Conformal particle film, conformal functional composite particle film and preparation method of conformal particle film and conformal functional composite particle film
Through improved gas-liquid interface self-assembly method and automated self-assembly device, a conformal particle film and functional composite film are prepared with high stability and good uniformity, which solves the problems of poor film performance and low preparation efficiency in the prior art. , realizes the efficient integrated application of conformal electronic devices.
Patent Information
- Application Number
- CN202411029685.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-12-06
AI Technical Summary
Existing film preparation methods such as natural particle sedimentation method, vacuum evaporation method and gas-liquid interface self-assembly method have poor performance, low preparation efficiency, poor stability and difficult to achieve batch production and large-area production in the preparation of conformal particle films. question.
Using the improved gas-liquid interface self-assembly method, the conformal particle film and the conformal functional composite particle film are prepared by an automated self-assembly device in an electric propulsion manner through an automated self-assembly device. The combined structure of the adhesive layer and the functional layer is used to realize the particle embedding and adhesion. The layer improves the stability of the film and the thickness controllability of the functional layer.
It achieves the improvement of film uniformity and stability, improves preparation efficiency, and can achieve batch and large-area production, which is suitable for integrated applications of conformal electronic devices.
Smart Images

Figure CN119078245A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conformal flexible electronic materials, and in particular to a conformal particle film and a conformal functional composite particle film and a preparation method thereof. Background Art
[0002] Flexible electronic devices can be conformally attached to complex curved surfaces such as the human body and prostheses. In actual use, they are usually faced with complex environments, which poses a huge challenge to the stability of the devices. In order to overcome various problems in the use of flexible electronic devices, flexible electronic devices based on conformal flexible functional materials, for example, electronic devices based on magnetic functional materials, play an important role in this field. Therefore, magnetic functional materials such as conformal magnetic films are important basic materials for functional devices such as storage, sensing, and antennas.
[0003] Existing thin film preparation methods mostly use natural particle sedimentation method, vacuum evaporation method and gas-liquid interface self-assembly method, but the inventors of the present application recognize that the above methods have some defects in the thin film preparation process, resulting in poor performance of conformal particle films prepared by the above film preparation methods and low preparation efficiency, which affects the application of conformal particle films in conformal electronic devices. Summary of the invention
[0004] Based on the research on the development status and trends of current conformal electronic materials and the recognition of the defects of current thin film preparation methods, the inventors of this application have improved the gas-liquid interface self-assembly method and provided an improved preparation method, and prepared conformal particle films and conformal functional composite particle films with good uniformity and stability. The preparation method is simple, low-cost, and automatically controlled. It is less affected by environmental and human factors, has high efficiency, and can realize batch and large-area film production. It has potential application prospects in common electronic devices, especially in integration.
[0005] According to one embodiment of the present invention, an object is to provide a conformal particle film and a conformal functional composite particle film and a preparation method thereof.
[0006] In order to achieve the above purpose, the following technical solutions can be used:
[0007] According to one aspect of the present invention, a method for preparing a conformal particle film is provided, comprising: coating an adhesion material on a substrate to form an adhesion layer conformal to the substrate; preparing a gas-liquid interface self-assembled film from a metal particle precipitate using an electric propulsion method through an automated self-assembly device; attaching the gas-liquid interface self-assembled film to the adhesion layer conformal to the substrate to form a functional layer, wherein the thickness of the functional layer is controllable; and drying to obtain a conformal particle film attached to the surface of the substrate, wherein in the conformal particle film, some metal particles of the gas-liquid interface self-assembled film are embedded in the adhesion layer.
[0008] According to one aspect of the present invention, a method for preparing a conformal functional composite particle film is provided, comprising: coating an adhesion material on a substrate to form an adhesion layer conformal to the substrate; preparing corresponding gas-liquid interface self-assembled films from metal particle precipitates using electric propulsion by multiple automated self-assembly devices; sequentially attaching each gas-liquid interface self-assembled film on the adhesion layer conformal to the substrate to form a functional layer by single-layer stacking, wherein each gas-liquid interface self-assembled film is the same or different and the thickness of the functional layer is controllable; and drying to obtain a conformal functional composite particle film attached to the surface of the substrate, wherein in the conformal functional composite particle film, some metal particles of the gas-liquid interface self-assembled film are embedded in the adhesion layer.
[0009] Optionally, the automated self-assembly device comprises: a film-making container, a bracket located on one side of the film-making container, and an electric propulsion control device; wherein the electric propulsion control device comprises: a controller, a controllable telescopic motor and a remote control connected to the controller, and a powder carrier connected to the end of a push rod of the controllable telescopic motor, wherein the controllable telescopic motor is mounted on the bracket and is located directly above the film-making container.
[0010] Optionally, each automated self-assembly device uses an electric propulsion method to prepare a corresponding gas-liquid interface self-assembly film from a metal particle precipitate, including the following steps: determining metal particles according to functional requirements, placing them in a solvent for ultrasonic dispersion, and letting them stand to obtain a precipitate; adding water to the film-making container; placing the precipitate in a powder carrier at the end of the controllable telescopic motor push rod, and placing the powder carrier above the liquid surface in the film-making container; electrically controlling the propulsion amount of the controllable telescopic motor by a remote control to drive the powder carrier into the liquid surface in the film-making container, and adjusting the vertical position of the powder carrier to keep the precipitate therein always at the air / water interface, thereby self-assembling to form a gas-liquid interface self-assembly film.
[0011] Optionally, an adhesive layer conforming to the substrate is sequentially placed below the air-liquid interface self-assembled film of each film-forming container, and each air-liquid interface self-assembled film is attached by lifting.
[0012] Optionally, the particle size of the metal particles is 0.1-100 μm.
[0013] Optionally, the metal particles are metal single substance particles or alloy particles.
[0014] Optionally, the metal component contained in the metal particles is any one or more of Ga, Ti, Fe, Co, and Ni.
[0015] Optionally, the adhesive material is coated on the substrate by electrospinning or spin coating.
[0016] Optionally, before the drying step, the method further comprises: using a spinning process to attach the encapsulation material to the surface of the functional layer to form an encapsulation layer.
[0017] Optionally, the adhesive material and the packaging material are any one of MA, PDMS, PU, Ecoflex, SEBS, PP, PU, TPE, LSR, LVER, and TPU solution.
[0018] Optionally, the method is used to mass-produce large-area conformal functional composite particle films.
[0019] According to one aspect of the present invention, a conformal particle film is provided, which is prepared by the method for preparing a conformal particle film, and comprises an adhesion layer conformal to a substrate and a functional layer, wherein the functional layer is a gas-liquid interface self-assembled film.
[0020] According to one aspect of the present invention, a conformal functional composite particle film is provided, which is prepared by the method for preparing a conformal functional composite particle film, and comprises an adhesion layer and a functional layer conformal to a substrate in sequence, wherein the functional layer is composed of a multilayer gas-liquid interface self-assembled film.
[0021] Beneficial effects: According to one embodiment of the present invention, the present invention improves the process of preparing thin films by the gas-liquid interface self-assembly method, which not only overcomes the defects of the existing gas-liquid self-assembly method for preparing thin films, but also makes the gas-liquid interface self-assembled film particles in the film evenly distributed, the film thickness is consistent, and the film has good stability during use. Moreover, the present invention can prepare a conformal functional composite particle film by sequentially attaching a single layer film, realizes controllable thickness of the functional layer, and can also realize the composite of a multifunctional gas-liquid interface self-assembled film, which has potential applications in the integration of conformal electronic devices.
[0022] Among them, the present invention accurately controls the propulsion amount through an automated self-assembly device, thereby improving the uniformity of particle distribution in the self-assembled film at the gas-liquid interface, making the film thickness consistent, and attaching it to an adhesion layer that is conformal to the substrate. Part of the metal particles are embedded in the interior of the adhesion layer to improve the bonding ability with the conformal surface, thereby ensuring the stability of the particles during use. For example, under stress conditions such as scratches and extrusion, the particles can maintain good adhesion.
[0023] In addition, the present invention can form a functional layer by sequentially attaching single layers of the same or different gas-liquid interface self-assembled films according to functional needs, thereby achieving controllable thickness of the functional layer. For example, the thickness of the functional layer can be equal to the sum of the diameters of the particles in each layer of the gas-liquid interface self-assembled film. The thickness-controllable conformal functional composite particle film (magnetic and conductive / shielding composite) provides a new idea for the integration of conformal electronic devices and has potential applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A schematic diagram of the principle of an automated self-assembly device in one embodiment of the present invention;
[0025] Figure 2 A schematic diagram of the layer structure of a conformal functional composite particle film attached to a substrate surface prepared in one embodiment of the present invention;
[0026] Figure 3 An optical side view of a self-assembly interface in a film-forming container in one embodiment of the present invention;
[0027] Figure 4 This is an optical image of a conformal amorphous magnetic granular film prepared in one embodiment of the present invention.
[0028] Reference numerals: 1 - base layer, 2 - MA adhesion layer, 3 - magnetic particle functional layer, 4 - liquid metal shielding layer, 5 - spinning encapsulation layer. DETAILED DESCRIPTION
[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] As mentioned above, the inventors of the present application have realized that the existing thin film preparation methods all have some defects. Through further research and summary of the process of preparing thin films by gas-liquid interface self-assembly method, it is realized that the following problems mainly affect the quality and preparation efficiency of the thin film.
[0031] 1) The manual operation process is difficult to accurately control. Due to the limitations of particle size and speed, the particles diffuse unevenly, and the roughness of the film surface is high after film formation. Although it is expected that the precipitate is always at the air / water interface, this standard cannot be guaranteed due to manual operation, resulting in uneven distribution of film thickness and composition on the surface, inconsistent film thickness, and affecting the performance of the film.
[0032] 2) The thickness of the film cannot be precisely controlled, especially for complex structures, which requires higher technical requirements and control methods.
[0033] 3) The quality of the film is unstable. During manual operation, the film may be affected by environmental conditions, such as changes in temperature and humidity, which may lead to instability, decomposition or structural changes of the film. In addition, during use, under certain stress conditions, the stability of the metal particles in the film cannot be guaranteed.
[0034] 4) The preparation efficiency of self-assembly film is low due to manual operation. In particular, for the conformal functional composite particle film proposed in this application, mass production cannot be achieved. In addition, the gas-liquid interface self-assembly method is usually only applicable to the preparation of thin films of small size or local area, but it is difficult to prepare large-area thin films.
[0035] 5) The self-assembly method at the gas-liquid interface is usually completed by transferring the thin film from the gas-liquid interface to a solid substrate first. However, the thin film transfer process has certain technical difficulties and there are problems with transfer and integration difficulties.
[0036] Based on the above understanding, the present invention provides a new preparation method, in which the automatic self-assembly device of the present invention adopts an electric propulsion method to accurately control the propulsion amount of the powder carrier, thereby improving the uniformity of particle distribution in the gas-liquid interface self-assembled film, making the film thickness consistent, and laying an adhesion layer on the substrate, which is attached to the adhesion layer conformal to the substrate. Some metal particles will be embedded in the interior of the adhesion layer, thereby improving the bonding ability of the gas-liquid interface self-assembled film with the conformal surface and ensuring the stability of the film during use.
[0037] In addition, the electric propulsion of the present application accurately controls the propulsion amount, thereby improving the uniformity of particle distribution in the gas-liquid interface self-assembled film and keeping the film thickness as consistent as possible. Based on this, in an optional embodiment, the present invention forms a functional layer by sequentially attaching a single layer of gas-liquid interface self-assembled film on an adhesion layer according to functional needs, and the thickness of the functional layer is controllable. For example, a multifunctional layer is formed by a plurality of different single layers of gas-liquid interface self-assembled films, etc. The functional conformal composite particle film with controllable thickness provides a new idea for the integration of conformal electronic devices and has potential applications.
[0038] Figure 1Schematic diagram of an automated self-assembly device in one embodiment of the present invention. Figure 1 As shown in the schematic diagram, the device includes: a film-making container, a bracket located on one side of the film-making container, and an electric propulsion control device installed on the bracket. The present invention improves conventional self-assembly components to form an automated self-assembly device based on an electric propulsion control device. By completing self-assembly film formation under electric propulsion, the uniformity of particle distribution is improved, the consistency of film thickness is ensured, and the efficiency of film preparation is improved, so that batch and large-area production of films can be achieved.
[0039] In addition, if Figure 1 As shown, the automated self-assembly device may further include: a horizontal placement platform, on which the bracket is vertically fixed, and may be biased toward an edge; and the film-making container is placed on the placement platform for subsequent automated self-assembly.
[0040] The electric propulsion control device, reference Figure 1 As shown, it may include: a controller, a controllable telescopic motor connected to the controller, and a powder carrier connected to the end of the controllable telescopic motor. The controllable telescopic motor is vertically mounted on a bracket and is located above the film-making container; the controllable telescopic motor has a telescopic push rod, and the powder carrier is connected to the end of the push rod. The powder carrier can be a slot structure such as a key. The controller adopts a DC wireless controller and is equipped with a remote controller. The push rod in the controllable telescopic motor is controlled by wireless control of the remote controller to control the advancement of the push rod, that is, to control the advancement of the powder carrier containing the precipitate, which is more conducive to the production of large batches and large areas of thin films.
[0041] A method for preparing a conformal particle film provided in one embodiment of the present invention comprises the following steps: 1) coating an adhesive material on a substrate to form an adhesive layer conformal to the substrate; 2) preparing a corresponding gas-liquid interface self-assembled film from a metal particle precipitate by electric propulsion through an automated self-assembly device; 3) attaching the gas-liquid interface self-assembled film to the adhesive layer conformal to the substrate to form a functional layer; 4) drying to obtain a conformal particle film attached to the surface of the substrate. The conformal particle film prepared in this embodiment has uniform particle dispersion, uniform film thickness, and some metal particles of the gas-liquid interface self-assembled film are embedded in the adhesive layer, thereby improving the stability of the film during use.
[0042] A method for preparing a conformal functional composite particle film provided in one embodiment of the present invention comprises:
[0043] Step S1, coating an adhesive material on a substrate to form an adhesive layer conformal to the substrate.
[0044] Furthermore, an adhesion layer can be conformally spread on the surface of the substrate by electrospinning or planar spin coating. The adhesion material can be MA (methyl acrylate), PDMS (polydimethylsiloxane), PU (polyurethane), Ecoflex (a thermoplastic elastomer material with environmentally friendly thermal properties produced by BASF, with a molecular formula of (C 18 H 34 O 10 )n), SEBS (hydrogenated styrene-butadiene block copolymer), PP (polypropylene), PU (polyurethane), TPE (thermoplastic elastomer), LSR (liquid silicone rubber), LVER (liquid ethylene-propylene rubber), TPU (thermoplastic polyurethane elastomer) solution. The above adhesive material can be combined with the metal particles in the present invention, and the bonding ability is high. Under the conditions of scratching, extrusion and other stresses, the metal particles of the present invention can maintain good adhesion, and the stability of the particles / film is guaranteed.
[0045] Step S2, using multiple automated self-assembly devices to electrically propel the metal particle precipitates to obtain corresponding gas-liquid interface self-assembled films.
[0046] The following is a further description of the present application using an automated self-assembly device as an example, including:
[0047] Step S21, according to functional requirements, metal particles are determined, placed in a solvent for ultrasonic dispersion, and allowed to stand to obtain a precipitate.
[0048] Specifically, the corresponding metal particles can be selected for preparation according to the functional requirements. The metal particles can be metal single-substance particles or alloy particles. For example, liquid metals with good deformation ability and high conductivity, such as gallium-indium alloys, are selected to prepare high-conductivity gas-liquid interface self-assembled films; for example, magnetic metal particles such as iron are selected to prepare magnetic gas-liquid interface self-assembled films. The metal component contained in the metal particles can be any one of Ga, Ti, Fe, Co, and Ni. Specifically, the type of the metal particles can be solidified liquid metals, such as Ga-In alloy particles, Ga particles, etc., and can be single-substance particles corresponding to solid metals Ti, Fe, Co, Ni and their related alloy particles.
[0049] In addition, the particle size of the metal particles is controlled to be 0.1-100 μm, such as 0.1 μm, 1 μm, 10 μm, 40 μm, 60 μm, 80 μm, 100 μm, etc. The inventors of the present application have found through further experiments that the above-mentioned micron-sized metal particles obtained by ball milling can realize self-assembly and form a film on the gas-liquid surface under the action of interfacial tension, Marangoni force, particle self-weight and other forces.
[0050] Step S22, adding water into the film-making container, placing the precipitate in a powder carrier at the end of the push rod of the controllable telescopic motor, and making the powder carrier be located above the liquid level in the film-making container.
[0051] Step S23, electrically controlling the propulsion amount of the controllable telescopic motor through the remote control, driving the powder carrier based on the electric propulsion method to control the precipitate to enter the liquid level in the film-making container, and adjusting the position of the powder carrier in the vertical direction through remote control to always keep the precipitate therein at the air / water interface until the solid particles in the precipitate diffuse and cover the water surface under the action of the solvent, and self-assemble to form a gas-liquid interface self-assembled film.
[0052] Step S3, sequentially attaching each gas-liquid interface self-assembled film on the adhesion layer conforming to the substrate to form a functional layer by stacking single layers.
[0053] Preferably, the gas-liquid interface self-assembled film prepared by water interface transfer forms a conformal particle film on the surface of the adhesion layer. Specifically, by sequentially placing the adhesion layer conformal to the substrate under the gas-liquid interface self-assembled film of each film-making container, each gas-liquid interface self-assembled film is attached by lifting, thus avoiding the separate transfer step of the gas-liquid interface self-assembled film, and because the setting of the adhesion layer can also ensure the binding ability of the particles with the conformal surface, the problem of the inability of the particles to be stably attached to the substrate in conventional substrate transfer can be overcome.
[0054] The thickness of the functional layer is controllable and is determined according to the particle diameter in each gas-liquid interface self-assembled film. The number of layers of the functional layer can be any number of layers in the range of 2-10 layers, which can be specifically determined according to functional requirements. Of course, the functional layer can be a homofunctional layer formed by multiple layers of the same gas-liquid interface self-assembled film, or a multifunctional layer formed by multiple layers of different gas-liquid interface self-assembled films.
[0055] Step S4, drying to obtain a conformal functional composite particle film attached to the surface of the substrate, wherein in the conformal functional composite particle film, part of the metal particles of the gas-liquid interface self-assembled film are embedded in the adhesion layer.
[0056] This embodiment has the following advantages: 1) Through the use of electric propulsion by the automated self-assembly device, each metal particle precipitate is prepared into a corresponding gas-liquid interface self-assembled film, in which the particles are evenly dispersed and the film thickness is consistent, overcoming the problem that the precipitate particles cannot always be at the gas-liquid interface by manually adjusting the key height, and solving the problem of poor particle distribution uniformity and easy particle stacking. 2) Through the simultaneous operation of multiple automated self-assembly devices, multiple gas-liquid interface self-assembled films can be prepared at the same time, greatly improving the efficiency of film preparation, and the equipment is simple and easy to operate, which can realize the batch production and large-area generation of films, that is, the preparation method of the present invention is particularly used for the batch production of large-area conformal functional composite particle films, and the effect is more prominent. 3) After the prepared gas-liquid interface self-assembled films are formed, the functional layer is formed by sequentially attaching the gas-liquid interface self-assembled films on the adhesion layer conformal to the substrate; the functional layer is formed by stacking multiple single layers, which solves the problem of uncontrollable thickness and uneven particle distribution leading to different thickness; wherein, the thickness of the functional layer is equal to the sum of the diameters of the particles in each layer (the adhesion layer embeds some particles because its function is not affected, and it can still be regarded as the actual functional thickness of the functional layer. In the case of multiple layers, such as generally ≤10 layers, the upper particle film may be interlaced with the lower particle film, so that the minimum thickness of the film is less than the actual thickness, but because the actual thickness depends on the maximum point when measuring the film thickness, the film thickness is equal to the sum of the particle diameters of each layer). 4) By setting an adhesion layer on the substrate, the problem of unstable particle structure is solved, that is, the present invention improves the bonding ability of particles and conformal surfaces through the adhesion layer, and some metal particles are embedded in the adhesion layer. When the film is subjected to stress such as scratching and extrusion, the metal particles can still maintain good adhesion, and the stability of the particles and the film is guaranteed.
[0057] In addition, the present invention has the following advantages: simple equipment, low cost, simplified process flow, improved ease of instrument use, and reduced film preparation cost; the present invention is greatly less affected by the environment and can stably prepare films under conditions of 10-40°C.
[0058] In an optional embodiment, the method, before the drying step, further includes: using a spinning process to attach the encapsulation material to the surface of the functional layer to form an encapsulation layer. In this embodiment, by sandwiching the functional layer between the adhesion layer and the encapsulation layer, the adhesion firmness of the particles is further improved, so that the film can maintain good stability even under stress. Furthermore, in order to obtain a better encapsulation effect and improve the stability of the particles in the functional layer, the encapsulation material can be consistent with the adhesion material of the above-mentioned adhesion layer, for example, it can be any one of TPU (thermoplastic polyurethane elastomer), MA, PDMS, PU, Ecoflex, SEBS, PP, PU, TPE, LSR, LVER and other solutions. In addition, the thickness of the encapsulation layer can be controlled to be 0.1-100μm.
[0059] In one embodiment of the present invention, a conformal particle film is provided, comprising an adhesion layer conformal to a substrate and a gas-liquid interface self-assembled film, and further comprising an encapsulation layer located on the surface of the gas-liquid interface self-assembled film.
[0060] In one embodiment of the present invention, a conformal functional composite particle film is provided, which comprises: an adhesion layer conformal to a substrate, and a functional layer. The functional layer is composed of a plurality of gas-liquid interface self-assembled films. The functional layer can be a homofunctional layer formed by a plurality of gas-liquid interface self-assembled films of the same type, or a multifunctional layer formed by a plurality of different gas-liquid interface self-assembled films.
[0061] In addition, it also includes an encapsulation layer located on the surface of the outermost gas-liquid interface self-assembled film in the functional layer. For example, the functional layer at least includes: a gas-liquid interface self-assembled magnetic particle film and a gas-liquid interface self-assembled liquid metal shielding particle film to form a conformal magnetic shielding composite particle film.
[0062] The present invention will be described more clearly and further below in conjunction with specific embodiments:
[0063] Example 1 [Conformal particle film]
[0064] MA is used as the adhesion layer material, and amorphous iron silicon boron is used as the metal particles.
[0065] The preparation method is as follows:
[0066] 1) The MA solution was conformally spin-coated on a 20×20 mm silicon wafer substrate to obtain an adhesion layer conformal to the silicon wafer, wherein the spin-coating speed was 1800 r / min and the spin-coating time was 30 seconds.
[0067] 2) Select amorphous FeSiB particles smaller than 10 μm, use alcohol as a dispersant, ultrasonically treat the particles, and then place them in a -5°C environment for 30 minutes. After stratification, remove the lower layer of FeSiB precipitate.
[0068] 3) Put 800 ml of water in an 800 ml beaker as the gas-liquid interface, take the iron silicon boron precipitate in step 2) and put it into the powder carrier at the lower end of the push rod in the electric propulsion control device, control the precipitate to enter the liquid surface by automatic propulsion, and adjust the push rod by remote control to always keep the precipitate at the air / water interface until the solid particles in the precipitate diffuse and cover the water surface under the action of the solvent, and complete the preparation of the amorphous iron silicon boron self-assembled film at the water-gas interface.
[0069] 4) The silicon wafer with the MA adhesion layer spin-coated thereon (i.e., the adhesion layer conformal to the silicon wafer obtained in step 1) is immersed under the amorphous FeSiB self-assembled film at the water interface, and the functional layer, i.e., the amorphous FeSiB self-assembled film, is conformally bonded to the upper surface of the MA adhesion layer by a lifting and bonding method.
[0070] 5) heating and drying to obtain a conformal film of amorphous magnetic particles. The performance and stability of the film are further improved by post-treatment of heating and drying.
[0071] Figure 3 FIG. 2 shows an optical side view of the self-assembly interface in the film-forming container in this embodiment. Figure 3 As shown, it can be seen that a dense single-layer particle film can be prepared at the junction of the water-air interface through the automatic assembly process.
[0072] Figure 4 FIG. 2 shows an optical image of the conformal metal particle film, i.e., the conformal amorphous magnetic particle film, prepared in this embodiment. Figure 4 As shown, after drying, the amorphous iron silicon boron particles are combined with the conformal surface, and some particles are embedded in the adhesion layer. The particles can maintain good adhesion. During the subsequent use of the film, even under scratches, extrusion and other stress conditions, the stability of the particles can still be guaranteed.
[0073] Example 2 [Multifunctional conformal functional composite particle film]
[0074] Figure 2 The layer structure of the multifunctional conformal functional composite particle film attached to the substrate surface prepared in this embodiment is schematically shown. Figure 2 As shown, it includes: a base layer 1, a MA adhesion layer 2, a magnetic particle functional layer 3, a liquid metal shielding layer 4 and a spinning encapsulation layer 5. The formation process of the layer structure may include the following steps:
[0075] 1) isopropyl alcohol, ethyl acetate and MA (methacrylic anhydride) are mixed in a mass ratio of 5:5:20 to obtain a MA solution, and a silicon wafer substrate is used as a base layer, and a uniform adhesion layer conforming to the base layer with a thickness of 1 μm is obtained by spin coating on the silicon wafer substrate.
[0076] 2) Amorphous (iron silicon boron) magnetic particles of 400-500 mesh were obtained by sieving through a sieve, and a gas-liquid interface self-assembled film was prepared by an automated self-assembly method; and the magnetic particles were transferred to the MA surface by a water transfer method, and heated and dried to obtain a magnetic particle-MA composite film with a thickness of about 38 μm.
[0077] 4) Liquid metal (pure gallium) particles with a particle size of 25-32 μm were prepared by microtube jetting, and a gas-liquid interface self-assembled film was prepared by automated self-assembly; then the film was transferred to the surface of the magnetic particle functional layer, heated and dried, and composited with the lower surface to obtain a liquid metal-magnetic particle-MA composite film. The thickness of the liquid metal shielding layer was about 30 μm, and the total thickness was about 68 μm.
[0078] 5) The membrane was pasted on the roller of the electrospinning machine, and then the MA solution was spun on the receiving roller of the electrospinning machine at a speed of 150 rpm for 15 minutes to obtain a spinning encapsulation layer.
[0079] The thickness of the functional layer in this multifunctional conformal functional composite particle film is 68μm. It has electromagnetic shielding and conductive functions, and after testing, its electromagnetic shielding performance is greater than 40dB, and the square resistance is evenly distributed in 500-1200mΩ / □.
[0080] In addition, this multifunctional conformal functional composite particle film has good stability. When the surface of the composite film is repeatedly scraped with a face scraper under a pressure greater than 1N, no particles fall off the surface, and the conductive and shielding properties remain stable after scraping.
[0081] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.
Claims
1. A method for preparing a conformal particle film, characterized in that: include: coating an adhesive material on a substrate to form an adhesive layer conformal to the substrate; The metal particle precipitate is prepared into a gas-liquid interface self-assembled film by using an automated self-assembly device and an electric propulsion method; Attaching the air-liquid interface self-assembled film on the adhesion layer conformal to the substrate to form a functional layer; wherein the thickness of the functional layer is controllable; Drying is performed to obtain a conformal particle film attached to the surface of the substrate; wherein, in the conformal particle film, part of the metal particles of the gas-liquid interface self-assembled film are embedded in the adhesion layer.
2. A method for preparing a conformal functional composite particle film, characterized in that: include: coating an adhesive material on a substrate to form an adhesive layer conformal to the substrate; The corresponding gas-liquid interface self-assembled films are prepared by using multiple automated self-assembly devices in an electric propulsion mode to precipitate each metal particle; Sequentially attaching each gas-liquid interface self-assembled film on the adhesion layer conforming to the substrate to form a functional layer by stacking the single layers; wherein each gas-liquid interface self-assembled film is the same or different; and the thickness of the functional layer is controllable; Drying is performed to obtain a conformal functional composite particle film attached to the surface of the substrate; wherein, in the conformal functional composite particle film, part of the metal particles of the gas-liquid interface self-assembled film are embedded in the adhesion layer.
3. The method for preparing a conformal functional composite particle film according to claim 2, characterized in that: The automated self-assembly device comprises: a film-making container, a bracket located on one side of the film-making container, and an electric propulsion control device; wherein the electric propulsion control device comprises: a controller, a controllable telescopic motor and a remote controller connected to the controller, and a powder carrier connected to the end of a push rod of the controllable telescopic motor, wherein the controllable telescopic motor is mounted on the bracket and is located directly above the film-making container.
4. The method for preparing a conformal functional composite particle film according to claim 3, characterized in that: Each automated self-assembly device uses electric propulsion to prepare the corresponding gas-liquid interface self-assembled film from the metal particle precipitate, including the following steps: According to functional requirements, metal particles are determined, placed in a solvent for ultrasonic dispersion, and allowed to stand to obtain a precipitate; Add water to the film-making container; place the precipitate in a powder carrier at the end of the controllable telescopic motor push rod, and make the powder carrier be located above the liquid level in the film-making container; The propulsion amount of the controllable telescopic motor is electrically controlled by a remote control to drive the powder carrier into the liquid surface in the film-making container, and the position of the powder carrier in the vertical direction is adjusted to keep the sediment inside it always at the air / water interface, thereby self-assembling to form a gas-liquid interface self-assembled film.
5. The method for preparing a conformal functional composite particle film according to claim 4, characterized in that: The adhesive layer conforming to the substrate is sequentially placed below the air-liquid interface self-assembled film in each film-forming container, and each air-liquid interface self-assembled film is attached by lifting up.
6. The method for preparing a conformal functional composite particle film according to claim 2, characterized in that: The particle size of the metal particles is 0.1-100 μm; The metal particles are metal single substance particles or alloy particles; The metal component contained in the metal particles is any one or more of Ga, Ti, Fe, Co and Ni.
7. The method for preparing a conformal functional composite particle film according to claim 6, characterized in that: The adhesive material is coated on the substrate by electrospinning or planar spin coating; The method, before the drying step, further comprises: using a spinning process to attach the encapsulation material to the surface of the functional layer to form an encapsulation layer; Wherein, the adhesive material and packaging material are any one of MA, PDMS, PU, Ecoflex, SEBS, PP, PU, TPE, LSR, LVER, and TPU solution.
8. The method for preparing a conformal functional composite particle film according to claim 2, characterized in that: The method is used for mass production of large-area conformal functional composite particle films.
9. A conformal particle film, characterized in that The conformal particle film is prepared by the method for preparing the conformal particle film according to claim 1, and comprises an adhesion layer and a functional layer conformal to the substrate, wherein the functional layer is a gas-liquid interface self-assembled film.
10. A conformal functional composite particle film, characterized in that: The film is prepared by the method for preparing a conformal functional composite particle film according to any one of claims 2 to 8, and comprises an adhesion layer and a functional layer conformal to a substrate in sequence, wherein the functional layer is composed of a multilayer gas-liquid interface self-assembled film.