: Cool the alloy to -196°C and keep it at this temperature for 6 hours;

[0044] S2: After the heat preservation is completed, the alloy is immediately placed in a drying oven at 100°C and heated for 10 minutes;

[0045] S3: Repeat steps S1 and S2 for a total of 4 times to complete the cyclic deep cold pre-fatigue treatment.

[0046] Step 3: heat treat the alloy obtained in step 2 at 700°C for 180 minutes.

[0047] The microstructure of the alloys obtained in step 1, step 2 and step 3 was observed using a transmission electron microscope.

[0048] Figure 2 , 3 4 are transmission electron microscope images of the alloy microstructure obtained in step 1, step 2, and step 3, respectively. Dislocation is a line defect, which appears as a curve in the transmission electron microscope image; stacking fault is a surface defect, which appears as a straight line in the transmission electron microscope image. Figure 3 As shown in the figure, after cyclic deep cold pre-fatigue treatment, dislocations in the alloy proliferate in large quantities and form dense cross stacking faults. The density of cross stacking faults calculated by ImageJ software is 5.4×10 14 m -2 The dislocation is pinned by the stacking fault, which improves the thermal stability of the dislocation. Figure 4 As shown in the figure, the alloy still maintains a high dislocation density after heat treatment.

[0049] The alloys obtained in step 1, step 2 and step 3 were subjected to XRD analysis, with a scanning angle 2θ ranging from 20° to 100° and a scanning speed of 2° / min.

[0050] Figure 5 (a) is the XRD spectrum of the alloys obtained in the three steps. Curves 1, 2, and 3 correspond to the XRD spectra of the alloys obtained in step 1, step 2, and step 3, respectively. The dislocation density of the three alloys was calculated using the Williamson-Hall method.

[0051] Table 1 shows the dislocation density (m) of the alloys obtained in step 1, step 2 and step 3. -2 )

[0052] alloy Step 1 Step 2 Step 3 Dislocation density <![CDATA[4.7×10 14 ]]> <![CDATA[8.2×10 14 ]]> <![CDATA[7.5×10 14 ]]>

[0053] The calculation results show that after cyclic deep cold pre-fatigue treatment, the dislocation density in the alloy increased by 74%. After heat treatment, the dislocation density only decreased by 8%, but the dislocation density was increased by 60% compared with the alloy obtained in step one.

[0054] The precipitation strengthening phase of the alloy obtained in step 3 was observed using the Inlens mode of a scanning electron microscope. Figure 5 As shown in (b), dense secondary strengthening phases were precipitated in the alloy matrix after heat treatment. The volume fraction of the secondary strengthening phases was calculated to be 18.2% using ImageJ software.

[0055] The tensile mechanical properties of the alloy obtained in step 3 were tested at room temperature using an ETM105D universal testing machine at a strain rate of 1×10 -3 / s, three samples were tested in total, and all the test samples were sampled on the plane parallel to the 304 stainless steel. Figure 6 As shown, the alloy has a yield strength of 1249 MPa and a plasticity of 14%, demonstrating extremely high strength and good strength-plasticity matching.

[0056] Comparative Example 1

[0057] This comparative example prepared an additive manufacturing L12 phase precipitation strengthening (CoCrNi) 94 Al3Ti3 medium entropy alloy, comprising the following steps:

[0058] Step 1: Using 304 stainless steel as the substrate, use a Directed Energy Deposition (DE) device equipped with a YDFL-4000CO2 fiber laser to prepare (CoCrNi) 94 Al3Ti3 medium entropy alloy. The nominal atomic percentage of the medium entropy alloy is Co 31.33at.%, Cr 31.33at.%, Ni 31.33at.%, Al 3.01at.%, Ti3at.%. The process parameters of the direct energy deposition are: laser power 800W, scanning speed 480mm / min, spot diameter 2.8mm, powder feeding rate 0.5r / min, overlap rate of adjacent scanning paths on each layer is 40%, layer thickness is 0.3mm, scanning path see Figure 1 a. The size of the prepared medium-entropy alloy is 70 mm×50 mm×30 mm (length×width×thickness).

[0059] Step 2: heat treat the alloy obtained in step 1 at 700°C for 180 minutes.

[0060] This comparative example adopts the same microstructure characterization, XRD analysis and mechanical property testing methods as Example 1.

[0061] Figure 7 This is a transmission electron microscope image of the alloy microstructure obtained in step 2. The results show that the dislocation density of the alloy is severely reduced. Figure 8 (a) is the XRD pattern of the alloy obtained in step 2. According to the XRD pattern, the dislocation density of the alloy is calculated to be 1.6×10 14 m -2 , heat treatment reduces the dislocation density of the alloy by 66%. Figure 8 (b) is the SEM image of the alloy obtained in step 2. It can be seen that the density of the secondary precipitation phase is relatively low. The volume fraction of the secondary strengthening phase calculated by ImageJ software is 13.8%. Fig. 9 This is the tensile stress-strain curve of the alloy obtained in step 2. The yield strength of the alloy is only 873 MPa and the plasticity is 15%.

[0062] Comparative Example 2

[0063] This comparative example prepared an additive manufacturing L12 phase precipitation strengthening (CoCrNi) 94 Al3Ti3 medium entropy alloy, comprising the following steps:

[0064] Step 1: Using 304 stainless steel as the substrate, use a Directed Energy Deposition (DE) device equipped with a YDFL-4000CO2 fiber laser to prepare (CoCrNi) 94 Al3Ti3 medium entropy alloy. The nominal atomic percentage of the medium entropy alloy is Co 31.33at.%, Cr 31.33at.%, Ni 31.33at.%, Al 3.01at.%, Ti3at.%. The process parameters of the direct energy deposition are: laser power 800W, scanning speed 480mm / min, spot diameter 2.8mm, powder feeding rate 0.5r / min, overlap rate of adjacent scanning paths on each layer is 40%, layer thickness is 0.3mm, scanning path see Figure 1 b (one layer is prepared by reciprocating left and right in the length direction, and the next layer is also prepared by reciprocating left and right in the length direction, that is, the scanning direction of each layer is the same as that of the previous layer.) The size of the prepared medium entropy alloy is 70mm×50mm×30mm (length×width×thickness).

[0065] Step 2: After the alloy obtained in step 1 is cooled to room temperature, it is immediately subjected to cyclic deep cooling pre-fatigue treatment, and the specific operation includes the following steps:

[0066] S1: Cool the alloy to -196°C and keep it at this temperature for 6 hours;

[0067] S2: After the heat preservation is completed, the alloy is immediately placed in a drying oven at 100°C and heated for 10 minutes;

[0068] S3: Repeat steps S1 and S2 for a total of 4 times to complete the cyclic deep cold pre-fatigue treatment.

[0069] Step 3: heat treat the alloy obtained in step 2 at 700°C for 180 minutes.

[0070] Fig.10 This is the transmission electron microscope image of the alloy obtained in step 2. After cyclic deep cold pre-fatigue treatment, only unidirectional stacking faults are formed in the alloy, and no dense cross stacking faults are formed. The stacking fault density calculated by ImageJ software is only 0.9×10 14 m -2 .

[0071] Fig. 9 This is the tensile stress-strain curve of the alloy obtained in step 3. The strength of the alloy is only 985 MPa and the plasticity is only 10%.

[0072] Example 2

[0073] This example prepares an additive manufacturing L12 phase precipitation strengthening (FeCoCrNi) 95 Al 2.5 Ti 2.5 High entropy alloy, the process and conditions are the same as in Example 1, except that the atomic percentages of the nominal components of the high entropy alloy are Fe 23.75 at.%, Co 23.75 at.%, Cr 23.75 at.%, Ni 23.75 at.%, Al 2.5 at.%, and Ti 2.5 at.%.

[0074] After cyclic deep-cold pre-fatigue treatment, the cross stacking fault density is 4.2×10 14 m -2 ; After heat treatment, the dislocation density of the alloy is 6.5×10 14 m -2 ; The volume fraction of the precipitated phase is 15.6%.

[0075] Example 3

[0076] This example prepares a high dislocation density additive manufacturing L12 phase precipitation strengthening (CoCrNi) 94 The Al3Ti3 medium entropy alloy has the same process and conditions as Example 1, except that in step 2 S1, the alloy is cooled to -170°C and kept warm for 7 hours.

[0077] After cyclic deep cold pre-fatigue treatment, the cross stacking fault density is 3.5×10 14 m -2 ; After heat treatment, the dislocation density of the alloy is 5.8×10 14 m -2 ; The volume fraction of the precipitated phase is 14.8%.

[0078] Example 4

[0079] This example prepares a high dislocation density additive manufacturing L12 phase precipitation strengthening (CoCrNi) 94 The Al3Ti3 medium entropy alloy has the same process and conditions as Example 1, except that in step 3 the alloy is kept at 800°C for 240 minutes.

[0080] After cyclic deep-cold pre-fatigue treatment, the cross stacking fault density is 5.4×10 14 m -2 ; After heat treatment, the dislocation density of the alloy is 2.5×10 14 m -2 ; The volume fraction of the precipitated phase is 19.1%.

[0081] Through the above examples and comparative examples, it can be seen that the method for preparing a precipitation-strengthened medium / high entropy alloy with high dislocation density of the present invention can effectively increase the dislocation density in the precipitation-strengthened medium / high entropy alloy, and also increase the density of the secondary precipitation strengthening phase, so that the strength of the alloy is greatly improved, while the plasticity remains almost unchanged, maintaining a good combination of strength and plasticity. This preparation method provides a new strengthening idea for additive manufacturing precipitation-strengthened medium / high entropy alloys, nickel-based high-temperature alloys, and aluminum alloys.

Claims

1. A method for preparing a high dislocation density additively manufactured precipitation-strengthened medium / high entropy alloy, characterized in that: The preparation method comprises the following steps: Step 1: Additive manufacturing to prepare precipitation-strengthened medium or high entropy alloys; Step 2: After the alloy obtained in step 1 is cooled to room temperature, it is immediately subjected to cyclic deep-cold pre-fatigue treatment; Step 3: heat treating the alloy obtained in step 2.

2. The preparation method according to claim 1, characterized in that: In the step 1, the additively manufactured precipitation-strengthened alloy is prepared by adopting a scanning strategy in which the scanning direction of each layer forms a 90° angle with the previous layer.

3. The preparation method according to claim 1, characterized in that: The cyclic deep cooling pre-fatigue treatment in step 2 comprises the following steps: (1) cooling the alloy to -150 to -196°C (preferably -170 to -196°C, more preferably -185 to -196°C), and keeping the temperature for 5 to 7 hours (preferably 6 to 7 hours, more preferably 6 to 6.5 hours); (2) After the insulation is completed, the alloy is immediately placed in a drying oven at 90-120°C (preferably 100-110°C) and heated for 5-10 minutes (preferably 5-6 minutes); (3) Repeat steps (2) and (3) for 3 to 6 times to complete the cyclic deep cryogenic pre-fatigue treatment.

4. The preparation method according to claim 1, characterized in that: The heat treatment temperature in step 3 is 700-900° C. (preferably 700-800° C., more preferably 700-750° C.), the heat preservation time is 180-240 min (preferably 180-200 min), and water quenching is performed after completion.

5. The preparation method according to claim 1, characterized in that: The constituent elements of the medium entropy alloy include two or more of Al, Ti, Ta, and V and two or more of Co, Cr, and Ni; the constituent elements of the high entropy alloy include two or more of Al, Ti, Ta, and V and three or more of Fe, Co, Cr, Ni, and Cu.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The dislocation density of the alloy after cyclic deep cold pre-fatigue treatment is not less than 6.8×10 14 m -2 , the cross stacking fault density is not less than 3.9×10 14 m -2 ; After heat treatment, the dislocation density in the alloy is not less than 6.3×10 14 m -2 , the volume fraction of the precipitated phase is not less than 15%.

7. An additively manufactured precipitation-strengthened neutral and / or high entropy alloy with high dislocation density prepared by the preparation method according to any one of claims 1 to 6.