Catalyst based on cobalt-nickel synergistic effect and application thereof
By preparing Na2Co2-xNixTeO6 catalyst, the complex and stability problems of existing catalyst synthesis are solved, and efficient and stable oxygen precipitation reaction is achieved. It is suitable for clean energy production, replace fossil fuels and reduce carbon emissions.
Patent Information
- Application Number
- CN202411194929.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The synthesis process of existing cobalt and nickel-based oxygen precipitation reaction catalysts is complex, which limits its large-scale preparation and industrial application, and its performance under long-term stability and high potential conditions need further verification.
Na2Co2-xNixTeO6 is used as a catalyst to prepare through the steps of grinding, calcining and sintering to optimize the doping ratio and sintering conditions of cobalt and nickel, and improve the performance and stability of the catalyst.
It significantly improves the performance and stability of the catalyst, reduces costs, and is suitable for clean energy hydrogen production in industrial production, replaces traditional fossil fuel power generation, and reduces carbon dioxide emissions.
Smart Images

Figure CN119079936A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials, and in particular to a high-efficiency catalyst for catalyzing water decomposition and a preparation method thereof. Background Art
[0002] The pursuit of efficient and sustainable energy conversion technologies has driven the intensive study of electrocatalysts, especially the oxygen evolution reaction (OER). OER is a key process in water electrolysis and metal-air batteries, and is the fundamental reaction for producing clean hydrogen fuel from renewable energy. Transition metal-based catalysts have attracted much attention due to their high performance, multivalent states, and abundant reserves.
[0003] Among these catalysts, cobalt-based catalysts have attracted extensive attention and research, including cobalt oxides, phosphides, nitrides, phosphates, sulfides, and selenides. In recent years, researchers have increasingly explored the introduction of nickel (Ni) into cobalt (Co) compounds to enhance their oxygen evolution reaction performance, a strategy that exploits synergistic effects and structural modifications.
[0004] Research from Lanzhou University of Technology shows that the excellent performance of Co3Ni1-NC is attributed to its unique crumpled carbon nanosphere structure and the synergistic effect between Co-Ni alloy nanoparticles and nitrogen-doped carbon layers, which provide multiple active sites and accelerate the reaction rate. Crumpled nitrogen-doped carbon nanospheres were synthesized using a soft template method, and cobalt and nickel salts were added to prepare bimetallic Co-Ni alloy nanoparticles. By incorporating melamine as a nitrogen source, the distribution and content of active sites were improved, and the surface area and active site density of the catalyst were increased. The oxygen evolution reaction (OER) performance was tested. Co3Ni1-N–C exhibited OER electrocatalytic performance at 10 mA / cm 2 The overpotential under current density is 0.360V, and the Tafel slope is 100mV / dec, which has a high overpotential and Tafel slope. However, its synthesis process is relatively complicated, including multi-step synthesis and specific experimental conditions, which limits the possibility of large-scale preparation and industrial application. And there is no further exploration of the doping ratio of cobalt and nickel. Although it shows good stability in short-term tests, the stability in long-term and complex environments still needs further verification and research, especially under high potential conditions. The migration and aggregation of metal particles may affect the long-term performance of the catalyst. Although a variety of characterization techniques are used for performance analysis, there are still challenges in understanding the microstructure and reaction mechanism of the active sites, which requires more in-depth research and analysis. Summary of the invention
[0005] Problem that the invention aims to solve
[0006] In order to solve the above problems existing in the prior art, the present invention provides a highly efficient oxygen evolution reaction electrocatalyst method, which utilizes the synergistic effect and structural modification of cobalt and nickel to improve the catalytic performance.
[0007] Solutions for solving problems
[0008] The present invention provides a catalyst, the general chemical formula of which is Na2Co 2-x Ni x TeO6, the value range of x is 0≤x≤1, and the value of x satisfies the charge balance of the chemical formula.
[0009] Preferably, x is 0, 0.4, 0.8 or 1.0.
[0010] The present invention provides a method for preparing the above catalyst, comprising the following steps:
[0011] S1: taking precursor materials Na2CO3, CoO, NiO and TeO2, grinding and mixing them to obtain a mixture;
[0012] S2: calcining the mixture obtained in step S1 to obtain a precursor;
[0013] S3: Sinter the precursor obtained in step S2 to obtain a catalyst.
[0014] Preferably, in the step S1, the grinding is performed using an agate mortar.
[0015] Preferably, the grinding time is 20-100 min, preferably 20-60 min, more preferably 40 min.
[0016] Preferably, the calcination in step S2 and the sintering in step S3 are performed in a crucible.
[0017] Preferably, the crucible is one of a corundum crucible and a porcelain crucible, preferably a corundum crucible, and more preferably an alumina crucible.
[0018] Preferably, in step S2, the calcination temperature is 600°C to 700°C, the heating rate is 4°C / min to 6°C / min, and the calcination time is 10 hours to 20 hours.
[0019] Preferably, in step S2, cooling is required after roasting.
[0020] More preferably, the temperature after cooling is 20°C to 30°C, and the cooling rate is 4°C / min to 6°C / min.
[0021] Preferably, the calcination temperature is 650° C., the heating rate is 5° C. / min, and the calcination time is 10 to 15 hours.
[0022] Preferably, the temperature after cooling is 25°C, and the cooling rate is 5°C / min.
[0023] Preferably, in step S3, the sintering temperature is 700-900° C., the heating rate is 4° C. / min-6° C. / min, and the sintering time is 20 hours-30 hours.
[0024] Preferably, in the step S3, grinding is required before sintering.
[0025] Preferably, the grinding is performed using an agate mortar; the grinding time is 20-100 min, preferably 20-60 min, and more preferably 40 min.
[0026] Preferably, in step S3, cooling is required after sintering.
[0027] More preferably, the temperature after cooling is 20°C to 30°C, and the cooling rate is 4°C / min to 6°C / min.
[0028] Preferably, the sintering temperature is 810° C., the heating rate is 5° C. / min, and the sintering time is 23 hours to 27 hours.
[0029] Preferably, the temperature after cooling is 25°C, and the cooling rate is 5°C / min.
[0030] The present invention provides the above catalyst and the catalyst prepared by the above preparation method for use in the process of producing hydrogen by electrolysis of water.
[0031] Effects of the Invention
[0032] The present invention provides a Na2Co 2-x Ni x TeO6 catalyst not only improves the performance of the catalyst, but also significantly enhances its stability and durability in practical applications, providing important theoretical and practical guidance for future energy conversion technologies. 2-x Ni x As a catalyst for catalyzing OER reactions, TeO6 has good durability, high activity and low cost. Compared with other precious metals such as Pt, Ru and Ir, it can be widely used in industrial production, such as the production of clean energy hydrogen. It can replace traditional fossil fuel power generation methods, reduce carbon dioxide emissions, protect the environment, and combine with renewable energy systems such as photovoltaics to achieve efficient water decomposition, convert hydrogen into electricity through fuel cells, and realize energy storage and reuse.
[0033] The present invention provides a method for synthesizing Na2Co by a spontaneous combustion solid phase reaction method. 2-x Nix By optimizing the mixing ratio and sintering conditions of the precursor materials and enhancing the catalytic performance by cobalt and nickel doping, an efficient and stable OER electrocatalyst was finally achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The Na2Co prepared in Example 1-4 2–x Ni x SEM images of TeO6 (x=0, 0.4, 0.8, 1.0) catalysts.
[0035] Figure 2 The Na2Co prepared in Example 1-4 2–x Ni x XRD diffraction patterns of TeO6 (x=0, 0.4, 0.8, 1.0) catalysts.
[0036] Figure 3 The Na2Co prepared in Example 1-4 2–x Ni x Electrocatalytic oxygen evolution reaction performance diagram of TeO6 (x=0, 0.4, 0.8, 1.0) catalyst. DETAILED DESCRIPTION
[0037] In order to make the technical solutions and beneficial effects of the present invention more clearly understandable, the following is a detailed description by listing specific embodiments. The drawings are not necessarily drawn to scale, and local features may be enlarged or reduced to more clearly show the details of the local features; unless otherwise defined, the technical and scientific terms used herein have the same meanings as those in the technical field to which this application belongs.
[0038] In one aspect, the present invention provides a catalyst having a general chemical formula of Na2Co 2-x Ni x TeO6, the value range of x is 0≤x≤1, and the value of x satisfies the charge balance of the chemical formula.
[0039] In certain embodiments, x is 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1.0.
[0040] In certain embodiments, x is 0, 0.4, 0.8 or 1.0.
[0041] In one aspect, the present invention provides a method for preparing the above catalyst, comprising the following steps:
[0042] S1: taking precursor materials Na2CO3, CoO, NiO and TeO2, grinding and mixing them to obtain a mixture;
[0043] S2: calcining the mixture obtained in step S1 to obtain a precursor;
[0044] S3: Sinter the precursor obtained in step S2 to obtain a catalyst.
[0045] In certain embodiments, in step S1, when x is 0, the molar ratio of Na2CO3, CoO and TeO2 is Na2CO3:CoO:TeO2=1:2:1.
[0046] In certain embodiments, in step S1, when x is 0.4, the molar ratio of Na2CO3, CoO, NiO and TeO2 is Na2CO3:CoO:NiO:TeO2=1:1.6:0.4:1.
[0047] In certain embodiments, in step S1, when x is 0.8, the molar ratio of Na2CO3, CoO, NiO and TeO2 is Na2CO3:CoO:NiO:TeO2=1:1.2:0.8:1.
[0048] In certain embodiments, in step S1, when x is 1, the molar ratio of Na2CO3, CoO, NiO and TeO2 is Na2CO3:CoO:NiO:TeO2=1:1:1:1.
[0049] In certain embodiments, in step S1, the grinding is performed using an agate mortar.
[0050] In certain embodiments, the grinding time is 20-100 min.
[0051] In certain embodiments, the grinding time is 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min, or 100 min.
[0052] In certain embodiments, the calcination in step S2 is performed in a crucible.
[0053] In certain embodiments, the crucible is one of a corundum crucible and a porcelain crucible.
[0054] In certain embodiments, the crucible is a corundum crucible.
[0055] In certain embodiments, the crucible is an alumina crucible.
[0056] In certain embodiments, in step S2, the calcination temperature is 600°C to 700°C, the heating rate is 4°C / min to 6°C / min, and the calcination time is 10 hours to 20 hours.
[0057] In certain embodiments, in step S2, the calcination temperature is 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, or 700°C; the heating rate is 4°C / min, 5°C / min, or 6°C / min; and the calcination time is 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, or 20 hours.
[0058] In certain embodiments, in step S2, the calcination temperature is 650°C, the heating rate is 5°C / min, and the calcination time is 10 hours to 15 hours.
[0059] In certain embodiments, in step S2, cooling is required after calcination.
[0060] In certain embodiments, the temperature after cooling is 20°C to 30°C, and the cooling rate is 4°C / min to 6°C / min.
[0061] In certain embodiments, the temperature after cooling is 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, or 30°C, and the cooling rate is 4°C / min, 5°C / min, or 6°C / min.
[0062] In certain embodiments, in step S2, the temperature after cooling is 25°C, and the cooling rate is 5°C / min.
[0063] In certain embodiments, the sintering in step S3 is performed in a crucible.
[0064] In certain embodiments, the crucible is one of a corundum crucible and a porcelain crucible.
[0065] In certain embodiments, the crucible is a corundum crucible.
[0066] In certain embodiments, the crucible is an alumina crucible.
[0067] In certain embodiments, in step S3, the sintering temperature is 700-900° C., the heating rate is 4° C. / min-6° C. / min, and the sintering time is 20 hours-30 hours.
[0068] In certain embodiments, in step S3, the sintering temperature is 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, the heating rate is 4°C / min, 5°C / min, 6°C / min, and the sintering time is 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours, 30 hours.
[0069] In certain embodiments, in step S3, the sintering temperature is 810°C, the heating rate is 5°C / min, and the sintering time is 23 hours to 27 hours.
[0070] In certain embodiments, in step S3, grinding is required before sintering.
[0071] In certain embodiments, the grinding is performed with an agate mortar.
[0072] In certain embodiments, the grinding time is 20-100 min.
[0073] In certain embodiments, the grinding time is 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, 65 min, 70 min, 75 min, 80 min, 85 min, 90 min, 95 min, or 100 min.
[0074] In certain embodiments, in step S3, cooling is required after sintering.
[0075] In certain embodiments, the temperature after cooling is 20°C to 30°C, and the cooling rate is 4°C / min to 6°C / min.
[0076] In certain embodiments, the temperature after cooling is 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, or 30°C, and the cooling rate is 4°C / min, 5°C / min, or 6°C / min.
[0077] In certain embodiments, the temperature after cooling is 25°C, and the cooling rate is 5°C / min.
[0078] On the one hand, the present invention provides the above-mentioned catalyst and the catalyst prepared by the above-mentioned preparation method for use in the process of electrolyzing water to produce hydrogen.
[0079] The method of the present invention is described below by means of specific examples. It should be understood that these examples are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following examples; the implementation conditions adopted in the examples can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in routine experiments.
[0080] In the following examples, unless otherwise indicated, all temperatures are degrees Celsius. Unless otherwise indicated, various starting materials and reagents are commercially available or synthesized according to known methods. Commercially available materials and reagents are used directly without further purification. Unless otherwise indicated, commercial manufacturers include but are not limited to DANIINGPAI, ALADDIN, SCR, DAMAS-BETA, etc.
[0081] Example 1 Preparation of Na2Co2TeO6 polycrystalline sample
[0082] Take the precursor materials Na2CO3 (DANIINGPAI, 99.8+%), CoO (ALADDIN, 99.9%) and TeO2 (damas-beta, 99.99%) and mix them in a molar ratio of Na2CO3: CoO: TeO2 = 1: 2: 1, and grind them with an agate mortar for 40 minutes to ensure sufficient mixing. The mixture is placed in an alumina crucible, heated from 25°C to 650°C at a rate of 5°C / min for 12 hours in an air environment, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain a precursor material. After cooling, the obtained powder is re-ground and placed in an alumina crucible again, and heated from 25°C to 810°C at a rate of 5°C / min in an air environment for 24 hours, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain a Na2Co2TeO6 polycrystalline sample.
[0083] Example 2 Preparation of Na2Co 1.6 Ni 0.4 TeO6 polycrystalline sample
[0084] Take the precursor materials Na2CO3 (DANIINGPAI, 99.8+%), CoO (ALADDIN, 99.9%), NiO (SCR, 98.0+%) and TeO2 (damas-beta, 99.99%) and mix them in a molar ratio of Na2CO3:CoO:NiO:TeO2=1:1.6:0.4:1, and grind them with an agate mortar for 40 minutes to ensure sufficient mixing. The mixture is placed in an alumina crucible, and heated from 25°C to 650°C at a rate of 5°C / min for 12 hours in an air environment, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain a precursor material. After cooling, the obtained powder is re-ground and placed in an alumina crucible again, and heated from 25°C to 810°C at a rate of 5°C / min in an air environment for sintering for 24 hours, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain Na2Co 1.6 Ni 0.4 TeO6 polycrystalline sample.
[0085] Example 3 Preparation of Na2Co 1.2 Ni 0.8 TeO6 polycrystalline sample
[0086] Take the precursor materials Na2CO3 (DANIINGPAI, 99.8+%), CoO (ALADDIN, 99.9%), NiO (SCR, 98.0+%) and TeO2 (damas-beta, 99.99%) and mix them in a molar ratio of Na2CO3:CoO:NiO:TeO2=1:1.2:0.8:1, and grind them with an agate mortar for 40 minutes to ensure thorough mixing. The mixture is placed in an alumina crucible, heated from 25°C to 650°C at a rate of 5°C / min for 12 hours in an air environment, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain a precursor material. After cooling, the obtained powder is re-ground and placed in an alumina crucible again, and heated from 25°C to 810°C at a rate of 5°C / min in an air environment for sintering for 24 hours, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain Na2Co 1.2 Ni 0.8 TeO6 polycrystalline sample.
[0087] Example 4 Preparation of Na2CoNiTeO6 polycrystalline sample
[0088] Precursor materials Na2CO3 (DANIINGPAI, 99.8+%), CoO (ALADDIN, 99.9%), NiO (SCR, 98.0+%) and TeO2 (damas-beta, 99.99%) were mixed in a molar ratio of Na2CO3:CoO:NiO:TeO2=1:1:1:1, and ground with an agate mortar for 40 minutes to ensure full mixing. The mixture was placed in an alumina crucible, heated from 25°C in an air environment at a rate of 5°C / min to 650°C for 12 hours, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain a precursor material. After cooling, the obtained powder was re-ground and loaded into the alumina crucible again, and the temperature was increased from 25°C to 810°C at a rate of 5°C / min in an air environment, and sintered for 24 hours, and then cooled to room temperature 25°C at a rate of 5°C / min to obtain a Na2CoNiTeO6 polycrystalline sample.
[0089] Example 5Na2Co 2–x Ni x Catalytic performance test of TeO6 (x=0, 0.4, 0.8, 1.0)
[0090] 5 mg of Na2Co 2–x Ni x TeO6 (x = 0, 0.4, 0.8, 1.0) powder was dispersed in a solution consisting of 250uL deionized water, 250uL ethanol and 25uL Nafion solution (0.5%), and ultrasonically treated for 30 minutes to ensure its uniformity. After the preparation was completed, 2μL of catalyst ink was dropped on the surface of the glassy carbon electrode and dried at room temperature for 2 hours. The addition of Nafion solution is intended to improve the stability and dispersibility of the powder on the electrode surface. In the three-electrode reaction system, the reference electrode selected is a saturated calomel electrode, and the counter electrode is a carbon rod electrode, where the rotation speed of the rotating disk electrode is set to 1600rpm. First, different scanning speeds of 5mV / s, 10mV / s, and 20mV / s were used to see whether linear sweep voltammetry (LSV) has performance in 1.0M KOH solution, and then the obtained material was subjected to OER cycle test at a scanning rate of 5mV / s, and the number of cycles was 100 times, 200 times, and 300 times, respectively. The specific results of the OER test are as follows Figure 3 As shown in Figure 2, the catalytic performance increases with the increase of nickel content. When x = 1.0, Na2CoNiTeO6 shows the best activity at 10 mA / cm 2 The minimum onset potential of 1.53 V was achieved at this current density, showing only an overpotential of 0.300 V, which is comparable to commercial RuO2. Figure 3 (a). Further adopt Figure 3The Tafel curve shown in (b) provides insight into the catalytic performance, and it is found that when the concentrations of cobalt and nickel are equal, the slope decreases from 108 mV / dec to a minimum of 58 mV / dec. 2–x Ni x The stability of TeO6 in the oxygen evolution reaction (OER) was tested by 100 to 300 cyclic voltammetry (CV) at 1.3 V to 1.8 V vs. RHE. Figure 3 (c)-(f). In general, Na2Co 2–x Ni x TeO6 (x = 0, 0.4, 0.8, 1.0) exhibited robust stability as OER catalysts, maintaining their performance over 300 cycles with minimal degradation. Such stability is critical for practical applications in water splitting and other electrochemical processes, where long-term durability of the catalyst is essential.
[0091] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.
Claims
1. A catalyst, It is characterized in that The general chemical formula of the catalyst is Na 2 Co 2-x Ni x TeO 6 , the value range of x is 0≤x≤1, and the value of x satisfies the charge balance of the chemical formula.
2. The catalyst according to claim 1, It is characterized in that The x is 0, 0.4, 0.8 or 1.
0.
3. A method for preparing the catalyst as claimed in claim 1, It is characterized in that The following steps are involved: S1: Take the precursor material Na 2 CO 3 , CoO, NiO and TeO 2 , grinding and mixing to obtain a mixture; S2: calcining the mixture obtained in step S1 to obtain a precursor; S3: Sinter the precursor obtained in step S2 to obtain a catalyst.
4. The preparation method according to claim 3, It is characterized in that In the step S1, the grinding is performed using an agate mortar; Preferably, the grinding time is 20-100 min, preferably 20-60 min, more preferably 40 min.
5. The preparation method according to claim 3, It is characterized in that The calcination in step S2 and the sintering in step S3 are carried out in a crucible; Preferably, the crucible is one of a corundum crucible and a porcelain crucible, preferably a corundum crucible, and more preferably an alumina crucible.
6. The preparation method according to any one of claims 3 to 5, It is characterized in that In step S2, the calcination temperature is 600°C to 700°C, the heating rate is 4°C / min to 6°C / min, and the calcination time is 10 hours to 20 hours; Preferably, in step S2, after roasting, cooling is required; More preferably, the temperature after cooling is 20°C to 30°C, and the cooling rate is 4°C / min to 6°C / min.
7. The preparation method according to claim 6, It is characterized in that The calcination temperature is 650°C, the heating rate is 5°C / min, and the calcination time is 10 to 15 hours; Preferably, the temperature after cooling is 25°C, and the cooling rate is 5°C / min.
8. The preparation method according to claim 3, It is characterized in that In step S3, the sintering temperature is 700-900°C, the heating rate is 4°C / min-6°C / min, and the sintering time is 20 hours-30 hours; Preferably, in the step S3, grinding is required before sintering; Preferably, the grinding is performed with an agate mortar; the grinding time is 20-100 min, preferably 20-60 min, more preferably 40 min; Preferably, in step S3, cooling is required after sintering; More preferably, the temperature after cooling is 20°C to 30°C, and the cooling rate is 4°C / min to 6°C / min.
9. The preparation method according to claim 8, It is characterized in that The sintering temperature is 810°C, the heating rate is 5°C / min, and the sintering time is 23 hours to 27 hours; Preferably, the temperature after cooling is 25°C, and the cooling rate is 5°C / min.
10. Use of the catalyst according to any one of claims 1 to 2 and the catalyst prepared by the preparation method according to any one of claims 3 to 9 in a process of producing hydrogen by electrolysis of water.
Citation Information
Patent Citations
Preparation method of modified sodium ion battery positive electrode material, positive electrode plate and battery
CN114914390A
Slurry for positive electrode of potassium ion secondary battery, positive electrode, potassium ion secondary battery, and resin composition for positive electrode of potassium ion secondary battery
JP2022119351A
Layered oxide materials for batteries