Method for repairing surface defects of polycarbonate liquid level observation window
By cleaning, drying, surface treatment and additive coating and curing the polycarbonate level observation window, the problem of surface defects is solved, the service life is extended and maintenance costs is reduced, and the efficient repair effect is achieved.
Patent Information
- Application Number
- CN202411211660.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The polycarbonate level observation window is prone to defects such as wear, scratches, corrosion or cracks during use, which leads to the need to be replaced and increases the maintenance cost of the company.
Provides a repair method including cleaning, drying, detecting surface defects, surface treatment (polishing, grinding or grinding) according to the defect type, cleaning and baking, additive coating and UV curing, to improve structural strength and Wear resistance.
The service life of the polycarbonate level observation window has been extended, and the maintenance costs of the enterprise have been reduced. The repaired product performance is close to new products, reducing maintenance costs by 30% to 40%.
Smart Images

Figure CN119078239A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of repairing material surface defects, and in particular to a method for repairing surface defects of a polycarbonate liquid level observation window. Background Art
[0002] Polycarbonate liquid level observation windows are widely used in EMUs. They are important parts of the EMU equipment compartment. They are mainly used to seal and observe the liquid levels of various liquids on the EMU trains to ensure the normal operation and safety of the EMU trains. Due to the harsh operating environment of polycarbonate liquid level observation windows, after the EMU has traveled a certain mileage, polycarbonate liquid level observation windows are prone to wear and cracking, forming scratches, corrosion or cracks on their surfaces. These defects seriously affect the performance of polycarbonate liquid level observation windows, and usually the defective polycarbonate liquid level observation windows are directly replaced. However, the cost of polycarbonate liquid level observation windows is high, which will lead to high maintenance costs for enterprises. Summary of the invention
[0003] In response to the problems pointed out in the background technology, in some embodiments, a method for repairing surface defects of a polycarbonate liquid level observation window is provided to solve the problem that the polycarbonate liquid level observation window in the prior art needs to be replaced after surface defects occur, which results in high maintenance costs for the enterprise.
[0004] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0005] In some embodiments, the present invention provides a method for repairing surface defects of a polycarbonate liquid level observation window, comprising the following steps:
[0006] Step (1), cleaning and drying the polycarbonate liquid level observation window;
[0007] Step (2), detecting the depth of the surface defect of the polycarbonate liquid level observation window treated in step (1), and determining the type of the surface defect according to the depth of the surface defect;
[0008] Step (3), performing surface treatment on the polycarbonate liquid level observation window according to the type of the surface defect;
[0009] Step (4), cleaning and baking the polycarbonate liquid level observation window treated in the above step (3);
[0010] Step (5), performing additive coating on the surface of the polycarbonate liquid level observation window treated in the above step (4), and performing curing treatment with ultraviolet light;
[0011] Step (6), testing the polycarbonate liquid level observation window treated in the above step (5) to determine whether its performance is qualified.
[0012] In some embodiments of the present application, the types of surface defects are divided into mild defects, moderate defects and severe defects; in step (3), the surface treatment process of the polycarbonate liquid level observation window is as follows:
[0013] When the surface defect is a slight defect, a polishing agent is applied to the surface of the polycarbonate liquid level observation window and a polishing process is performed using a sponge pad;
[0014] When the type of the surface defect is a medium defect, firstly, an abrasive is applied to the surface of the polycarbonate liquid level observation window, and a grinding process is performed using a wool wheel; then, a polishing agent is applied to the ground surface of the polycarbonate liquid level observation window, and a polishing process is performed using a sponge pad;
[0015] When the type of surface defect is a severe defect, first, the surface of the polycarbonate liquid level observation window is ground with sandpaper; second, the surface of the polycarbonate liquid level observation window after the grinding is coated with abrasive, and the window is ground with a wool wheel; third, the surface of the polycarbonate liquid level observation window after the grinding is coated with polishing agent, and the window is polished with a sponge pad.
[0016] In some embodiments of the present application, the temperature of the polishing process is 50-80°C, and the temperature of the grinding process and the lapping process are both 30-60°C.
[0017] In some embodiments of the present application, the coating thickness of the polishing agent and the grinding agent is 0.5-1 mm.
[0018] In some embodiments of the present application, the process of grinding the surface of the polycarbonate liquid level observation window with sandpaper comprises the following steps:
[0019] First, the surface defects are removed by grinding with coarse sandpaper;
[0020] Then, fine sandpaper is used to grind and remove fine lines around the surface defect until the surface defect becomes hazy.
[0021] In some embodiments of the present application, the polishing agent includes one or a combination of aluminum oxide, sodium oxide, silicon dioxide or iron oxide.
[0022] In some embodiments of the present application, the abrasive includes one or a combination of boron carbide, paraffin, sheep oil or turpentine.
[0023] In some embodiments of the present application, the depth of the surface defect is d;
[0024] When d<0.01mm, the type of surface defect is a slight defect;
[0025] When 0.01mm≤d<0.1mm, the type of the surface defect is a moderate defect; when 0.1mm≤d≤0.5mm, the type of the surface defect is a severe defect.
[0026] In some embodiments of the present application, the baking temperature in step (4) is 90-100° C. and the baking time is 50-60 min.
[0027] In some embodiments of the present application, the additively coated material is self-healing polycarbonate;
[0028] The self-healing polycarbonate comprises the following raw materials in parts by weight: 100-140 parts of modified silica sol, 200-240 parts of vinyl polysiloxane-polycarbonate block polymer, 8-100 parts of propylene glycol, 300-400 parts of tetrahydrofuran, and 20-25 parts of benzoin dimethyl ether.
[0029] Compared with the prior art, the present invention has the following advantages or beneficial effects: by cleaning and drying the polycarbonate liquid level observation window, surface defects can be completely exposed, which is convenient for subsequent detection of the depth of surface defects and determination of the type of surface defects; then the polycarbonate liquid level observation window is surface treated according to the type of surface defects, and different types of surface defects can be improved; the polycarbonate liquid level observation window after surface treatment is cleaned and baked, cleaning can remove surface impurities, and baking can remove residual stress of the polycarbonate liquid level observation window and reduce deformation; finally, the surface of the baked polycarbonate liquid level observation window is additively coated and ultraviolet light cured to improve the structural strength; the repair method of the present application can ensure the performance of the polycarbonate liquid level observation window under normal use, extend the service life of the polycarbonate liquid level observation window, and help reduce the maintenance cost of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 This is a schematic structural diagram of the polycarbonate liquid level observation window provided by the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0033] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.
[0034] In some embodiments, the present disclosure provides a method for repairing surface defects of a polycarbonate liquid level observation window, the method comprising the following steps:
[0035] Step (1), at room temperature, using an ultrasonic cleaning machine to clean the polycarbonate liquid level observation window, the ultrasonic cleaning time is 10 minutes, and a cleaning agent dedicated to polycarbonate is selected to remove dirt on the surface of the polycarbonate liquid level observation window; wherein the ultrasonic cleaning machine uses a sinusoidal wave band, and the sinusoidal wave can generate stable vibration, which is conducive to cavitation and straight flow in the cleaning process, thereby effectively removing dirt, and then rinsing with clean water;
[0036] Next, the cleaned polycarbonate liquid level observation window is dried to remove surface moisture.
[0037] Step (2), detecting the depth of the surface defect of the polycarbonate liquid level observation window treated in step (1), and determining the type of the surface defect according to the depth of the surface defect.
[0038] Step (3), performing surface treatment on the polycarbonate liquid level observation window according to the type of surface defects. The main purpose of the surface treatment is to polish away the defects on the surface of the polycarbonate liquid level observation window so that the surface of the polycarbonate liquid level observation window becomes smoother.
[0039] Step (4), ultrasonically cleaning the polycarbonate liquid level observation window treated in the above step (3) to remove impurities remaining from the grinding treatment; then, wiping it clean and baking it to remove the residual stress of the polycarbonate liquid level observation window after the surface treatment.
[0040] Residual stress is the internal stress generated in the polycarbonate liquid level observation window during the surface treatment process due to external constraints or internal uneven temperature changes. If this stress state is not effectively removed, it may cause the polycarbonate liquid level observation window to deform, thereby affecting the accuracy of shape and size. Therefore, removing residual stress is of great significance to extending the service life of the polycarbonate liquid level observation window.
[0041] Specifically, the method for removing residual stress is mainly heat treatment, for example, by changing the internal structure of the material through heating and cooling processes, thereby eliminating or reducing residual stress.
[0042] The equipment used for baking in the above step (4) can be an electric heating blast drying oven or the like.
[0043] Step (5), performing additive coating on the surface of the polycarbonate liquid level observation window treated in the above step (4) to form a coating, and curing the coating with ultraviolet light.
[0044] The above treatment can enhance the strength of the surface coating of the polycarbonate liquid level observation window, thereby improving the wear resistance, corrosion resistance and fatigue resistance of the polycarbonate liquid level observation window; the coating can also increase the hardness and strength of the surface material of the polycarbonate liquid level observation window, and improve the service life and durability of the polycarbonate liquid level observation window.
[0045] The method for repairing surface defects of a polycarbonate liquid level observation window according to the embodiment of the present disclosure prolongs the service life of the polycarbonate liquid level observation window by 60% to 80%, and reduces the maintenance cost of the enterprise by 30% to 40%.
[0046] Specifically, by cleaning and drying the polycarbonate liquid level observation window, the surface defects can be completely exposed, which is convenient for subsequent detection of the depth of the surface defects of the polycarbonate liquid level observation window and determination of the type of the surface defects.
[0047] The polycarbonate liquid level observation window is surface treated according to the type of surface defects, so that different types of surface defects can be improved.
[0048] The polycarbonate liquid level observation window after surface treatment is subjected to ultrasonic cleaning and baking treatment. Cleaning can remove surface impurities, and baking can remove residual stress of the polycarbonate liquid level observation window after surface treatment and reduce deformation.
[0049] The surface of the polycarbonate liquid level observation window after baking is additively coated to improve the structural strength; the repair method of the present application can ensure the performance of the polycarbonate liquid level observation window under normal use, extend the service life of the polycarbonate liquid level observation window, and help reduce the maintenance cost of the enterprise.
[0050] Step (6) inspects the polycarbonate liquid level observation window treated in the above step (5) to determine whether its performance is qualified.
[0051] In some embodiments of the present application, the types of surface defects are divided into mild defects, moderate defects and severe defects. By grading the surface defects, it is convenient to match the corresponding repair process according to the type of surface defects for repair; in step (3), the surface treatment process of the polycarbonate liquid level observation window is as follows:
[0052] The first case: When the type of surface defect is a slight defect, install a polishing disc on the polishing machine, stick the sponge pad to the polishing disc, and apply polishing agent on the surface of the polycarbonate liquid level observation window, and use the sponge pad for polishing.
[0053] At the beginning of polishing, place the polishing disc gently and slowly on the surface of the polycarbonate liquid level observation window, and gradually and evenly increase the pressing force of the polishing disc; during the polishing process, the polishing disc moves back and forth in a straight line on the working surface, and the last pass of the polishing disc on the working surface should be pressed tightly to one-third of the previous pass to avoid vacant polishing positions; at the same time, it is carried out alternately up and down according to the area of the polycarbonate liquid level observation window; at the end of polishing, the pressing force of the polishing disc is gradually and evenly reduced, and finally the polishing disc is gently and slowly raised from the working surface, and the surface of the polycarbonate liquid level observation window becomes transparent again after polishing.
[0054] During the polishing process, the work surface needs to be kept dry.
[0055] The second case: When the type of surface defect is a moderate defect, first, install a grinding disc on the polishing machine, and then stick the wool wheel to the grinding disc; coat the surface of the polycarbonate liquid level observation window with abrasive, and use the wool wheel to grind until the surface of the polycarbonate liquid level observation window is restored to be flat and smooth, and ultrasonically clean and dry the ground polycarbonate liquid level observation window.
[0056] At the beginning of grinding, the grinding disc needs to be gently and slowly placed on the surface of the polycarbonate liquid level observation window, and the pressing force of the grinding disc needs to be gradually and evenly increased; during the grinding process, the grinding disc moves back and forth in a straight line on the working surface, and the last pass of the grinding disc on the working surface should be pressed tightly to one-third of the previous pass to avoid vacant grinding positions; at the same time, it is carried out alternately up and down according to the area of the polycarbonate liquid level observation window; until the surface returns to the smooth platform, at the end of grinding, the pressing force of the grinding disc needs to be gradually and evenly reduced, and finally the grinding disc is gently and slowly raised from the working surface.
[0057] Next, the surface of the polycarbonate liquid level observation window after the grinding process is fully coated with a polishing agent, and a sponge pad is used for polishing. The above polishing steps are repeated, which will not be repeated here.
[0058] The third case: When the type of surface defect is a severe defect, first, install the grinding disc on the polishing machine, and then stick the sandpaper onto the grinding disc, and use the sandpaper to grind the surface of the polycarbonate liquid level observation window until the surface defect is removed, and then clean and dry the ground polycarbonate liquid level observation window.
[0059] Secondly, replace the grinding disc and stick the wool wheel, and apply abrasive to the surface of the polycarbonate liquid level observation window and repeat the above grinding steps, which will not be repeated here, until the surface of the polycarbonate liquid level observation window is restored to be flat and smooth, and the ground polycarbonate liquid level observation window is cleaned and dried.
[0060] Again, replace the polishing disc and stick the sponge pad, apply polishing agent on the surface of the ground polycarbonate liquid level observation window, polish it with the sponge pad, and repeat the above polishing steps, which will not be repeated here, until the surface of the polycarbonate liquid level observation window becomes transparent again.
[0061] It should be noted that during the grinding and grinding process, there is a lot of frictional heat generated on the surface of the polycarbonate liquid level observation window, and the thermal performance of the polycarbonate material is very poor. It is necessary to connect a resistive temperature sensor on its surface to measure the surface temperature of the polycarbonate liquid level observation window during the grinding and grinding process, and use water cooling to control the temperature rise. This can not only remove surface defects to the greatest extent, but also reduce the impact of excessive temperature on sintering of the surface of the polycarbonate liquid level observation window.
[0062] The frictional heat generated during the polishing process is less, so air cooling is sufficient. The work surface needs to be kept dry during polishing.
[0063] When the surface defects of the polycarbonate liquid level observation window exceed 0.5mm in depth, it is difficult to maintain its complete performance through repair.
[0064] In some embodiments of the present application, the temperature of the polishing process is 50-80°C, and the temperature of the grinding process and the lapping process are both 30-60°C.
[0065] In the disclosed embodiments, the temperature of the grinding and lapping treatments is not easy to be too high, which can avoid local burns on the working surface and reduce the internal thermal stress caused by high temperature, which is beneficial to maintaining geometric accuracy and surface quality; during the grinding and lapping process, high temperature may increase the surface roughness of the polycarbonate liquid level observation window, and maintaining an appropriate processing temperature helps to control the quality of the polycarbonate liquid level observation window and avoid the adverse effects of abrasive chips and sand generated by high temperature on the surface.
[0066] In some embodiments of the present application, the coating thickness of the polishing agent and the grinding agent is 0.5-1 mm.
[0067] In the disclosed embodiments, the coating thickness of the polishing agent and the grinding agent should not be too thick or too thin. If the coating thickness of the polishing agent and the grinding agent is too thick, it will directly lead to an increase in cost. Secondly, it may cause more impurities, increase processing costs, and easily cause pollution. If the coating thickness of the polishing agent and the grinding agent is too thin, it will lead to frequent polishing and grinding, which may easily cause surface aging. Secondly, if the coating thickness of the polishing agent and the grinding agent is uneven, it may affect the surface quality of the polycarbonate liquid level observation window.
[0068] In some embodiments of the present application, the process of grinding the surface of the polycarbonate liquid level observation window with sandpaper includes the following steps:
[0069] First, the surface defects are removed by grinding with coarse sandpaper; the grit size of the coarse sandpaper is F300-F500; the sandpaper has a larger grit size and can quickly remove most of the surface defects, laying a foundation for subsequent grinding, avoiding excessive time and energy in subsequent stages, and thus improving work efficiency.
[0070] Exemplarily, the grit size of the coarse sandpaper is F310, F320, F350, F400, F450, F500, etc.
[0071] Then, fine sandpaper is used to grind and remove fine lines around the surface defect until the surface defect is mist-like. The grit size of the fine sandpaper is F700-F1200; the grit size of the sandpaper is small, which further improves the surface quality of the polycarbonate liquid level observation window.
[0072] Exemplarily, the grit size of the fine sandpaper is F750, F800, F850, F900, F950, F1000, etc.
[0073] In some embodiments of the present application, the polishing agent includes one or a combination of aluminum oxide, sodium oxide, silicon dioxide or iron oxide.
[0074] Specifically, the polishing agent is mainly formulated into an aluminum oxide polishing liquid. The aluminum oxide polishing liquid has good polishing efficiency, uniform particle size, good suspension and dispersibility, and does not scratch the surface of the polished object. The main components of the aluminum oxide polishing liquid are aluminum oxide particles and stabilizers. The size of the aluminum oxide particles determines the abrasive properties of the polishing liquid. Smaller particles provide a more delicate polishing effect, while larger particles are suitable for polishing rough surfaces. The stabilizer plays a role in stabilizing and adjusting the pH value in the polishing liquid, preventing the aluminum oxide particles from agglomerating and depositing during the polishing process, and maintaining the uniformity and stability of the polishing liquid. At the same time, the stabilizer can also adjust the pH of the polishing liquid to meet the polishing requirements of different materials.
[0075] In some embodiments of the present application, the proportions of the components in the aluminum oxide polishing liquid are as follows: 99.95% aluminum oxide, 0.03% sodium oxide, 0.01% silicon dioxide, 0.01% iron oxide, and the rest is water.
[0076] During polishing, aluminum oxide usually exists in the form of fine particles, which can cut and abrade the surface of the material during the polishing process, making the surface of the observation window smoother, smoother and more transparent.
[0077] The alumina polishing liquid is prepared in an alkali-resistant container, and water is first added to the alkali-resistant container, and then the polishing agent is added, and the polishing liquid is ground and stirred until it is in a suspended state.
[0078] In some embodiments of the present application, the abrasive includes one or a combination of boron carbide, paraffin, sheep oil or turpentine.
[0079] Exemplarily, the abrasive is boron carbide abrasive paste, and the proportions of the components of the boron carbide abrasive paste are as follows: 76% boron carbide, 12% paraffin, 10% sheep oil, and 2% turpentine.
[0080] The boron carbide grinding paste can be prepared by mixing the above-mentioned various components together and stirring. During grinding, the boron carbide grinding paste can reduce the friction coefficient, reduce the heat and wear during the grinding process, and make the surface of the observation window flat and smooth after grinding.
[0081] In some embodiments of the present application, the grinding disc and the polishing disc are 6-inch rubber discs.
[0082] In some embodiments of the present application, the grinding disc is a rubber disc with an outer diameter of 4 inches.
[0083] In some embodiments of the present application, the sandpaper disc is also called velvet-backed disc sandpaper, and a wavy transverse structure made of a felt material is provided on one side used for grinding, and gravel is spread on the wavy transverse structure, and its back side is sandpaper roll velvet for easy sticking on the grinding disc.
[0084] In some embodiments of the present application, the depth of the surface defect is d. When d<0.01mm, the type of the surface defect is a mild defect; when 0.01mm≤d<0.1mm, the type of the surface defect is a moderate defect; when 0.1mm≤d≤0.5mm, the type of the surface defect is a severe defect.
[0085] In some embodiments of the present application, the baking temperature in step (4) is 90-100° C. and the baking time is 50-60 min to facilitate the removal of internal stress.
[0086] In some embodiments of the present application, the additively coated material is self-healing polycarbonate;
[0087] The self-healing polycarbonate comprises the following raw materials in parts by weight: 100 to 140 parts of modified silica sol, 200 to 240 parts of vinyl polysiloxane-polycarbonate block polymer, 8 to 100 parts of propylene glycol, 300 to 400 parts of tetrahydrofuran, and 20 to 25 parts of benzoin dimethyl ether.
[0088] In some embodiments, the thickness of the self-repairing polycarbonate coating is consistent with the depth of the corresponding surface defect, which is helpful to repair the polycarbonate liquid level observation window to its original state as much as possible.
[0089] In some embodiments of the present application, in step (6), the repaired polycarbonate liquid level observation window is subjected to a comprehensive performance test and a type test, wherein the comprehensive performance test is mainly for the surface hardness and light transmittance; the type test mainly includes: temperature change test, impact vibration test, gravel impact resistance test, ball pressure hardness test, penetration test, fatigue strength test, detection of prohibited and restricted substances, appearance quality and size detection.
[0090] Among them, the temperature change test is to immerse the test piece in hot water at (90±2)℃ for 10 minutes, and then immediately put it into ice water at 0℃ for 3 minutes after taking it out. Repeat this twice, then wipe the surface of the test piece dry and check whether there is any damage or warping.
[0091] Shock vibration test: The test is carried out under the vibration and shock amplitude in the direction specified by Class 1, Level A in IEC 61373. The panels shall not be permanently deformed or damaged, and the working surface shall be able to withstand various vibrations and shocks during normal operation of the EMU.
[0092] Gravel impact resistance test: The requirements and methods shall be carried out in accordance with Article 5.3.4 of TB / T1451.
[0093] Ball pressure hardness test: The ball pressure hardness of the panel is required to be no less than 115N / mm 2; The maximum penetration force is not less than 5500N at 23℃ and not less than 6400N at -40℃.
[0094] Penetration test: The light transmittance is required to be no less than 90%, and both sides are treated with UV curing after molding.
[0095] Fatigue strength test: It requires that the observation panel should be able to withstand ±2500Pa fatigue pneumatic load without damage. The surface should have good wear resistance and weather resistance. In normal use environment (wind, sand, rain, snow, etc.) and cleaning and maintenance conditions, the observation window surface will not be affected by wear and scratches that affect the perspective observation function.
[0096] Prohibited and restricted substances testing: is carried out in accordance with TB / T3139 standards.
[0097] Appearance quality and size: The inspection requires that the surface is smooth and flat, colorless, clear and transparent, and must not have cracks, scratches, warping, deformation, astigmatism, etc., and must comply with the requirements of the new drawings and technical conditions.
[0098] Example 1: A polycarbonate liquid level observation window with the deepest depth of surface defects of 0.005 mm is selected. First, the polycarbonate liquid level observation window is ultrasonically cleaned and dried; a polishing agent with a thickness of 0.5 mm is evenly coated on the surface of the polycarbonate liquid level observation window, and it is polished with a sponge pad until the surface of the polycarbonate liquid level observation window is transparent again; then it is ultrasonically cleaned and dried, and then placed in an electric blast drying oven at 90°C and baked for 60 minutes to remove residual stress; after cooling to room temperature, a self-repairing polycarbonate coating with a thickness of 0.005 mm is coated on the surface of the polycarbonate liquid level observation window, and cured with ultraviolet light; finally, performance testing is performed.
[0099] Example 2: A polycarbonate liquid level observation window with the deepest depth of surface defects of 0.015 mm was selected. First, the polycarbonate liquid level observation window was ultrasonically cleaned and dried; then, an abrasive with a thickness of 0.5 mm was evenly coated on the surface of the polycarbonate liquid level observation window, and the abrasive was grinded with a wool wheel until the surface of the polycarbonate liquid level observation window was restored to be flat and smooth, and then the polycarbonate liquid level observation window was ultrasonically cleaned and dried;
[0100] Then, a polishing agent with a thickness of 0.5 mm was evenly coated on the surface of the polycarbonate liquid level observation window, and it was polished with a sponge pad until the surface of the polycarbonate liquid level observation window became transparent again; then it was ultrasonically cleaned and dried, and then placed in an electric blast drying oven at 90°C and baked for 60 minutes to remove residual stress; after cooling to room temperature, a self-repairing polycarbonate coating with a thickness of 0.015 mm was coated on the surface of the polycarbonate liquid level observation window, and cured with ultraviolet light; finally, performance testing was carried out.
[0101] Example 3: A polycarbonate liquid level observation window with a maximum surface defect depth of 0.25 mm is selected. First, the polycarbonate liquid level observation window is ultrasonically cleaned and dried; then, sandpaper with a grit size of F320 is used to grind and remove surface defects, and then sandpaper with a grit size of F800 is replaced to grind and remove fine lines around the defects until the surface defects of the polycarbonate liquid level observation window appear foggy; then the polycarbonate liquid level observation window is ultrasonically cleaned and dried.
[0102] Next, a 0.5 mm thick abrasive is evenly coated on the surface of the polycarbonate liquid level observation window, and a wool wheel is used to grind the surface of the polycarbonate liquid level observation window until the surface of the polycarbonate liquid level observation window is restored to be flat and smooth, and then the surface is ultrasonically cleaned and dried;
[0103] Then, a polishing agent with a thickness of 0.5 mm was evenly coated on the surface of the polycarbonate liquid level observation window, and it was polished with a sponge pad until the surface of the polycarbonate liquid level observation window became transparent again; then it was ultrasonically cleaned and dried, and then placed in an electric blast drying oven at 90°C and baked for 60 minutes to remove residual stress; after cooling to room temperature, a self-healing polycarbonate coating with a thickness of 0.25 mm was coated on the surface of the polycarbonate liquid level observation window, and cured with ultraviolet light; finally, performance testing was carried out.
[0104] Example 4: The treatment method is the same as that of Example 3, except that the deepest depth of the surface defects of the polycarbonate liquid level observation window is 0.3 mm.
[0105] Example 5: The treatment method is the same as that of Example 3, except that the maximum depth of the surface defects of the polycarbonate liquid level observation window is 0.6 mm.
[0106] Comparative Example 1: blank control, using an intact polycarbonate liquid level observation window.
[0107] Comparative Example 2: The treatment method is the same as that of Example 3, except that the maximum depth of the surface defects of the polycarbonate liquid level observation window is 0.3 mm, and the self-repairing polycarbonate coating is not applied.
[0108] The test results are shown in the following table.
[0109] Table 1 shows the comprehensive performance test results.
[0110]
[0111] It can be seen from Table 1 above that the depths of surface defects in Example 1, Example 2, Example 3 and Example 4 are all less than or equal to 0.3 mm, and the surface hardness of the corresponding repaired polycarbonate liquid level observation window is basically maintained at about 2H, the surface hardness is relatively large, and scratches are not easily generated; and the light transmittance of the repaired polycarbonate liquid level observation window is basically above 90%, the light transmittance is good, and it is convenient for users to observe the liquid level.
[0112] The surface hardness and light transmittance of the repaired polycarbonate liquid level observation windows of Example 1, Example 2, Example 3 and Example 4 are slightly different from those of the blank control sample of Comparative Example 1, indicating that the repaired polycarbonate liquid level observation windows have better overall performance, which is beneficial to extending service life and reducing costs.
[0113] The surface of the repaired polycarbonate liquid level observation window in Example 4 feels smooth and delicate to the touch, while the surface of the comparative example 2, which is not coated with self-repairing polycarbonate, feels slightly blocked to the touch; it can be seen that coating the self-repairing polycarbonate coating can improve the smoothness of the surface.
[0114] However, when the surface defect depth of Example 5 is 0.6 mm and the self-repairing polycarbonate coating is not applied to Comparative Example 2, the surface hardness of Example 5 and Comparative Example 2 is 1H, which is average and relatively easy to be scratched; and the light transmittance of Example 5 and Comparative Example 2 is about 80%, which is average and affects the use. Therefore, when the defect exceeds 0.5 mm or the self-repairing polycarbonate coating is not applied during repair, the comprehensive performance will be affected.
[0115] In order to fully verify the performance of the repaired polycarbonate liquid level observation window, samples corresponding to Example 3 and Example 5 were selected for type testing, and the results are shown in Table 2 below.
[0116] Table 2 shows the type test results.
[0117]
[0118] The samples corresponding to Example 3 and Example 5 were ground, polished and coated with a self-repairing polycarbonate coating. It can be seen from Table 2 that after the samples corresponding to Example 3 and Example 5 were repaired, the results of their type tests were all qualified, indicating that the repair of the polycarbonate liquid level observation window was effective. It can be inferred that other samples with defect depths smaller than that of Example 3 and Example 5 can also maintain good performance after complete repair.
[0119] The disclosed embodiment can completely expose the surface defects by cleaning and drying the polycarbonate liquid level observation window, so as to facilitate the subsequent detection of the depth of the surface defects and determination of the type of the surface defects; then the polycarbonate liquid level observation window is surface treated according to the type of the surface defects, so as to improve different types of surface defects; the polycarbonate liquid level observation window after the surface treatment is cleaned and baked, wherein cleaning can remove surface impurities, and baking can remove residual stress of the polycarbonate liquid level observation window and reduce deformation; finally, the surface of the baked polycarbonate liquid level observation window is additively coated and UV-cured to improve the structural strength; the repair method of the present application can ensure the performance of the polycarbonate liquid level observation window under normal use, extend the service life of the polycarbonate liquid level observation window, and help reduce the maintenance cost of the enterprise.
[0120] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0121] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for repairing surface defects of a polycarbonate liquid level observation window, It is characterized in that The following steps are involved: Step (1), cleaning and drying the polycarbonate liquid level observation window; Step (2), detecting the depth of the surface defect of the polycarbonate liquid level observation window treated in step (1), and determining the type of the surface defect according to the depth of the surface defect; Step (3), performing surface treatment on the polycarbonate liquid level observation window according to the type of the surface defect; Step (4), cleaning and baking the polycarbonate liquid level observation window treated in the above step (3); Step (5), performing additive coating on the surface of the polycarbonate liquid level observation window treated in the above step (4), and performing curing treatment with ultraviolet light; Step (6), testing the polycarbonate liquid level observation window treated in the above step (5) to determine whether its performance is qualified.
2. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 1, It is characterized in that The types of surface defects are divided into mild defects, moderate defects and severe defects; in step (3), the surface treatment process of the polycarbonate liquid level observation window is as follows: When the surface defect is a slight defect, a polishing agent is applied to the surface of the polycarbonate liquid level observation window and a polishing process is performed using a sponge pad; When the type of the surface defect is a medium defect, firstly, an abrasive is applied to the surface of the polycarbonate liquid level observation window, and a grinding process is performed using a wool wheel; then, a polishing agent is applied to the ground surface of the polycarbonate liquid level observation window, and a polishing process is performed using a sponge pad; When the type of surface defect is a severe defect, first, the surface of the polycarbonate liquid level observation window is ground with sandpaper; second, the surface of the polycarbonate liquid level observation window after the grinding is coated with abrasive, and the window is ground with a wool wheel; third, the surface of the polycarbonate liquid level observation window after the grinding is coated with polishing agent, and the window is polished with a sponge pad.
3. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 2, It is characterized in that The temperature of the polishing process is 50-80°C, and the temperatures of the grinding process and the lapping process are both 30-60°C.
4. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 2, It is characterized in that The coating thickness of the polishing agent and the grinding agent is 0.5 to 1 mm.
5. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 2, It is characterized in that The process of grinding the surface of the polycarbonate liquid level observation window with sandpaper comprises the following steps: First, the surface defects are removed by grinding with coarse sandpaper; Then, fine sandpaper is used to grind and remove fine lines around the surface defect until the surface defect becomes hazy.
6. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 2, It is characterized in that The polishing agent includes one or a combination of aluminum oxide, sodium oxide, silicon dioxide or iron oxide.
7. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 2, It is characterized in that The abrasive comprises one or a combination of boron carbide, paraffin, sheep oil or turpentine.
8. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 2, It is characterized in that The depth of the surface defect is d; When d<0.01mm, the type of surface defect is a slight defect; When 0.01mm≤d<0.1mm, the type of surface defect is a moderate defect; When 0.1 mm ≤ d ≤ 0.5 mm, the type of the surface defect is a severe defect.
9. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 1, It is characterized in that In step (4), the baking temperature is 90-100° C. and the baking time is 50-60 min.
10. The method for repairing surface defects of a polycarbonate liquid level observation window according to claim 1, It is characterized in that The additively coated material is self-healing polycarbonate; The self-healing polycarbonate comprises the following raw materials in parts by weight: 100-140 parts of modified silica sol, 200-240 parts of vinyl polysiloxane-polycarbonate block polymer, 8-100 parts of propylene glycol, 300-400 parts of tetrahydrofuran, and 20-25 parts of benzoin dimethyl ether.