Preparation method of high-compaction-density iron phosphate

By controlling the pH value of monoammonium phosphate and the excess of iron, floc complexes are generated to avoid sulfate wrapping, combined with segmented aging and multi-step filtration and washing, the problem of sulfate wrapping during the growth of iron phosphate crystals is solved, and the problem of sulfate wrapping during the growth of iron phosphate crystals is improved. The purity and compaction density of iron phosphate are improved, and the performance of lithium batteries is improved.

CN119079957AActive Publication Date: 2024-12-06GUIZHOU PHOSPHATING NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411210651.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

In the prior art, iron phosphate is prone to wrap the sulfate in the reaction liquid during crystal growth, resulting in a decrease in product purity and a synchronous increase in crystal size and sulfur content, affecting the performance of lithium batteries.

Method used

By controlling the pH value of monoammonium phosphate and the excess of iron, Fe3H6(PO4)43+ ions are generated to form floc complexes, avoid sulfate wrapping, and improve the purity of iron phosphate through segmented aging and multi-step filtration washing and Compact density.

Benefits of technology

It significantly improves the purity and compaction density of iron phosphate, reduces the sulfur content, and improves the performance and product quality of lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079957A_ABST
    Figure CN119079957A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of production of iron phosphate, and particularly discloses a preparation method of high-compaction-density iron phosphate. Comprising the following five steps: preparing a ferrous sulfate solution, preparing a solution, oxidizing and reacting, washing and filtering, aging in sections, filtering, washing, drying and calcining, reacting monoammonium phosphate and ferric sulfate, controlling the pH value change of the reaction, enabling the reaction to be carried out in two steps, carrying out one-step 3Fe < 3 + > + 4H3PO4 = Fe3H6 (PO4) 43 < 3 + > + 6H < + > complex reaction, adsorbing SO4 < 2 + > by Fe3H6 (PO4) 43 < 3 + > ions to form a complex, and carrying out secondary purification on the complex. The technical problem that impurities exist in a final iron phosphate product due to the fact that sulfate in reaction liquid is easily wrapped by iron phosphate crystals in the growth process when iron phosphate is prepared in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ferric phosphate production, and in particular to a method for preparing high-density ferric phosphate. Background Art

[0002] The chemical formula of iron phosphate is FePO4. It is an inorganic compound that can be used as an important precursor of lithium iron phosphate, the positive electrode material of lithium-ion batteries. In recent years, lithium-ion batteries, as a new generation of green batteries, have attracted widespread attention due to their high theoretical capacity, high voltage, low self-discharge rate, excellent cycle performance, wide operating temperature range and environmental friendliness. With the continuous expansion of new energy vehicles and energy storage, the demand for lithium-ion batteries is also growing rapidly. As an important precursor for the synthesis of lithium iron phosphate, the preparation process and product quality of iron phosphate have a direct impact on the performance, quality and cost of lithium iron phosphate positive electrode materials. How to obtain iron phosphate with stable quality, good uniformity and low cost is a hot topic of great concern in the lithium battery industry.

[0003] In the prior art, the production process of iron phosphate mainly includes liquid phase precipitation method. The liquid phase precipitation method mainly uses iron sulfate and phosphate as raw materials, performs oxidation reaction in aqueous solution, and performs aging, filtration, drying and calcination after oxidation to generate iron phosphate products. In the process of generating iron phosphate by oxidation reaction, the product will go through two stages: crystal nucleation and crystal growth. The initial stage of the reaction is the stage of iron phosphate crystal nucleation, forming a large number of fine iron phosphate crystal nuclei with small particle size and high purity. However, after entering the crystal growth stage, the crystal nuclei gradually grow and are easy to encapsulate sulfate in the reaction solution to form a mixture of FePO4·xMSO4. Therefore, in the crystal growth stage, the crystal size of iron phosphate and the sulfur content in the crystal increase synchronously, and the encapsulated sulfate affects the purity of the iron phosphate product, and the performance of the lithium iron phosphate battery prepared therefrom is also affected. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing high compaction density iron phosphate, so as to solve the technical problem that when preparing iron phosphate in the prior art mentioned above, iron phosphate crystals are easily wrapped with sulfate in the reaction solution during the growth process, resulting in impurities in the final iron phosphate product.

[0005] In order to solve the above problems, the technical solution adopted by the present invention is as follows: a method for preparing high compaction density iron phosphate, comprising the following steps:

[0006] S1: Prepare ferrous sulfate solution: Mix titanium dioxide slag with desalted water, add phosphoric acid, ammonia water and flocculant to pretreat the solution, filter to remove suspended insoluble matter after complete dissolution, and obtain FeSO4·7H2O solution after suction filtration;

[0007] S2: Liquid preparation for oxidation and reaction: Calculate the required amount of phosphoric acid while ensuring that the iron excess is 8%-12%, prepare phosphoric acid and ammonia water into a monoammonium phosphate solution, and control the pH value of the monoammonium phosphate solution to 6.5-7.5, mix the monoammonium phosphate solution with the FeSO4·7H2O solution prepared in S1, and slowly add hydrogen peroxide to the mixed solution for oxidation reaction, and the pH value of the final reaction is controlled between 2-3;

[0008] S3: washing and filtration: add desalted water to the filter cake after suction filtration of the mixed solution at a ratio of 1:3 between material and water, and repeat the washing and filtration three times to obtain iron phosphate.

[0009] The beneficial effects of this embodiment are:

[0010] 1. In the process of oxidative synthesis of iron phosphate in the prior art, after the iron phosphate crystal is generated and enters the crystal growth stage, the crystal nucleus gradually grows and tends to wrap the sulfate in the reaction solution to form a mixture of FePO4·xMSO4. Therefore, in the crystal growth stage, the crystal size of iron phosphate and the sulfur content in the crystal increase synchronously, and the wrapped sulfate affects the product purity of iron phosphate. In the present application, the iron content is excessive and the pH value of monoammonium phosphate is controlled, so that during the reaction, the oxidized Fe 3+ The ions do not directly react with phosphate to form FePO4, but first react to form Fe3H6(P04)4 3+ Ion, Fe3H6(P04)4 3+ and SO4 2+ Forming flocculent complexes, so that when iron phosphate is generated, it will not wrap SO4 2+ , the reaction equation is as follows: First reaction: 3Fe 3+ +4H3PO4=Fe3H6(PO4)4 3+ +6H + , the second reaction: Fe3H6(P04)4 3+ +6H20=3FePO4*2H20+H3PO4+3H + The reaction process is as follows: At the beginning, due to the high pH value of monoammonium phosphate, the pH value of the mixed solution of ferrous iron and monoammonium phosphate is also high. After adding hydrogen peroxide, the first reaction proceeds forward, and the generated Fe3H6(PO4)4 3+ and SO4 2+ When the complex is formed, H + The pH value of the mixed solution decreases. After the pH value decreases, a pH environment is provided for the formation of iron phosphate. Most of the other Fe 3+ Iron phosphate can be generated normally, the reaction formula is: 2FeSO4+H2PO 4- +H2O2→FePO4↓+2SO4 2-+H2O; as the amount of hydrogen peroxide continues to increase, a large amount of Fe3H6(PO4)4 is generated 3+ At the same time, the pH is further reduced, and the first reaction is Fe3H6(PO4)4 3+ The resulting reaction is inhibited or reversed, and due to Fe3H6(PO4)4 3+ If the concentration is too high, the second reaction will proceed forward to generate iron phosphate, which will release sulfate. At this time, since most of the iron phosphate has completed crystal growth, the influence of sulfate is very small. Therefore, the purity of the iron phosphate in the product of this application is relatively high.

[0011] 2. In the prior art, since the iron phosphate is synthesized by oxidation in one step, the crystal size of the synthesized iron phosphate is consistent, so that when compacted, the gaps between the particles cannot be filled. The iron phosphate in this application is generated in two parts, namely: Fe2(SO4)3+2NH4H2PO4=2FePO4+(NH4)2SO4+2H2SO4, Fe3H6(PO4)4 3+ +6H20=3FePO4*2H20+H3PO4+3H + The iron phosphate generated by the first reaction will slowly grow into large particles due to its slow reaction and the absence of sulfate interference, and will form square dihydrate iron phosphate after aging. The other part of the iron phosphate generated by the second reaction will precipitate from the complex ions in the later stage and will be adsorbed on the surface of the large iron phosphate generated by the first reaction, and will form amorphous fine particles after aging. During compaction, the fine particles will be forced to be added to the gaps in the square crystals, so its compaction density is higher than the compaction density of the sheet-like or square iron phosphate in the prior art.

[0012] Further, S4: staged aging: add desalted water to the filter cake after filtering in S3 at a material ratio of 1:2 to water, stir evenly and then raise the solution temperature to 55-65°C, add ammonia water to the solution, control the pH value of the reaction solution between 1.8-2.4, keep warm for 1-2 hours for the first stage of aging, raise the temperature to 90-100°C, add phosphoric acid, keep warm for 3-4 hours for the second stage of aging, and precipitate FePO4·2H2O; S5: filtering, washing, drying and calcining: filter the aged solution and add desalted water to wash at a material ratio of 1:2 to water, filter and dry after washing, and calcine the dried sample to obtain the iron phosphate product.

[0013] Furthermore, the iron-phosphorus ratio in the S2 is 1.1:1.

[0014] Furthermore, the pH value of the monoammonium phosphate in S2 is controlled to be 7, and the pH of the final reaction is controlled between 2.2-2.3.

[0015] Furthermore, in the S4, the first stage aging temperature is controlled at 60° C., the pH value is controlled at 2.2-2.3, and the insulation time is controlled at 1 hour.

[0016] Furthermore, the second stage aging temperature in S4 is controlled to be 95° C., and the insulation time is controlled to be 3 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM image of the iron phosphate product of Example 1 of the present invention. DETAILED DESCRIPTION

[0018] The following is further described in detail through specific implementation methods:

[0019] First, it should be understood that when used in the present specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, wholes, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or collections thereof.

[0020] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, the singular forms "a", "an" and "the" are intended to include plural forms unless the context clearly indicates otherwise.

[0021] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0022] Example 1

[0023] S1: Prepare ferrous sulfate solution

[0024] After titanium dioxide slag is mixed with desalted water, where titanium dioxide slag refers to the solid byproduct of ferrous sulfate produced by the sulfuric acid process to produce titanium dioxide, desalted water is added at 1.5-2.5 times the mass of titanium dioxide slag to dissolve, and ammonium phosphate is added to adjust the pH to 2-3, so that the ferrous sulfate in the titanium dioxide slag is dissolved in the water body. After stirring and dissolving for 1-2 hours, a flocculant is added to pretreat the undissolved impurities in the titanium dioxide slag in the solution. The flocculant flocculates small particles of impurities into suspended insoluble impurity clusters. After complete dissolution, the suspended insoluble matter is filtered to remove the suspended insoluble matter, and a FeSO4·7H2O solution is obtained after suction filtration. The concentration of the FeSO4·7H2O solution is controlled at 4% to 6%.

[0025] S2: Liquid oxidation and reaction

[0026] The required amount of phosphoric acid is calculated according to the iron-phosphorus ratio of 1.1:1. Ammonia water is added to the required phosphoric acid to react with phosphoric acid and ammonia water to form a monoammonium phosphate solution. The pH value is adjusted to 7 with ammonia water. After the monoammonium phosphate solution is prepared, it is directly mixed with the FeSO4·7H2O solution for reaction. Since no oxidant is added, the reaction does not proceed. After the monoammonium phosphate and FeSO4·7H2O solution are evenly mixed, since the pH value of the monoammonium phosphate solution is 7, the pH value of the mixed solution after mixing with the FeSO4·7H2O solution is relatively high, about 4.0. At this time, hydrogen peroxide is slowly added to the mixed solution to oxidize the divalent iron into trivalent iron. Since there is no pH environment for the generation of iron phosphate, iron phosphate is not directly generated at this time, but 3Fe 3+ +4H3PO4=Fe3H6(PO4)4 3+ +6H + The coordination reaction generates Fe3H6(PO4)4 3+ and H + , H + The pH value of the mixed solution is reduced, creating a pH environment for the formation of iron phosphate, and then most of the Fe3 + The normal reaction produces iron phosphate, and the reaction produces SO4 2+ With Fe3H6(P04)4 3+ The formation of flocculent complexes will not affect the growth of iron phosphate crystals. As the amount of hydrogen peroxide continues to increase, the pH further decreases and Fe3H6(PO4)4 3+ The concentration of Fe3H6(PO4)4 increases, generating 3+ The reaction is inhibited or reversed, and hydrolysis is performed to generate iron phosphate. At this time, sulfate is released. At this time, because most of the iron phosphate has completed crystal growth, the effect of sulfate is small. The pH of the final reaction is controlled between 2.2-2.3.

[0027] When the reaction starts, the pH is too high, so the iron can generate Fe3H6(PO4)4 3+ When forming a complex with sulfate ions, it can also form an additional iron hydroxide colloid to form flocs with sulfate, so that the iron phosphate in the present invention does not wrap sulfate during crystal growth, and its purity is high. 3+ Normal reaction produces iron phosphate, Fe3H6(PO4)4 3+ Hydrolysis generates iron phosphate to form two forms of iron phosphate, Fe 3+ The normal reaction generates iron phosphate. As its crystals have time to grow, it precipitates as large amorphous iron phosphate. After aging, it becomes a large cube. Fe3H6(PO4)4 3+The iron phosphate generated by hydrolysis is in a fine amorphous state and is also in small particles after aging. Therefore, when the iron phosphate of the present application is compacted, the fine particles will be forced to fill the gaps in the block crystals, so its compaction density is higher than the compaction density of the sheet-like or block-like iron phosphate in the prior art.

[0028] After the addition of hydrogen peroxide is completed, the mixture is stirred and reacted for 2-3 hours to obtain a mixed solution of an iron phosphate product.

[0029] S3: Washing and filtration

[0030] After the mixed liquor of the ferric phosphate product is filtered, the filter cake is washed with desalted water in a weight ratio of 1:3 between material and water. The washing is repeated three times. The washing can effectively reduce the metal impurities and S content in the ferric phosphate filter cake. After washing, the ferric phosphate filter cake is obtained.

[0031] S4: Aging

[0032] The washed iron phosphate filter cake is added with desalted water in a weight ratio of 1:2 to water. After the reslurry is stirred evenly, the solution temperature is raised to 60°C for insulation. At the same time, ammonia water is added to the slurry to raise the pH value to between 2.2 and 2.3, and the slurry is aged for 1 hour.

[0033] The aging process is to quickly dissipate the water in the amorphous iron phosphate and form a stable crystal structure. Therefore, it is usually necessary to carry out the aging process at a high temperature of about 90°C to accelerate the redistribution of water inside the amorphous iron phosphate and form stable dihydrate iron phosphate crystals. The present application is first aged for 1 hour under a relatively low temperature (60±5°C) environment. The main reason is that when the temperature is low, the supersaturation of iron phosphate is large, the amorphous iron phosphate crystals are slow in the water dissipation process, and the small particles of amorphous crystals are easy to agglomerate between the large particles, so that the small particles and the large particles are evenly distributed; and during the aging process, the slurry pH will continue to decrease, H + As the concentration increases, the H + It can inhibit the formation of precipitation in the solution, and the iron phosphate particles cannot be fully aggregated, so ammonia water is added to neutralize H + , the inhibitory effect is reduced, and the iron phosphate crystals have more opportunities to grow and develop. Then, the temperature is raised to 95℃ and kept warm for 3 hours, and phosphoric acid is added. The amount added is based on the liquid level of the aging material, that is, 1% to 3% of the volume, to adjust the acid-base environment of the aging. After the temperature is raised, H + The inhibitory effect of PO4 3-The increase in promotes the transformation of amorphous precipitates with disordered arrangement into a stable binary phase. Iron phosphate reduces its inherent energy. High temperature can effectively increase the divergence rate of water in amorphous iron phosphate, thereby increasing the transformation of iron phosphate from the amorphous state of FePO4·xH2O to the binary crystal of FePO4·2H2O, thereby improving the crystallinity of iron phosphate.

[0034] S5: Filtration, washing, drying and calcination

[0035] After filtering the aged solution, add deionized water to wash it at a material ratio of 1:2. After filtering again, put the filter cake into an oven for drying at 160°C for 2 hours. Put the dried sample into a muffle furnace for calcination at 650°C for 2 hours to obtain the iron phosphate product. The SEM image of the final product iron phosphate is as follows: Figure 1 As shown, its crystals include large square particles and amorphous fine particles, and its compaction density is high.

[0036] The relevant performance data are as follows: The units of metal ions not specified are mg / kg

[0037]

[0038] From the above data, it can be seen that the compacted density of the iron phosphate product of the present application is 2.53 g / cm 3 , much higher than the 2.15g / cm 3 The sulfur content of the iron phosphate product is only 65 mg / kg, which is much lower than that of other iron phosphate products prepared from titanium dioxide slag, and other metal impurities are at a relatively low level.

[0039] Example 2

[0040] The difference between Example 2 and Example 1 is that in Example 2, S2: the iron-phosphorus ratio in the liquid oxidation and reaction is 1.08:1; the pH value of monoammonium phosphate is controlled at 6.5, and the pH of the final reaction is controlled between 2.4-2.7; and S4: the low-temperature aging temperature in the aging is 55°C, and ammonia water is added to the slurry at the same time to raise the pH value to between 2.0-2.2, and the aging is carried out for 1.5 hours, and the high-temperature aging temperature is 90°C, and the aging is carried out for 3.5 hours. The rest is exactly the same as Example 1.

[0041] The performance data related to Example 2 are as follows: The units of metal ions not specified are all mg / kg

[0042]

[0043] Example 3

[0044] The difference between Example 3 and Example 1 is that: in Example 3, S2: the iron-phosphorus ratio in the liquid oxidation and reaction is 1.12:1; the pH value of monoammonium phosphate is controlled at 7.5, and the pH of the final reaction is controlled between 2.7-3.0; and S4: the low-temperature aging temperature in the aging is 65°C, and ammonia water is added to the slurry at the same time to raise the pH value to between 1.8-2.0, and the aging is carried out for 2 hours of heat preservation, and the high-temperature aging temperature is 100°C for 3 hours. The rest is exactly the same as Example 1.

[0045] The experimental data of Example 3 are as follows: The units of metal ions not specified are all mg / kg

[0046]

[0047] Comparative Example 1

[0048] Comparative Example 1 The preparation of ferric phosphate comprises the following steps:

[0049] (1) Dissolving and refining ferrous sulfate: dissolving the solid ferrous sulfate byproduct produced by the sulfuric acid process in titanium dioxide in water, adding iron powder, and collecting the filtrate to obtain a refined ferrous sulfate solution;

[0050] (2) oxidation of ferrous sulfate, adding hydrogen peroxide to the refined ferrous sulfate solution for full reaction, the molar ratio of H2O2 in the added hydrogen peroxide to the iron element in the refined ferrous sulfate solution is 0.7:1, the reaction temperature is 45°C, and the reaction time is 30 minutes to obtain an oxidation solution;

[0051] (3) Preparation of ferric phosphate: adding a monoammonium phosphate solution with a mass percentage concentration of 25% to the oxidizing solution, wherein the molar ratio of NH4H2PO4 in the added monoammonium phosphate solution to the iron element in the oxidizing solution is 1:1, adding the monoammonium phosphate solution at a uniform speed, and simultaneously steam heating for reaction, the heating temperature is 80-90°C, the addition time of the monoammonium phosphate solution is 90 minutes, and the total reaction time is 2.5 hours, to obtain ferric phosphate slurry;

[0052] (4) primary filtration and slurrying, filtering the iron phosphate slurry, collecting the solid part and washing it, the washing end point is that the conductivity of the effluent water is ≤4000 μs / cm, and obtaining a primary filter cake; adding pure water to the washed primary filter cake and stirring it, and transferring it to a conversion kettle for aging to obtain an aged iron phosphate slurry;

[0053] (5) multi-stage filtration, performing secondary filtration on the aged iron phosphate slurry, collecting the solid part and washing it, the washing end point is that the effluent conductivity is ≤1500 μs / cm, and obtaining a secondary filter cake; adding pure water to the washed secondary filter cake and stirring, and then performing tertiary filtration, collecting the solid part, and obtaining a tertiary filter cake;

[0054] (6) Drying-calcination-crushing: drying the three-stage filter cake to obtain ferric phosphate containing crystal water, calcining the ferric phosphate containing crystal water in a rotary kiln at a calcination temperature of 600°C for 2.5 hours, and crushing the ferric phosphate in a crushing device. The exhaust gas after crushing passes through a pulse dust collector and is discharged into the air in compliance with the standards. The crushed materials are mixed evenly to obtain high-density ferric phosphate.

[0055] The compacted density of the iron phosphate prepared in Comparative Example 1 is 0.93 g / cm 3.

[0056] By comparing with the comparative example, the compaction density of the iron phosphate product of the present application is much higher than that of the prior art.

[0057] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for producing high compaction density iron phosphate, Features: The following steps are involved: S1: Prepare ferrous sulfate solution: Mix titanium dioxide slag with desalted water, add phosphoric acid, ammonia water and flocculant to pretreat the solution, filter to remove suspended insoluble matter after complete dissolution, and obtain FeSO4·7H2O solution after suction filtration; S2: Liquid preparation for oxidation and reaction: Calculate the required amount of phosphoric acid while ensuring that the iron excess is 8%-12%, prepare phosphoric acid and ammonia water into a monoammonium phosphate solution, and control the pH value of the monoammonium phosphate solution to 6.5-7.5, mix the monoammonium phosphate solution with the FeSO4·7H2O solution prepared in S1, and slowly add hydrogen peroxide to the mixed solution for oxidation reaction, and the pH value of the final reaction is controlled between 2-3; S3: washing and filtration: add desalted water to the filter cake after suction filtration of the mixed solution at a ratio of 1:3 between material and water, and repeat the washing and filtration three times to obtain iron phosphate.

2. The method for preparing high compacted density ferric phosphate according to claim 1, Features: The following steps are also included: S4: staged aging: add desalted water to the filter cake after filtration in S3 at a ratio of 1:2, stir evenly, raise the solution temperature to 55-65°C, add ammonia water to the solution, control the pH value of the reaction solution between 1.8-2.4, keep warm for 1-2 hours for the first stage of aging, raise the temperature to 90-100°C, add phosphoric acid, keep warm for 3-4 hours for the second stage of aging, and precipitate FePO4·2H2O; S5: Filtration, washing, drying and calcination: Filter the aged solution and add desalted water at a material-water ratio of 1:2 for washing. After washing, filter and dry the solution. Calcine the dried sample to obtain the iron phosphate product.

3. The method for preparing high compacted density ferric phosphate according to claim 2, Features: The iron-phosphorus ratio in the S2 is 1.1:

1.

4. The method for preparing high compacted density ferric phosphate according to claim 3, Features: The pH value of the monoammonium phosphate in S2 is controlled to be 7, and the pH of the final reaction is controlled between 2.2-2.

3.

5. The method for preparing high compacted density ferric phosphate according to claim 4, Features: In the first stage of S4, the aging temperature is controlled at 60° C., the pH value is controlled at 2.2-2.3, and the insulation time is controlled at 1 hour.

6. The method for preparing high compacted density ferric phosphate according to claim 5, Features: The second stage aging temperature in S4 is controlled to be 95° C., and the insulation time is controlled to be 3 hours.

Citation Information

Patent Citations

  • Synthesizing method for low-cost battery-grade iron phosphate

    CN106044735A

  • Method for preparing iron phosphate by using titanium dioxide byproduct ferrous sulfate

    CN113184820A

  • Efficient preparation method of battery-grade iron phosphate

    CN114988383A

  • Preparation method of iron phosphate

    CN115403019A

  • Continuous preparation method of high-quality iron phosphate

    CN117623257A

Cited By

  • Lithium iron phosphate dihydrate and preparation method and application thereof

    CN120736493A