Impurity removal agent for polycrystalline silicon high-boiling residues and preparation method and impurity removal method of impurity removal agent

By hydrolysis and decomposition of polycrystalline silicon production waste gas and waste liquid, recovered salts were prepared as impurities removal agents and used for distillation of high boiling substances, which solved the problem of poor removal of aluminum and titanium impurities in the prior art. It achieves efficient and economical impurity removal effects, and ensures environmental protection and recycling of impurity removal agents.

CN119080007APending Publication Date: 2024-12-06XINJIANG DAQO NEW ENERGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411196780.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing impurity removal process of high boiling polysilicon cannot effectively remove aluminum and titanium impurities, and there are problems such as unsatisfactory removal effect, high cost, unrecoverable impurities removal agents, and easy introduction of new impurities.

Method used

The waste gas and waste liquid generated in polycrystalline silicon production are hydrolyzed, the pH is adjusted to neutral, and the silicon removal and impurity removal are carried out. The recovered salt is obtained by distillation as a decompression agent, which is used to mix with high boiling substances for distillation treatment to remove aluminum. and titanium impurities.

Benefits of technology

It realizes efficient removal of aluminum and titanium impurities in high boiling substances, reduces production costs, avoids the introduction of new impurities, and the impurity remover can be recycled and reused.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080007A_ABST
    Figure CN119080007A_ABST
Patent Text Reader

Abstract

The invention relates to an impurity removal agent for a polycrystalline silicon high-boiling residue, and a preparation method and an impurity removal method of the impurity removal agent. The preparation method of the impurity removal agent for the polycrystalline silicon high-boiling residues comprises the following steps: (1) hydrolyzing waste gas containing chlorosilane, and adjusting the pH value of a hydrolysis solution to be neutral, so as to obtain neutral wastewater; and (2) carrying out filter pressing on the neutral wastewater, and sequentially carrying out silicon removal, impurity removal treatment, evaporative crystallization and drying to obtain recovered salt, namely the impurity removal agent. According to the impurity removal agent for the polycrystalline silicon high-boiling residues as well as the preparation method and the impurity removal method of the impurity removal agent, the recycled salt obtained by treating waste gas in polycrystalline silicon is used for removing impurities of the polycrystalline silicon high-boiling residues, aluminum and titanium impurities can be removed at the same time, and the impurity removal agent has the advantages of being high in impurity removal effect, low in cost and capable of being repeatedly used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of removing impurities from high boiling points of polysilicon, and in particular relates to an impurity remover for high boiling points of polysilicon, a preparation method thereof, and an impurity removal method. Background Art

[0002] Polysilicon is the basic raw material of the photovoltaic industry, and some by-products are produced during its preparation process. Some of the by-products are high-boiling compounds (commonly known as "high-boiling substances") with a boiling point exceeding 70°C, and their mass accounts for 7.0-8.0% of the crude monomer product. These high-boiling substances are very complex, mainly including hexachloroethoxysilane, pentachloroethoxysilane and other oxygen silanes and hexachlorodisilane, pentachlorodisilane and other polychlorosilanes, and the boiling points of each component are relatively close. It is difficult to separate the components by the commonly used separation method, so they cannot be effectively utilized. In the actual production process, the main treatment method for high-boiling substances is to concentrate and separate them, recover a part of the low-boiling substances such as silicon tetrachloride remaining in the high-boiling substances, and then hydrolyze the remaining high-boiling substances together with solid impurities brought out during the processing of other polysilicon such as metal chlorides. Although this treatment method is simple and effective, it consumes a large amount of Si and Cl elements that should be valuable, which is not conducive to the sustainable development of polysilicon production. In addition, if these high-boiling substances are not properly handled, it will also increase the production cost of the enterprise and cause safety and environmental protection problems.

[0003] In order to solve the above problems, people have developed a method of using organic amines as catalysts to catalyze the cracking of polychlorosilane into monosilicon compounds. That is, tri-n-octylamine, N, N-diethylbutylamine, etc. are used as catalysts to crack high-boiling products and convert them into chlorosilanes for recycling. However, high-boiling products contain some metal impurities, among which aluminum trichloride and titanium tetrachloride impurities are the most representative, and the mass content of these two metal elements can reach hundreds to thousands of ppm. The metal impurities in the high-boiling products will react with the organic amines in the catalyst, causing a large loss of the cracking catalyst during the catalytic cracking process. In order to ensure the catalytic effect, it is necessary to continuously replenish the lost catalyst during the cracking process, which not only increases the operating cost, but also seriously affects the stability of the production process. In addition, these metal impurities will also enter the subsequent distillation system with the cracked monosilicon compounds, increasing the pressure of distillation and impurity removal. Under normal pressure conditions, the boiling point of titanium tetrachloride is 135-136°C, and the boiling point of aluminum trichloride is 182.7°C, but sublimation will occur at 177.8°C. These temperatures are very close to the distillation range of high boiling products (120-180°C), so it is difficult to separate the two metal chlorides from other components in the high boiling products by conventional distillation treatment and the like.

[0004] The current process for removing impurities from high-boiling products of polysilicon is to add an impurity remover to the high-boiling products to form a mixed system of non-volatile compounds with metal impurities, and then separate the remaining components in the high-boiling products from the mixed system by distillation to remove aluminum chloride impurities. Alternatively, aluminum chloride is allowed to exist in a stable solid form by cooling and settling crystallization, and then the purpose of aluminum removal is achieved by filtering. However, these methods have the problems of complex impurity removers, inability to remove impurities such as aluminum and titanium at the same time, unsatisfactory impurity removal effects, complex impurity removal processes, high impurity removal costs, impurity removers that cannot be recycled, and easy introduction of new impurities.

[0005] In view of this, the present invention proposes a new impurity remover for high-boiling points of polysilicon and a preparation method and an impurity removal method thereof, which uses recycled salt obtained by treating waste gas in polysilicon to remove impurities from high-boiling points of polysilicon, and can remove aluminum and titanium impurities at the same time, having the advantages of high impurity removal effect, low cost and reusability. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a doping agent for high-boiling substances of polysilicon, and the preparation method is simple.

[0007] In order to achieve the above purpose, the technical solution adopted is:

[0008] A method for preparing an impurity remover for high boiling points of polysilicon, characterized by comprising the following steps:

[0009] (1) After the waste gas and waste liquid containing chlorosilane are hydrolyzed, the pH of the hydrolysis solution is adjusted to neutral to obtain neutral wastewater;

[0010] (2) After filtering the neutral wastewater, the wastewater is subjected to desiliconization and de-impurity treatments in sequence, evaporated and crystallized, and then dried to obtain recovered salt, i.e., the de-impurity agent.

[0011] Furthermore, in the step (1), sodium hydroxide solution is used to adjust the hydrolysis solution to neutrality.

[0012] Furthermore, in the step (2), the silicon removal treatment comprises: adding calcium hydroxide;

[0013] Furthermore, in step (2), the impurity removal treatment is: adding carbonate ions to remove Mg 2+ , Ca 2+ , Ba 2+ , Sr 2+ .

[0014] Another object of the present invention is to provide a polysilicon high boiling point remover, which is prepared by the above-mentioned preparation method. The remover uses solid waste generated in the production of polysilicon as a treatment agent and has low cost.

[0015] Another object of the present invention is to provide a method for removing impurities from high-boiling products in polysilicon. This method can remove aluminum and titanium impurities at the same time and has the advantages of significant impurity removal effect, low cost, and no introduction of new impurities.

[0016] In order to achieve the above purpose, the technical solution adopted is:

[0017] A method for removing impurities from high-boiling polysilicon products, characterized in that the method comprises: mixing an impurity remover with the high-boiling polysilicon products, and then performing a distillation treatment to obtain the high-boiling polysilicon products after impurities are removed;

[0018] The impurity remover is the impurity remover mentioned above.

[0019] Furthermore, the mass ratio of the impurity remover to the high boiling point of polysilicon is 0.8-1.8:100.

[0020] Furthermore, the mass ratio of the impurity remover to the high boiling point of polysilicon is 0.8-1.05:100.

[0021] Furthermore, the temperature of the distillation treatment is greater than 150°C.

[0022] Furthermore, the pressure of the distillation treatment is 20-100 kPa.

[0023] Furthermore, after the distillation treatment, the solution that is not distilled out is subjected to hydrolysis, neutralization, filter pressing, silicon removal, impurity removal, evaporation crystallization, and drying treatment, and the obtained solid matter can be used as an impurity remover to remove impurities from high-boiling products of polysilicon again.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. In the technical solution of the present invention, solid waste (recovered salt) generated in the production of polysilicon is used as an impurity remover without any additional cost, and waste is turned into treasure, creating benefits, being economical and environmentally friendly.

[0026] 2. In the technical solution of the present invention, the recycled salt is used as the impurity remover, which can not only efficiently remove aluminum in high boiling water, but also has a certain titanium removal effect.

[0027] 3. In the technical solution of the present invention, the solid waste generated in the production of polysilicon is mainly composed of various inorganic salts and trace organic matter in the original system, and no new impurities will be introduced into the system. Moreover, these trace organic matter will be recycled in the system along with the solid waste as an impurity remover, and will not cause subsequent environmental problems. At the same time, the impurity removal cost is low.

[0028] 4. In the technical solution of the present invention, after the impurity remover is complexed with impurities such as aluminum and titanium, it can be recycled and re-formed into solid waste and then reused as an impurity remover after post-treatment such as hydrolysis, thereby further reducing the cost of impurity removal. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the process of Example 1. DETAILED DESCRIPTION

[0030] In order to further explain the impurity remover for high boiling point of polysilicon and its preparation method and impurity removal method of the present invention, and to achieve the expected purpose of the invention, the following is a detailed description of the impurity remover for high boiling point of polysilicon and its preparation method and impurity removal method according to the present invention, its specific implementation method, structure, characteristics and efficacy, in combination with the preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics of one or more embodiments may be combined in any suitable form.

[0031] Before describing in detail the impurity remover for high boiling point polysilicon and its preparation method and impurity removal method of the present invention, it is necessary to further explain the relevant background mentioned in the present invention to achieve better results.

[0032] The current existing technology can provide some methods to separate metal impurities and avoid the loss of catalysts caused by metal impurities. For example:

[0033] Patent CN108658082A discloses a method for removing aluminum chloride by pre-treating high-boiling materials. The method includes sending the high-boiling materials to a cooling stirring tank, stirring them at low temperature for 1-5 hours, sending them to a settling tank, and then allowing the high-boiling materials to settle in a nitrogen environment for 1-20 hours, thereby separating a slurry including solid impurities and metal halides. However, the method has a long processing flow and the effect of removing aluminum chloride is not ideal.

[0034] Patent CN113149017A discloses a complexing agent for removing aluminum from high-boiling products of polysilicon and its application. The complexing agent has a complex structure and is difficult to be applied on a large scale in actual production.

[0035] Patent CN105271246A discloses a method for removing aluminum chloride from high boiling materials. The method first adds an auxiliary agent and aluminum-containing impurities to the high boiling materials to form a mixed system containing non-volatile aluminum compounds, and then separates the remaining components in the high boiling materials from the mixed system by distillation, thereby removing the aluminum chloride impurity. However, the auxiliary agent used in the method is obtained by mixing "deferoxamine", "deferiprone" and "testirani" in a certain proportion. The iron removal effect is relatively high, but the aluminum removal effect is not ideal, and the cost is also relatively high.

[0036] Patent CN116216724A discloses a compound of alkali metal chloride and aminocarboxylate as a reagent for removing aluminum and titanium impurities from high-boiling products of polysilicon. The impurity remover can increase the boiling point or sublimation temperature of metal impurities in high-boiling products of polysilicon, and is helpful for separating high-boiling products of polysilicon from metal impurities in distillation treatment, thereby reducing the loss of metal impurities to organic amine catalysts in catalytic cracking operations. However, the impurity remover cannot be recovered.

[0037] Patent CN117342563A discloses a method for removing aluminum from high-boiling products of polysilicon, wherein cations in pyrrolidine ionic liquids or piperidine ionic liquids combine with aluminum chloride in high-boiling products of polysilicon to form chloroaluminate ionic liquids, and the generated chloroaluminate ionic liquids can further be used as catalysts for catalytic cracking reactions of high-boiling products of polysilicon. However, the impurity remover cannot be recovered and has high cost.

[0038] CN104402004A discloses a method for treating chlorosilane slurry by extraction, wherein a certain alkane is used as an extractant and mixed with high-boiling products of polysilicon, and then dried in a dryer, evaporated in an evaporator, and then distilled in a distillation tower to separate aluminum chloride.

[0039] CN115893424A discloses a treatment agent for removing aluminum from high-boiling products of polysilicon and its application. The treatment agent is a compound of alkali metal chlorides, alkaline earth metal chlorides, transition metal chlorides and alkaline earth metal sulfates. The metal salts in the treatment agent are mixed with high-boiling products of polysilicon to form a multi-component molten salt system, which is separated by distillation.

[0040] Therefore, the existing impurity removal technology has the following problems:

[0041] (1) Aluminum treatment agents in the prior art include organic and inorganic types. Organic ones, such as pyrrolidine ionic liquids or piperidine ionic liquids or C12-C16 alkanes, are costly and require additional steps and costs for the recovery of the treatment agent. If the recovery is incomplete, organic matter will be introduced into the water body during the subsequent hydrolysis treatment and will not be easily removed, thus failing to meet the environmental protection requirements for external drainage. Inorganic ones are a compound of four salts: alkali metal chlorides, alkaline earth metal chlorides, transition metal chlorides and alkaline earth metal sulfates, and have a complex composition.

[0042] (2) The existing high-boiling aluminum treatment agent has a single function, which is only effective in removing aluminum but not titanium.

[0043] (3) The existing complex impurity removers cannot be recycled and reused.

[0044] After understanding the relevant background mentioned in the present invention, the following will further introduce in detail a polysilicon high boiling point remover and its preparation method and impurity removal method of the present invention in combination with specific embodiments:

[0045] The technical solution of the present invention is:

[0046] A method for preparing a polysilicon high boiling point remover comprises the following steps:

[0047] (1) After the waste gas and waste liquid containing chlorosilane are hydrolyzed (reacted with water), the pH of the hydrolysis solution is adjusted to neutral to obtain neutral wastewater;

[0048] (2) After filtering the neutral wastewater, the wastewater is subjected to desiliconization and de-impurity treatments in sequence, and then evaporated, crystallized and dried to obtain recovered salt, i.e., the de-impurity agent.

[0049] Preferably, in the step (1), sodium hydroxide solution is used to adjust the hydrolysis solution to neutrality.

[0050] Preferably, in the step (2), the silicon removal treatment comprises: adding calcium hydroxide;

[0051] Preferably, in step (2), the impurity removal treatment is: adding carbonate ions to remove Mg 2+ , Ca 2+ , Ba 2+ , Sr 2+ .

[0052] A method for removing impurities from high-boiling polysilicon products, comprising: mixing an impurity remover with the high-boiling polysilicon products, and performing distillation treatment to obtain the high-boiling polysilicon products after impurities are removed;

[0053] The impurity remover is the impurity remover mentioned above.

[0054] In the above technical solution, the recovered salt can complex the metal impurities such as aluminum, titanium, iron, calcium, magnesium, copper, nickel, zinc, etc. in the high boiling point, and transform them into substances with higher boiling points, which remain at the bottom of the purification kettle.

[0055] Preferably, the mass ratio of the impurity remover to the high boiling point of polysilicon is 0.8-1.8:100.

[0056] Further preferably, the mass ratio of the impurity remover to the high boiling point of polysilicon is 0.8-1.05: 100. Preferably, the temperature of the distillation treatment is greater than 150°C.

[0057] Preferably, the pressure of the distillation treatment is 20-100 kPa.

[0058] Preferably, after the distillation treatment, the solution that is not distilled out is subjected to hydrolysis, neutralization, filter pressing, silicon removal, impurity removal, evaporation crystallization, and drying treatment, and the obtained solid matter, i.e., the recovered salt, can be used as an impurity remover to remove impurities from high-boiling products of polysilicon again.

[0059] In the above technical scheme, the neutralization, filter pressing, silicon removal, impurity removal, and evaporation crystallization treatments are the same as the preparation method of the impurity remover.

[0060] Example 1.

[0061] The specific steps are as follows:

[0062] A Preparation and Recovery of Salt

[0063] (1) The production of polysilicon will produce some waste gas and waste liquid containing chlorosilane. The waste liquid will also contain some ester and aniline organic matter, which cannot be discharged and needs to be hydrolyzed. Chlorosilane and water react to produce HCl, which needs to be neutralized by adding NaOH solution to form neutral wastewater.

[0064] (2) Neutral wastewater contains silicon dioxide, silicon powder, etc., which enter the filter press system and form a filter cake. After removing silicon dioxide and silicon powder, the neutral wastewater is desiliconized and Mg is removed. 2+ , Ca 2+ , Ba 2+ , Sr 2+ After the impurities are removed, the recovered salt is produced through evaporation and crystallization. At this time, the moisture content of the recovered salt is about 10%, and it needs to be dried by a single cone dryer to a dew point of ≤-50℃ before use.

[0065] Among them, silicon removal treatment: add calcium hydroxide to the neutral wastewater after removing silicon dioxide and silicon powder, stir, and make Ca 2+ It forms calcium silicate precipitate with silicate ions, settles naturally in the inclined plate settler, and is initially filtered by the quartz sand filter to remove large solid impurities. Then, PAC coagulant is added, and the first-level self-cleaning filter further removes CaSiO3 precipitate, and then the first-level ultrafiltration membrane intercepts solid particles ≥ 0.02um.

[0066] Mg Removal 2+ , Ca 2+ , Ba 2+ , Sr 2+ Impurities: Add sodium carbonate, carbonate ions and Mg 2+ , Ca 2+ , Ba 2+ , Sr 2+ Impurities form precipitation, thus removing Mg 2+ , Ca 2+ , Ba 2+ , Sr 2+ Impurities.

[0067] The main component of the recovered salt after the above treatment is the inorganic salt sodium chloride, and it also contains trace amounts of sodium silicate and trace amounts of other inorganic chloride salts. There is also a small amount of calcium silicate residue produced in the silicon removal step. Calcium silicate can appropriately prevent the sodium chloride from caking in the impurity remover, so trace amounts of calcium silicate can act as an anti-caking agent. It also contains trace amounts of aniline organic matter and trace amounts of organic sodium salts generated by ester hydrolysis in an alkaline environment. The combination of organic and inorganic substances not only makes it possible to efficiently remove aluminum in high boiling points, but also has a certain titanium removal effect.

[0068] B Polysilicon high boiling point impurity removal: combined Figure 1

[0069] The recovered salt and high boiling products are mixed in a certain proportion in a purification kettle and heated for distillation. The distillation temperature is greater than 150°C and the pressure is 20-100kPa. The purification kettle is turned on for stirring to fully mix the recovered salt and the high boiling products of polysilicon. The vaporized substances in the reactor are condensed through a condenser and collected in a container connected to the condenser.

[0070] Preferably, the mass ratio of the impurity remover, i.e., the recovered salt, to the high boiling products of polysilicon is 0.8-1.8:100.

[0071] The condensed liquid is a high-boiling product from which metal impurities such as aluminum have been removed, and can enter the subsequent titanium removal system and cracking conversion system.

[0072] The recovered salt can complex the metal impurities such as aluminum, titanium, iron, calcium, magnesium, copper, nickel, zinc, etc. in the high-boiling products and transform them into substances with higher boiling points, which will remain at the bottom of the purification kettle and can be hydrolyzed together with the unvaporized high-boiling products. The hydrolyzed product will enter the filter press system after the pH is adjusted to the required standard. The neutral wastewater after the filter press will be desiliconized and de-Mgated. 2+ , Ca 2+ , Ba 2+ , Sr 2+ After a series of treatments such as evaporation, crystallization, and drying (this series of treatments is the same as the method in step A), the recovered salt can be obtained again for recycling.

[0073] The aluminum removal rate and titanium removal rate in the embodiment are defined as follows:

[0074] Aluminum removal rate = (1-Al content of the condensed and collected evaporation / Al content in the polysilicon high boiling product to be treated) × 100%.

[0075] Titanium removal rate = (1-Ti content of the condensed and collected evaporation / Ti content in the polysilicon high boiling product to be treated) × 100%.

[0076] Example 2.

[0077] The operation steps of Example 2 are the same as those of Example 1, except that:

[0078] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 0.8% of its mass of the recovered salt (the recovered salt prepared in step A of Example 1) were added into the reactor, stirred and distilled at 155°C and 100 kPa.

[0079] The gas phase condensate was sampled and the Al content was measured to be 56.977 ppm and the Ti content was 130.002 ppm. Through calculation, it can be known that the aluminum removal rate of this embodiment is 88.14% and the titanium removal rate is 67.74%.

[0080] Example 3.

[0081] The operation steps of Example 3 are the same as those of Example 2, except that:

[0082] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 0.9% of the recovered salt by mass were added into the reactor, and stirred and distilled at 155° C. and 100 kPa.

[0083] The gas phase condensate was sampled and measured to have an Al content of 32.563 ppm and a Ti content of 91.462 ppm. Calculation showed that the aluminum removal rate in this embodiment was 93.22% and the titanium removal rate was 77.31%.

[0084] Example 4.

[0085] The operation steps of Example 4 are the same as those of Example 2, except that:

[0086] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 1.0% of the recovered salt by mass were added into the reactor, and stirred and distilled at 155° C. and 100 kPa.

[0087] The gas phase condensate was sampled and measured to have an Al content of 11.045 ppm and a Ti content of 62.323 ppm. Calculation showed that the aluminum removal rate in this embodiment was 97.70% and the titanium removal rate was 84.54%.

[0088] Example 5

[0089] The operation steps of Example 5 are the same as those of Example 1, except that:

[0090] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 1.05% of the recovered salt by mass were added into the reactor, and stirred and distilled at 155° C. and 100 kPa.

[0091] The gas phase condensate was sampled and measured to have an Al content of 0 ppm and a Ti content of 60.002 ppm. Calculation showed that the aluminum removal rate in this embodiment was 100% and the titanium removal rate was 85.11%.

[0092] Example 6.

[0093] The operation steps of Example 6 are the same as those of Example 2, except that:

[0094] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 1.05% by mass of the recovered salt were added into the reactor, stirred and distilled at 158° C. and 100 kPa.

[0095] The gas phase condensate was sampled and measured to have an Al content of 0 ppm and a Ti content of 61.032 ppm. Calculation showed that the aluminum removal rate in this embodiment was 100% and the titanium removal rate was 84.86%.

[0096] Example 7.

[0097] In the stirring distillation process, the recovered salt complexes the metal impurities such as aluminum, titanium, iron, calcium, magnesium, copper, nickel, zinc, etc. in the high-boiling products in the purification kettle, and transforms them into substances with higher boiling points, which remain at the bottom of the purification kettle and are hydrolyzed together with the unvaporized high-boiling products. The hydrolyzed products are then adjusted to pH and enter the filter press system. The neutral wastewater after the filter press is desiliconized and de-Mgated. 2+ , Ca 2+ , Ba 2+ , Sr 2+ After a series of treatments such as evaporation, crystallization, and drying (this series of treatments is the same as the method in step A), recovered salt is obtained again, and this secondary recovered salt is used again for removing impurities from high boiling points.

[0098] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 1.05% by mass of the secondary recovered salt were added to the reactor, stirred and distilled at 155° C. and 100 kPa.

[0099] The gas phase condensate was sampled and measured to have an Al content of 0 ppm and a Ti content of 63.942 ppm. Calculation showed that the aluminum removal rate in this embodiment was 100% and the titanium removal rate was 84.13%.

[0100] Example 8.

[0101] The operation steps of Example 8 are the same as those of Example 2, except that:

[0102] The high boiling point to be treated (Al content of 344.119 ppm, Ti content of 528.414 ppm) and 1.05% by mass of the recovered salt were added to the reactor, stirred and distilled at 155° C. and 100 kPa.

[0103] The gas phase condensate was sampled and measured to have an Al content of 0 ppm and a Ti content of 52.3287 ppm. Calculation showed that the aluminum removal rate in this embodiment was 100% and the titanium removal rate was 90.10%.

[0104] Example 9.

[0105] The operation steps of Example 9 are the same as those of Example 2, except that:

[0106] (1) The high boiling point to be treated (Al content of 228.825 ppm, Ti content of 1193.067 ppm) and 1.05% of the recovered salt by mass were added to a reactor, stirred and distilled at 155° C. and 100 kPa.

[0107] The gas phase condensate was sampled and measured to have an Al content of 2.212 ppm and a Ti content of 483.355 ppm. Calculation showed that the aluminum removal rate in this embodiment was 99.03% and the titanium removal rate was 59.49%.

[0108] The high boiling point to be treated has a high Ti content, resulting in the amount of impurity remover being unable to meet the titanium removal effect.

[0109] (2) The high-boiling (Al content of 228.825 ppm, Ti content of 1193.067 ppm) recovered salt to be treated was added to the reactor, stirred and distilled at 155° C. and 100 kPa.

[0110] The mass ratios of recovered salt to high boiling products are 1.3:100, 1.5:100 and 1.8:100 respectively.

[0111] The gas phase condensate was sampled to determine the impurity removal effect. The aluminum removal rate and titanium removal rate increased with the increase of the amount of recovered salt used. When the mass ratio of recovered salt to high boiling point was 1.5:100, the aluminum removal rate was 100%. When the mass ratio of recovered salt to high boiling point was 1.8:100, the titanium removal rate was 88.25%.

[0112] Example 10.

[0113] The operation steps of Example 10 are the same as those of Example 2, except that:

[0114] The high boiling point to be treated (Al content of 344.119 ppm, Ti content of 528.414 ppm) and 1.05% of the recovered salt by mass were added into the reactor, and stirred and distilled at 155° C. and 20 kPa.

[0115] The gas phase condensate was sampled and measured to have an Al content of 0 ppm and a Ti content of 48.254 ppm. Calculation showed that the aluminum removal rate in this embodiment was 100% and the titanium removal rate was 90.87%.

[0116] Example 11.

[0117] The operation steps of Example 11 are the same as those of Example 2, except that:

[0118] The high boiling point to be treated (Al content of 344.119 ppm, Ti content of 528.414 ppm) and 1.05% of the recovered salt by mass were added into the reactor, and stirred and distilled at 155° C. and 80 kPa.

[0119] The gas phase condensate was sampled and measured to have an Al content of 0 ppm and a Ti content of 50.148 ppm. Calculation showed that the aluminum removal rate in this embodiment was 100% and the titanium removal rate was 90.51%.

[0120] Comparative Example 1.

[0121] The high boiling point to be treated (Al content of 480.576 ppm, Ti content of 403.018 ppm) and 1.05% of the recovered salt by mass were added into the reactor, and stirred and distilled at 145° C. and 100 kPa.

[0122] The gas phase condensate was sampled and measured to have an Al content of 59.937 ppm and a Ti content of 226.584 ppm. Calculation showed that the aluminum removal rate in this embodiment was 87.53% and the titanium removal rate was 43.78%.

[0123] By comparing Comparative Example 1 with Example 2, it can be seen that the effect of distillation temperature on the impurity removal effect is very obvious.

[0124] Comparative Example 2.

[0125] According to patent CN115893424A, 960 parts of NaCl, 2 parts of KCl, 3 parts of CaCl2, 1 part of FeCl3 and 2 parts of CaSO4 were added to a ball mill and ball-milled for 3 hours, then put into a vibrating screen, and sieved through a 120-mesh stainless steel screen to prepare a treatment agent for removing aluminum from high-boiling polysilicon in this comparative example.

[0126] 50g of the high boiling point product to be treated (Al content is 480.576ppm, Ti content is 403.018ppm) and 1g of the polysilicon high boiling point product aluminum removal treatment agent of this comparative example were added into the reactor, stirred and distilled at 155°C, and the operating pressure was controlled at 0.2MPa.

[0127] The gas phase condensate was sampled and measured to have an Al content of 7.655 ppm and a Ti content of 392.569 ppm. Calculation showed that the aluminum removal rate of this comparative example was 98.41% and the titanium removal rate was 2.59%.

[0128] Comparing Comparative Example 2 with Examples 2-9, it can be seen that Comparative Example 2 does not have a titanium removal effect (the titanium removal rate of 2.59% here is more of the titanium removal effect of the distillation process itself), and the amount of impurity remover used is large. Therefore, compared with Comparative Example 2, the technical solution of the present invention can not only efficiently remove aluminum in high boiling water, but also has a certain titanium removal effect.

[0129] Comparative Example 3.

[0130] The operation steps of Comparative Example 3 are the same as those of Example 2, except that the impurity remover is sodium chloride.

[0131] The gas phase condensate was sampled and the Al content was measured to be 91.437 ppm and the Ti content was 398.584 ppm. Through calculation, it can be known that the aluminum removal rate of this embodiment is 80.97% and the titanium removal rate is 1.10%.

[0132] It can be seen from Comparative Example 3 that the single chloride salt has a poor aluminum removal effect and has no titanium removal effect (the titanium removal rate of 1.10% here is the titanium removal effect of the distillation process itself).

[0133] The above is only a preferred embodiment of the embodiment of the present invention, and does not impose any form of limitation on the embodiment of the present invention. Any simple modification, equivalent changes and modifications made to the above embodiment based on the technical essence of the embodiment of the present invention are still within the scope of the technical solution of the embodiment of the present invention.

Claims

1. A method for preparing a polysilicon high boiling point remover, characterized in that: The following steps are involved: (1) After the waste gas and waste liquid containing chlorosilane are hydrolyzed, the pH of the hydrolysis solution is adjusted to neutral to obtain neutral wastewater; (2) After filtering the neutral wastewater, the wastewater is subjected to desiliconization and de-impurity treatments in sequence, evaporated and crystallized, and then dried to obtain recovered salt, i.e., the de-impurity agent.

2. The preparation method according to claim 1, characterized in that: In the step (1), sodium hydroxide solution is used to adjust the hydrolysis solution to neutrality.

3. The preparation method according to claim 1, characterized in that: In the step (2), the silicon removal treatment is: adding calcium hydroxide.

4. The preparation method according to claim 1, characterized in that: In the step (2), the impurity removal treatment is: adding carbonate ions to remove Mg 2+ , Ca 2+ , Ba 2+ , Sr 2+ .

5. A polysilicon high boiling point remover, characterized in that: The preparation method is described in any one of claims 1 to 4.

6. A method for removing impurities from high boiling points of polysilicon, characterized in that: The impurity removal method comprises: mixing an impurity remover with polysilicon high boiling products, and then performing distillation treatment to obtain the polysilicon high boiling products after impurity removal; The impurity remover is the impurity remover according to claim 5.

7. The impurity removal method according to claim 6, characterized in that: The mass ratio of the impurity remover to the high boiling point of polysilicon is 0.8-1.8:

100.

8. The impurity removal method according to claim 7, characterized in that: The mass ratio of the impurity remover to the high boiling point of polysilicon is 0.8-1.05:

100.

9. The impurity removal method according to claim 6, characterized in that: The temperature of the distillation treatment is greater than 150°C; The pressure of the distillation treatment is 20-100 kPa.

10. The impurity removal method according to claim 6, characterized in that: After the distillation treatment, the solution that is not distilled out is subjected to hydrolysis, neutralization, filter pressing, silicon removal, impurity removal, evaporation crystallization, and drying treatment, and the obtained solid matter can be used as an impurity remover to remove impurities from polysilicon high boiling points again.

Citation Information

Patent Citations

  • Zero discharge processing method of polysilicon production wastewater

    CN110451709A

  • Three-waste cooperative treatment process system in granular silicon production process

    CN114956433A

  • Polycrystalline silicon industry wastewater treatment process

    CN115180764A