Penetration damage repairing method for composite material semi-closed cavity structure
By grinding and supporting the penetrating damage parts of the laminated semi-enclosed cavity structure, combined with magnet adsorption and rope traction technology, the problems of high repair costs and low efficiency are solved, and the repair process is simplified and efficiency improvement is achieved. , and the back plate can be reused.
Patent Information
- Application Number
- CN202411217610.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the laminated semi-enclosed cavity structure has high repair costs and low repair efficiency, and the backplate cannot be reused, resulting in a complex and high cost in repair process.
By grinding the penetrating damaged parts and setting a detachable iron sheet on the inner wall of the cavity as a repair support back plate, the iron sheet is tightly attached to the inner surface of the cavity by using magnet adsorption and string pulling, simplifying the repair process and on the outer surface Paint the repair layer for curing.
It realizes the convenience and efficiency of the repair process, with simple operation, few repair processes, short repair time, high repair efficiency, and the metal backplane can be reused, reducing repair costs.
Smart Images

Figure CN119078241A_ABST
Abstract
Description
[Technical field]
[0001] The invention relates to composite material repair technology, and in particular to a composite material semi-enclosed cavity structure penetration damage repair method. [Background technology]
[0002] Composite materials are widely used in aircraft due to their advantages of light weight and high strength and stiffness. Composite materials have become the mainstream trend of aircraft control surfaces. Composite materials control surfaces are mostly semi-closed cavity structures, integrally formed, and the skin cannot be disassembled. This means that when the composite material control surface skin is penetrated and damaged, only the aerodynamic side has repair space.
[0003] At present, when there is repair space on only one side of the rudder skin, there are more methods for repairing penetration damage to the sandwich structure skin, and fewer methods for repairing penetration damage to the laminated structure skin. The difficulty in repairing penetration damage to the laminated semi-closed cavity structure skin is that there is insufficient repair space inside the cavity, which makes it inconvenient to set up a backboard. When the repair layer laid on the outside of the cavity is vacuum cured, the repair layer will deform due to the pressure difference between the inside and outside of the cavity and cannot be cured. Therefore, for the repair of penetration damage to the laminated semi-closed cavity structure, the backboard is crucial.
[0004] For the above damage, the existing repair method is generally to use a thin rope to pull a composite patch through the through-damage hole on the cavity, and use an adhesive to first glue the composite patch to the inner surface of the cavity as a backing plate, or use fasteners to fix the composite patch to the inner surface of the cavity, and then perform subsequent repairs. Whether gluing the composite patch or fixing the composite patch with fasteners, additional repair processes are required, and the backing plate made of the composite patch cannot be reused, resulting in high repair costs and low repair efficiency. [Summary of the invention]
[0005] The present invention provides a method for repairing penetration damage of a composite material semi-enclosed cavity structure. Aiming at the problems of high repair cost and low repair efficiency of single-sided repair of penetration damage of a laminated semi-enclosed cavity structure, the damage repair method provided has a convenient and efficient repair process, simple operation, fewer repair steps, short repair time, high repair efficiency, little damage to the composite structure, and a reusable metal back plate, and is easy to promote and popularize among various aircraft manufacturers.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A method for repairing penetration damage of a composite material semi-enclosed cavity structure comprises the following steps:
[0008] Step 1: grinding the penetration damage part on the semi-enclosed cavity structure of the laminated composite material, wherein the maximum size of the penetration damage hole after grinding does not exceed the maximum size of the original through hole of the semi-enclosed cavity structure;
[0009] Step 2: prefabricate a long and narrow iron sheet. The outer dimensions of the iron sheet are determined according to the dimensions of the through-damage hole after grinding. The maximum dimension of the long side of the iron sheet is required to exceed the maximum dimension of the repair area.
[0010] Step 3: A small magnet pulled by a thin rope is magnetically adsorbed in the center of the narrow iron sheet, and the narrow iron sheet is passed through the penetration damage hole and extended into the cavity. The position of the iron sheet in the cavity is adjusted by the thin rope. After the position of the iron sheet is determined, the thin rope is tightened to make the iron sheet close to the inner surface of the cavity and completely cover the penetration damage hole;
[0011] Step 4: On the outer surface of the cavity, two magnets are used to magnetically attract the two ends of the narrow iron sheet through the composite laminate. After ensuring that the iron sheet is attracted and will not move, a thin rope is pulled to pull the small magnet pulled by the thin rope off the iron sheet, thereby completing the preparation of the repaired backplane;
[0012] Step 5: Then, lay the repair layer and repair and solidify the damaged area;
[0013] Step 6. When the repair is cured, remove the two magnets on the outer surface of the cavity and restore the protection of the outer surface of the cavity. At this time, the iron sheet inside the cavity falls off due to the lack of magnetic attraction. Then, pour the iron sheet out through the original through hole of the semi-closed cavity or use the magnet to suck it out, and the repair is completed.
[0014] Furthermore, the iron sheet in the step 2 is a long and narrow strip of iron sheet, which can be sucked and lifted by a magnet, and the outer dimensions of the iron sheet are required to be able to pass through the original passable hole on the semi-closed cavity structure; the maximum dimension of the long side of the iron sheet exceeds the maximum dimension of the repair area, and when two magnets suck the two ends of the long side of the iron sheet through the composite laminate, the positions of the two magnets cannot interfere with the repair area; the maximum dimension of the short side of the iron sheet is required not to exceed the minimum passable dimension of the through-damage hole after grinding, ensuring that the iron sheet can pass through the through-damage hole after grinding and enter the cavity.
[0015] Furthermore, the magnetic force of the two magnets on the outer surface of the cavity in step four is large enough to attract the iron sheet on the inner surface of the cavity through the composite laminate, and the sum of the suction forces of the two magnets on the iron sheet is much greater than the suction force of the small magnet on the iron sheet, so that the small magnet can be smoothly detached from the iron sheet under the pulling force of the thin rope.
[0016] Furthermore, the penetration damage hole formed after grinding the penetration damage part is a circular through hole or a square through hole.
[0017] Furthermore, the specific steps of laying the repair layer and repairing and curing the damaged part in step 5 include:
[0018] 1) Preparation of the repair area: Bevel the perimeter of the penetration damage hole to keep the cut surface smooth and with rounded corners;
[0019] After cutting, use sandpaper to smooth the paving area;
[0020] Then, clean the polished area, at least 1-3 mm beyond the edge of the polished area;
[0021] Next, dry the surface to be bonded;
[0022] 2) Prepare prepreg and adhesive film: The ply direction of carbon fiber prepreg is consistent with the original structure. The structure repaired with unidirectional tape prepreg has two layers of [-45 / 45] ply added on the basis of the original ply. The structure repaired with fabric prepreg has one layer of
[45] ply added on the basis of the original ply.
[0023] Cut the unidirectional tape or fabric prepreg to the required shape and size according to the ply order. The first layer boundary of the overlap area must exceed the boundary of the damaged area by at least 1 3mm, and the boundary of each subsequent layer must exceed the boundary of the previous layer by at least 13mm.
[0024] 3) Laying: Lay the prepreg on the side with the repair space. First, lay a layer of film on the laying area. The film is 6mm larger than the prepreg laying area. Then lay the prepreg layer by layer upwards.
[0025] If there is a copper mesh on the surface of the original structure, lay a layer of medium-temperature copper mesh film on the outermost layer;
[0026] 4) Curing: Install vacuum bag and heating equipment, and perform curing under vacuum pressure and required temperature;
[0027] On the basis of step five, in the corresponding step six, after the repair curing is completed, the vacuum bag and the heating device are removed, and the repair area is sanded with sandpaper until the original surface contour is restored, and the two magnets on the outer surface of the cavity are removed to restore the protection of the outer surface of the cavity.
[0028] The beneficial effects of the present invention are:
[0029] The present invention aims to solve the problems of high repair cost and low repair efficiency of single-sided repair of penetration damage in a laminated semi-enclosed cavity structure. The penetration damage part is polished, and a detachable iron sheet used as a repair support back plate is arranged at the polished penetration damage hole, which is close to the inner wall of the cavity, so as to facilitate the laying and curing of the repair layer. The repair process is convenient and efficient, the operation is simple, the repair process is less, the repair time is short, the repair efficiency is high, the damage to the composite structure is small, and the metal back plate is reusable. The invention has strong versatility, simple and ingenious structure, low production cost, and is easy to promote and popularize among various aircraft manufacturers.
Brief Description of the Drawings
[0030] Figure 1 is a schematic diagram of a through-hole damage hole after polishing of a semi-enclosed cavity structure in the present invention;
[0031] Figure 2 It is a schematic diagram of a small magnet pulled by a thin rope to attract an iron sheet in the present invention;
[0032] Figure 3 It is a schematic diagram of an iron sheet attracted by two magnets in the present invention, which is closely attached to the inner surface of the cavity;
[0033] Figure 4 Schematic diagram of the circular penetrating damage hole on the inner surface of the cavity completely covered by the iron sheet in the present invention;
[0034] Figure 5 Schematic diagram of the square penetrating damage hole on the inner surface of the cavity completely covered by the iron sheet in the present invention;
[0035] Figure 6 It is a schematic diagram of repairing penetrating damage by laying a repair layer in the present invention.
[0036] Figure numerals: 1. Laminated semi-closed cavity structure; 2. Round penetrating damage hole after grinding; 3. Square penetrating damage hole after grinding; 4. Iron sheet; 5. Small magnet; 6. Thin rope; 7. Two magnets; 8. Repair layer. [Specific implementation method]
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] A method for repairing penetration damage of a composite material semi-enclosed cavity structure comprises the following steps:
[0039] Step 1: Figure 1As shown, the penetration damage part on the laminated composite material semi-enclosed cavity structure 1 is polished, and the penetration damage hole formed after polishing the penetration damage part is a circular through hole 2 or a square through hole 3. The maximum size of the penetration damage hole after polishing does not exceed the maximum size of the original through hole of the semi-enclosed cavity structure 1, otherwise this method cannot be used for repair;
[0040] Step 2: Figure 2 and Figure 3 As shown, a narrow and long iron sheet 4 is prefabricated, and the outer dimensions of the iron sheet 4 are determined according to the size of the penetrating damage hole after grinding, and the maximum dimension of the long side of the iron sheet is required to exceed the maximum dimension of the repair area; in this embodiment, the iron sheet 4 is a narrow and long strip of iron sheet, the iron sheet 4 can be sucked and lifted by the magnet 5, and the outer dimensions of the iron sheet 4 are required to be able to pass through the original passable hole on the semi-closed cavity structure 1; and the maximum dimension of the long side of the iron sheet 4 exceeds the maximum dimension of the repair area, and when the two magnets 7 suck the two ends of the long side of the iron sheet 4 through the composite laminate, the positions of the two magnets 7 cannot interfere with the repair area; the maximum dimension of the short side of the iron sheet 4 is required not to exceed the minimum passable dimension of the penetrating damage hole after grinding, to ensure that the iron sheet 4 can pass through the penetrating damage hole after grinding into the cavity. For example, when the through-hole damage hole after grinding is a circular through hole 2, the maximum size of the short side does not exceed the diameter of the circular hole 2; when the through-hole damage hole after grinding is a square through hole 3, the maximum size of the short side does not exceed the length of the longest diagonal of the square through hole 3; at the same time, the thickness of the iron sheet 4 should not be too thin, and it is required to have sufficient rigidity so that it is not easy to deform during vacuum curing in the subsequent step five, and the thickness of the iron sheet 4 should not be too thick, resulting in that when the damaged surface of the cavity is a curved surface, the iron sheet 4 cannot bend and stick to the inner surface of the cavity when the thin rope is tightened in the subsequent step three;
[0041] Step 3: Figures 3 to 5 As shown, a small magnet 5 pulled by a thin rope 6 is magnetically adsorbed on the center of a narrow iron sheet 4, and the narrow iron sheet 4 is passed through the penetrating damage hole and extended into the cavity. The position of the iron sheet 4 in the cavity is adjusted by the thin rope 6. After the position of the iron sheet 4 is determined, the thin rope 6 is tightened to make the iron sheet close to the inner surface of the cavity and completely cover the penetrating damage hole.
[0042] Step 4: Figures 3 to 5 As shown, two magnets 7 are used on the outer surface of the cavity to magnetically attract the two ends of the narrow iron sheet 4 through the composite laminate. After confirming that the iron sheet 4 is attracted and will not move, the thin rope 6 is pulled to pull the small magnet 5 pulled by the thin rope 6 off the iron sheet 4, completing the preparation work for the repaired backplane. When in use, the magnetic force of the two magnets 7 on the outer surface of the cavity is large enough to attract the iron sheet 4 on the inner surface of the cavity through the composite laminate. The sum of the suction force of the two magnets 7 on the iron sheet 4 is much greater than the suction force of the small magnet 5 on the iron sheet 4, so that the small magnet 5 can be smoothly detached from the iron sheet 4 under the pulling force of the thin rope 6.
[0043] Step 5. Then, Figure 6 As shown, the repair layer is laid and the damaged part is repaired and cured;
[0044] 1) Preparation of the repair area: Bevel the perimeter of the penetration damage hole to keep the cut surface smooth and with rounded corners;
[0045] After cutting, use sandpaper larger than 80 grit to sand the paving area;
[0046] Then, clean the polished area, at least 1-3 mm beyond the edge of the polished area;
[0047] Next, dry the surface to be bonded;
[0048] 2) Prepare prepreg (repair material) and adhesive film: The ply direction of carbon fiber prepreg is consistent with the original structure. The structure repaired with unidirectional tape prepreg has two layers of [-45 / 45] ply added to the outermost layer on the basis of the original ply. The structure repaired with fabric prepreg has one layer of
[45] ply added to the outermost layer on the basis of the original ply.
[0049] Cut the unidirectional tape or fabric prepreg to the required shape and size according to the ply order. The first layer boundary of the overlap area must exceed the boundary of the damaged area by at least 1 3mm, and the boundary of each subsequent layer must exceed the boundary of the previous layer by at least 13mm.
[0050] 3) Laying: Lay the prepreg on the side with the repair space. First, lay a layer of film on the laying area. The film is 6mm larger than the prepreg laying area. Then lay the prepreg layer by layer upwards.
[0051] If there is a copper mesh on the surface of the original structure, lay a layer of medium-temperature copper mesh film on the outermost layer;
[0052] 4) Curing: Install vacuum bag and heating equipment, and perform curing under vacuum pressure and required temperature;
[0053] Step 6. After the repair is cured, remove the vacuum bag and the heating equipment, and use sandpaper to polish the repair area until the original surface contour is restored. Remove the two magnets 7 on the outer surface of the cavity, and restore the protection of the outer surface of the cavity. At this time, the iron sheet 4 inside the cavity falls off due to the lack of magnetic attraction. Then, pour out the iron sheet through the original through hole of the semi-closed cavity or use the magnet to suck it out, and the repair is completed.
[0054] In this embodiment, the entire repair process is convenient and efficient, the operation is simple, the repair process is few, the repair time is short, the repair efficiency is high, the damage to the composite structure is small, and the metal back panel is reusable, which is easy to promote and popularize among various aircraft manufacturers.
[0055] In the description of the present invention, it should be noted that the terms "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the inventive product is usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0056] The above-described embodiments are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. All equivalent changes made based on the shape, structure and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for repairing penetration damage of a composite semi-enclosed cavity structure, characterized in that: The following steps are involved: Step 1: grinding the penetration damage part on the semi-enclosed cavity structure of the laminated composite material, wherein the maximum size of the penetration damage hole after grinding does not exceed the maximum size of the original through hole of the semi-enclosed cavity structure; Step 2: prefabricate a long and narrow iron sheet. The outer dimensions of the iron sheet are determined according to the dimensions of the through-damage hole after grinding. The maximum dimension of the long side of the iron sheet is required to exceed the maximum dimension of the repair area. Step 3: A small magnet pulled by a thin rope is magnetically adsorbed in the center of the narrow iron sheet, and the narrow iron sheet is passed through the penetration damage hole and extended into the cavity. The position of the iron sheet in the cavity is adjusted by the thin rope. After the position of the iron sheet is determined, the thin rope is tightened to make the iron sheet close to the inner surface of the cavity and completely cover the penetration damage hole; Step 4: On the outer surface of the cavity, two magnets are used to magnetically attract the two ends of the narrow iron sheet through the composite laminate. After ensuring that the iron sheet is attracted and will not move, a thin rope is pulled to pull the small magnet pulled by the thin rope off the iron sheet, thereby completing the preparation of the repaired backplane; Step 5: Then, lay the repair layer and repair and solidify the damaged area; Step 6. When the repair is cured, remove the two magnets on the outer surface of the cavity and restore the protection of the outer surface of the cavity. At this time, the iron sheet inside the cavity falls off due to the lack of magnetic attraction. Then, pour the iron sheet out through the original through hole of the semi-closed cavity or use the magnet to suck it out, and the repair is completed.
2. A method for repairing penetration damage of a composite material semi-enclosed cavity structure according to claim 1, characterized in that: The iron sheet in step 2 is a long and narrow strip of iron sheet, which can be sucked and lifted by a magnet, and the outer dimensions of the iron sheet are required to be able to pass through the original passable hole on the semi-closed cavity structure; the maximum dimension of the long side of the iron sheet exceeds the maximum dimension of the repair area, and when two magnets suck the two ends of the long side of the iron sheet through the composite laminate, the positions of the two magnets cannot interfere with the repair area; the maximum dimension of the short side of the iron sheet is required not to exceed the minimum passable dimension of the through-damage hole after grinding, ensuring that the iron sheet can pass through the through-damage hole after grinding and enter the cavity.
3. The method for repairing penetration damage of a composite material semi-enclosed cavity structure according to claim 1, characterized in that: The magnetic force of the two magnets on the outer surface of the cavity in step 4 is large enough to attract the iron sheet on the inner surface of the cavity through the composite laminate. The sum of the suction forces of the two magnets on the iron sheet is much greater than the suction force of the small magnet on the iron sheet, so that the small magnet can be smoothly detached from the iron sheet under the pulling force of the thin rope.
4. The method for repairing penetration damage of a composite material semi-enclosed cavity structure according to claim 1, characterized in that: The penetration damage hole formed after grinding the penetration damage part is a circular through hole or a square through hole.
5. The method for repairing penetration damage of a composite material semi-enclosed cavity structure according to claim 1, characterized in that: The specific steps of laying the repair layer and repairing and curing the damaged part in step 5 include: 1) Preparation of the repair area: Bevel the perimeter of the penetration damage hole to keep the cut surface smooth and with rounded corners; After cutting, use sandpaper to smooth the paving area; Then, clean the polished area, and the cleaning range should be at least 13mm beyond the edge of the polished area; Next, dry the surface to be bonded; 2) Prepare prepreg and adhesive film: The ply direction of carbon fiber prepreg is consistent with the original structure. The structure repaired with unidirectional tape prepreg has two layers of [-45 / 45] ply added on the basis of the original ply. The structure repaired with fabric prepreg has one layer of [45] ply added on the basis of the original ply. Cut the unidirectional tape or fabric prepreg to the required shape and size according to the ply order. The boundary of the first layer of the overlap area must exceed the boundary of the damaged area by at least 13mm, and the boundary of each subsequent layer must exceed the boundary of the previous layer by at least 13mm. 3) Laying: Lay the prepreg on the side with the repair space. First, lay a layer of film on the laying area. The film is 6mm larger than the prepreg laying area. Then lay the prepreg layer by layer upwards. If there is a copper mesh on the surface of the original structure, lay a layer of medium-temperature copper mesh film on the outermost layer; 4) Curing: Install vacuum bag and heating equipment, and perform curing under vacuum pressure and required temperature; On the basis of step five, in the corresponding step six, after the repair curing is completed, the vacuum bag and the heating device are removed, and the repair area is sanded with sandpaper until the original surface contour is restored, and the two magnets on the outer surface of the cavity are removed to restore the protection of the outer surface of the cavity.