Nickel-copper-iron-manganese precursor and preparation method thereof, positive electrode material, positive electrode plate and sodium ion battery

Through the co-precipitation reaction of nickel copper iron-manganese precursor and solid-liquid separation method, a positive electrode material with a frame structure was prepared, which solved the problem of taking into account both material density and surface area in the prior art, and achieved high efficiency and stable electrochemistry performance.

CN119080082APending Publication Date: 2024-12-06JIANGXI JIANA ENERGY TECH CO LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226788.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing layered oxide positive electrode materials cannot take into account high tap density and large specific surface area during the preparation process, resulting in low Coulomb efficiency and poor circulation performance, and copper ion segregation affects electrochemical performance.

Method used

NixCu1-x-y-xFeyMnz(OH)2 was prepared by co-precipitation reaction and solid-liquid separation method. A stabilizer was added to optimize the distribution and particle size of copper ions to form secondary particles with frame structure and improve the material. uniformity and structural stability.

Benefits of technology

It achieves high first-time Coulomb efficiency and excellent cycling performance, combines high tap density and large specific surface area, reduces copper ion segregation and sulfur impurity content, and improves the mechanical strength and structural stability of the cathode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080082A_ABST
    Figure CN119080082A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of positive electrode materials, in particular to a nickel-copper-iron-manganese precursor, a preparation method of the nickel-copper-iron-manganese precursor, a positive electrode material, a positive plate and a sodium ion battery. The chemical formula of the nickel-copper-iron-manganese precursor is Ni < x > Cu < 1-x-y-x > Fe < y > Mn < z > (OH) < 2 >. The nickel-copper-iron-manganese precursor comprises secondary particles formed by stacking and arranging primary crystal grains in a radial shape; the primary crystal grains comprise sheet-shaped first crystal grains with frame structures and sheet-shaped second crystal grains which are radially filled among the first crystal grains; the tap density of the nickel-copper-iron-manganese precursor is greater than or equal to 1.4 g / cm < 3 >, and the specific surface area is gt; and 30m < 2 > / g. The nickel-copper-iron-manganese precursor has the advantages of high tap density and large specific surface area at the same time. The positive electrode material prepared from the nickel-copper-iron-manganese precursor has high initial coulombic efficiency and excellent cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a nickel-copper-iron-manganese precursor and a preparation method thereof, a positive electrode material, a positive electrode sheet and a sodium ion battery. Background Art

[0002] In recent years, with the rapid development of the electric vehicle industry, people's demand for lithium-ion batteries has been increasing day by day. However, due to the limited, uneven distribution and high price of lithium resources, it is unable to meet the growing demand for large-scale applications. In addition, the poor performance of lithium-ion batteries in low temperature environments also limits their scope of application. Sodium-ion batteries, which were born almost at the same time as lithium-ion batteries, have a similar working mechanism to the former. Compared with the scarce and expensive lithium element, sodium is very abundant on the earth, widely distributed, and cheaper. At the same time, its low-temperature performance is better than that of lithium-ion batteries, which makes sodium-ion secondary batteries regarded as an ideal supplement to lithium-ion batteries, and are expected to be used in energy storage equipment and two-wheeled vehicles.

[0003] There are three main types of positive electrode materials for sodium ion batteries: layered oxides, Prussian blue, and polyanions. Layered oxides are considered the focus of development due to their superior performance. However, the precursors used to prepare layered oxide positive electrode materials often cannot take into account both specific surface area and tap density, resulting in a low first coulombic efficiency of the positive electrode materials produced after the reaction and poor cycle performance.

[0004] In addition, the study found that Cu 2+ Layered oxide materials have redox properties, and the addition of copper ions can also enhance the air stability of positive electrode materials. However, during the synthesis of materials, copper ion segregation is often accompanied, which adversely affects the electrochemical properties of the materials, such as the first effect and cycle performance.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first purpose of the present invention is to provide a nickel-copper-iron-manganese precursor, which can simultaneously have the advantages of high tap density and large specific surface area. The positive electrode material prepared by using the nickel-copper-iron-manganese precursor has a high first coulombic efficiency.

[0007] The second object of the present invention is to provide a method for preparing a nickel-copper-iron-manganese precursor, which can solve the problem of copper ion segregation, optimize the particle size distribution, and improve the uniformity of the nickel-copper-iron-manganese precursor.

[0008] The third object of the present invention is to provide a positive electrode material having a single crystal morphology with a smooth surface, which is conducive to reducing stress, inhibiting cracks, and improving structural stability.

[0009] A fourth object of the present invention is to provide a positive electrode sheet having high initial efficiency and excellent cycle performance.

[0010] A fifth object of the present invention is to provide a sodium ion battery having high first coulombic efficiency and good cycle performance.

[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0012] The present invention first provides a nickel-copper-iron-manganese precursor, wherein the chemical formula of the nickel-copper-iron-manganese precursor is Ni x Cu 1-x-y-x Fe y Mn z (OH)2, where 0.1≤x≤0.6, 0.1≤y≤0.5, 0.1≤z≤0.5, 0.01≤1-xyx≤0.2.

[0013] The nickel-copper-iron-manganese precursor includes secondary particles formed by radially stacked primary grains; wherein the primary grains include first grains with a framework structure, and second grains radially filled between the first grains; the first grains and the second grains are both in the shape of sheets.

[0014] The tap density of the nickel-copper-iron-manganese precursor is ≥1.4 g / cm 3 .

[0015] The specific surface area of ​​the nickel-copper-iron-manganese precursor is>30m 2 / g.

[0016] Furthermore, in each of the secondary particles, the number of the first crystal grains is ≥6.

[0017] Furthermore, the thickness of the first crystal grain is 0.3-1.5 μm.

[0018] Furthermore, the thickness of the second crystal grain is ≤0.1 μm.

[0019] Furthermore, the secondary particles may be spherical and / or quasi-spherical in shape.

[0020] Furthermore, the particle size D of the nickel-copper-iron-manganese precursor is 50 3~15μm.

[0021] Furthermore, the sulfur content in the nickel-copper-iron-manganese precursor is less than 600 ppm.

[0022] The present invention further provides a method for preparing the nickel-copper-iron-manganese precursor, comprising the following steps: mixing a nickel-iron-manganese mixed salt solution, a complexing agent solution, a precipitant solution and a copper-ammonia solution and performing a coprecipitation reaction, followed by solid-liquid separation to obtain the nickel-copper-iron-manganese precursor.

[0023] Furthermore, the molar concentration of copper ions in the copper ammonia solution is 0.2-1.0 mol / L.

[0024] Furthermore, the pH of the copper ammonia solution is 9.5-13.0.

[0025] Furthermore, the copper ammonia solution also includes a stabilizer, the complexing ability of the stabilizer for copper ions and / or iron ions is greater than the complexing ability of the complexing agent solution for copper ions and / or iron ions, and the stabilizer includes at least one of acetylacetone, oxalic acid, citric acid, ethylenediaminetetraacetic acid, sulfosalicylic acid, tartaric acid and succinic acid; the molar concentration of the stabilizer in the copper ammonia solution is 0.01-0.1 mol / L.

[0026] Furthermore, the total molar concentration of metal elements in the nickel-iron-manganese mixed salt solution is 1.5 to 3.0 mol / L.

[0027] Furthermore, the nickel-iron-manganese mixed salt solution also includes an antioxidant, the antioxidant includes vitamin C, and the molar concentration of the antioxidant in the nickel-iron-manganese mixed salt solution is 0.01-0.1 mol / L.

[0028] Furthermore, the molar concentration of the complexing agent in the complexing agent solution is 0.5-2.0 mol / L.

[0029] Furthermore, the complexing agent solution includes at least one of an aqueous ammonia solution, an oxalic acid solution, a citric acid solution, an ethylenediaminetetraacetic acid solution and a tartaric acid solution.

[0030] Furthermore, the molar concentration of the precipitant in the precipitant solution is 9.8 to 11.8 mol / L.

[0031] Furthermore, the precipitant solution comprises a sodium hydroxide solution.

[0032] Furthermore, after the coprecipitation reaction is completed and before the solid-liquid separation, an aging step is also included.

[0033] Furthermore, after the solid-liquid separation, the method further includes the steps of washing, drying and screening.

[0034] Further, the mixing and the coprecipitation reaction are carried out under an inert atmosphere.

[0035] Furthermore, the coprecipitation reaction specifically includes: first controlling the pH of the reaction system to 11.0-13.0 and the ammonium ion concentration to 2-5 g / L, and performing a first coprecipitation reaction, the time of the first coprecipitation reaction is 10-90 min; then increasing the feed flow rate of the nickel-iron-manganese mixed salt solution to 1.2-3.0 times the feed flow rate of the nickel-iron-manganese mixed salt solution during the first coprecipitation reaction, increasing the feed flow rate of the copper-ammonia solution to 1.2-3.0 times the feed flow rate of the copper-ammonia solution during the first coprecipitation reaction, and increasing the feed flow rate of the complexing agent solution to 1.5-4.0 times the feed flow rate of the complexing agent solution during the first coprecipitation reaction, and adjusting the pH of the reaction system to 9.5-12.0, and performing a second coprecipitation reaction until the particles grow to the desired particle size.

[0036] The present invention further provides a positive electrode material, which is mainly formed by mixing the nickel-copper-iron-manganese precursor with a sodium source and then sintering; wherein the positive electrode material has a single crystal morphology.

[0037] The present invention further provides a positive electrode sheet, comprising the positive electrode material.

[0038] The present invention also provides a sodium ion battery, comprising the positive electrode sheet.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] (1) The nickel-copper-iron-manganese precursor provided by the present invention has the advantages of high tap density and large specific surface area.

[0041] (2) The nickel-copper-iron-manganese precursor provided by the present invention has high mechanical strength.

[0042] (3) The copper ions in the nickel-copper-iron-manganese precursor provided by the present invention are evenly distributed.

[0043] (4) The nickel-copper-iron-manganese precursor provided by the present invention has a low sulfur impurity content.

[0044] (5) The preparation method of the nickel-copper-iron-manganese precursor provided by the present invention uses a copper-ammonia solution as a copper source, making full use of the stability of copper-ammonia, and can reduce the situation where copper ions react directly with ammonia water to generate copper hydroxide precipitation. The use of this method to prepare the nickel-copper-iron-manganese precursor can solve the problem of copper ion segregation (i.e., uneven distribution of copper ions), optimize the particle size distribution, and the uniformity of the obtained nickel-copper-iron-manganese precursor is good, thereby improving the first effect and cycle performance of the positive electrode material.

[0045] (6) The preparation method provided by the present invention can obtain a nickel-copper-iron-manganese precursor with a specific structure, which has both high tap density and high specific surface area.

[0046] (7) The preparation method of the nickel-copper-iron-manganese precursor provided by the present invention can further reduce the generation of crystal defects by adding a stabilizer, thereby reducing the adsorption of impurity S by the crystal defects in the precursor and reducing the impurity sulfur content in the nickel-copper-iron-manganese precursor. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0048] Figure 1 A schematic diagram of the microstructure of secondary particles of the nickel-copper-iron-manganese precursor provided by the present invention;

[0049] Figure 2 This is a SEM image of the nickel-copper-iron-manganese precursor prepared in Example 1 provided by the present invention;

[0050] Figure 3 This is a SEM image of the positive electrode material prepared in Example 1 provided by the present invention. DETAILED DESCRIPTION

[0051] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0052] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0053] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0054] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0055] In a first aspect, the present invention provides a nickel-copper-iron-manganese precursor, wherein the chemical formula of the nickel-copper-iron-manganese precursor is Ni x Cu 1-x-y-x Fe y Mn z (OH)2, where 0.1≤x≤0.6, 0.1≤y≤0.5, 0.1≤z≤0.5, 0.01≤1-xyx≤0.2. Wherein, x includes but is not limited to any one of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6 or a range of values ​​between any two of them; y includes but is not limited to any one of 0.1, 0.2, 0.3, 0.4, 0.5 or a range of values ​​between any two of them; z includes but is not limited to any one of 0.1, 0.2, 0.3, 0.4, 0.5 or a range of values ​​between any two of them; 1-xyx includes but is not limited to any one of 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.08, 0.1, 0.12, 0.14, 0.15, 0.16, 0.18, 0.2 or a range of values ​​between any two of them.

[0056] The nickel-copper-iron-manganese precursor includes secondary particles formed by radially stacked primary grains; that is, along the direction from the center to the surface of the secondary particles, the primary grains are radially stacked.

[0057] The primary crystal grains include first crystal grains having a frame structure and second crystal grains radially filled between the first crystal grains. Figure 1 The figure shows a schematic diagram of the microstructure of the secondary particles of the nickel-copper-iron-manganese precursor provided by the present invention. It can be understood that the first crystal grain is larger than the second crystal grain as a supporting structure. A plurality of second crystal grains are radially filled between the first crystal grain and the first crystal grain. The shapes of the first crystal grain and the second crystal grain are both flaky, and the thickness of the first crystal grain is greater than that of the second crystal grain.

[0058] The tap density of the nickel-copper-iron-manganese precursor is ≥1.4 g / cm 3 ; Including but not limited to 1.4g / cm 3, 1.41g / cm 3 , 1.42g / cm 3 , 1.43g / cm 3 , 1.44g / cm 3 , 1.45g / cm 3 , 1.47g / cm 3 , 1.48g / cm 3 , 1.5g / cm 3 Any point value in or any range of values ​​between them.

[0059] The specific surface area of ​​the nickel-copper-iron-manganese precursor is>30m 2 / g, including but not limited to 31m 2 / g, 32m 2 / g, 33m 2 / g, 34m 2 / g, 35m 2 / g, or a range of values ​​between them.

[0060] The secondary particles of the nickel-copper-iron-manganese precursor provided by the present invention have a frame structure similar to that in a building, which is composed of a frame and bricks. The nickel-copper-iron-manganese precursor can have the advantages of high tap density and large specific surface area at the same time. The positive electrode material prepared by using the nickel-copper-iron-manganese precursor has high first coulomb efficiency (hereinafter referred to as first efficiency) and excellent cycle stability.

[0061] Specifically, the first crystal grains with a framework structure mainly provide compaction and mechanical strength. Higher compaction allows more samples to be loaded during a single sintering process, thereby improving production efficiency (sintering efficiency). High mechanical strength can ensure that the precursor is not easily broken during the preparation of the positive electrode material. The second crystal grains, which are equivalent to bricks and radially filled between the first crystal grains, mainly provide specific surface area. The large specific surface area makes the material have a larger contact area with oxygen during the sintering process, making it easy to sinter into a single crystal positive electrode material.

[0062] In some specific embodiments, the copper source used to prepare the nickel-copper-iron-manganese precursor is a copper-ammonia solution. The nickel-copper-iron-manganese precursor with a specific structure can be obtained by using the copper-ammonia solution as the copper source, and the copper ions in the nickel-copper-iron-manganese precursor are evenly distributed.

[0063] In some specific embodiments, in each of the secondary particles, the number of the first grains is ≥ 6, including but not limited to any point value of 6, 7, 8, 10, 12, 14, 15, 16, 18, 20 or a range value between any two of them.

[0064] In some specific embodiments, the thickness of the first grain is 0.3-1.5 μm, including but not limited to any point value of 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 1.2 μm, 1.3 μm, 1.5 μm or a range value between any two of them.

[0065] In some specific embodiments, the thickness of the second grain is ≤0.1 μm, including but not limited to any point value of 0.1 μm, 0.08 μm, 0.06 μm, 0.05 μm, 0.03 μm, 0.01 μm, 0.005 μm, 0.001 μm, or a range value between any two of them.

[0066] In some specific embodiments, the secondary particles are spherical and / or quasi-spherical in shape.

[0067] In some specific embodiments, the particle size D of the nickel-copper-iron-manganese precursor is 50 It is 3 to 15μm, including but not limited to any point value of 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, and 15μm, or a range value between any two of them.

[0068] In some specific embodiments, the sulfur content in the nickel-copper-iron-manganese precursor is less than 900ppm, the sulfur content in the nickel-copper-iron-manganese precursor is preferably less than 851ppm, and the sulfur content in the nickel-copper-iron-manganese precursor is more preferably less than 600ppm, including but not limited to any point value of 550ppm, 500ppm, 450ppm, 400ppm, 350ppm, 300ppm, 250ppm, 200ppm, 150ppm, 100ppm, 50ppm, 10ppm or any range value between two thereof. The nickel-copper-iron-manganese precursor provided by the present invention has few crystal defects, so the adsorption of impurity S by crystal defects can be reduced, thereby reducing the sulfur content in the nickel-copper-iron-manganese precursor.

[0069] In a second aspect, the present invention provides a controllable preparation method of the nickel-copper-iron-manganese precursor, comprising the following steps: mixing a nickel-iron-manganese mixed salt solution, a complexing agent solution, a precipitant solution and a copper-ammonia solution, and conducting a co-precipitation reaction, and after the co-precipitation reaction is completed, performing solid-liquid separation on the obtained slurry to obtain the nickel-copper-iron-manganese precursor.

[0070] The preparation method of the nickel-copper-iron-manganese precursor provided by the present invention uses a copper-ammonia solution as a copper source, fully utilizing the stability of copper-ammonia, and can reduce the situation where copper ions react directly with ammonia water to generate copper hydroxide precipitation. The preparation of the nickel-copper-iron-manganese precursor using this method can solve the copper ion segregation (i.e., uneven copper ion distribution), optimize the particle size distribution, and the uniformity of the obtained nickel-copper-iron-manganese precursor is good. The positive electrode material generated by the high-temperature solid-phase reaction of the nickel-copper-iron-manganese precursor prepared by this method has good first effect and cycle performance.

[0071] In addition, the above preparation method can be used to obtain a nickel-copper-iron-manganese precursor with a specific structure, which has both high tap density and high specific surface area.

[0072] In some specific embodiments, the molar concentration of copper ions in the copper ammonia solution is 0.2-1.0 mol / L, including but not limited to any one of 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, and 1.0 mol / L, or a range between any two of them.

[0073] In some specific embodiments, the pH of the copper ammonium solution is 9.5-13.0, including but not limited to any point value of 9.5, 10, 10.5, 11, 11.5, 12, 12.5, 13.0 or a range between any two of them.

[0074] In some specific embodiments, the copper ammonia solution further includes a stabilizer. The complexing ability of the stabilizer to copper ions and / or iron ions is greater than the complexing ability of the complexing agent solution to copper ions and / or iron ions. The addition of the stabilizer can further reduce the generation of crystal defects, thereby reducing the adsorption of impurity S by crystal defects in the precursor and reducing the impurity sulfur content in the nickel-copper-iron-manganese precursor.

[0075] In some specific embodiments, the stabilizer includes at least one of acetylacetone, oxalic acid, citric acid, ethylenediaminetetraacetic acid, sulfosalicylic acid, tartaric acid and succinic acid.

[0076] In some specific embodiments, the molar concentration of the stabilizer in the copper ammonia solution is 0.01-0.1 mol / L, including but not limited to any one of 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.05 mol / L, 0.06 mol / L, 0.08 mol / L, and 0.1 mol / L, or a range between any two of them.

[0077] In some specific embodiments, the total molar concentration of metal elements in the nickel-iron-manganese mixed salt solution (i.e., the sum of the molar concentrations of the three elements nickel, cobalt and manganese) is 1.5-3.0 mol / L; including but not limited to any one of 1.5 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L, 2.5 mol / L, 2.8 mol / L, 3.0 mol / L or a range between any two of them.

[0078] In some specific embodiments, the nickel-iron-manganese mixed salt solution further includes an antioxidant, and the antioxidant includes vitamin C. The antioxidant can alleviate the influence of trivalent iron ions and is beneficial to improving the tap density of the material.

[0079] In some specific embodiments, the molar concentration of the antioxidant in the nickel-iron-manganese mixed salt solution is 0.01-0.1 mol / L; including but not limited to any one of 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.05 mol / L, 0.06 mol / L, 0.08 mol / L, 0.1 mol / L or a range between any two of them.

[0080] In some specific embodiments, the molar concentration of the complexing agent in the complexing agent solution is 0.5-2.0 mol / L, including but not limited to any one of 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.3 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L or a range between any two of them.

[0081] In some specific embodiments, the complexing agent solution includes at least one of an aqueous ammonia solution, an oxalic acid solution, a citric acid solution, an ethylenediaminetetraacetic acid solution, and a tartaric acid solution.

[0082] In some specific embodiments, at least two complexing agent solutions are used, or the complexing agent in the complexing agent solution includes at least two complexing agents, which are recorded as the first complexing agent and the second complexing agent. Preferably, the molar ratio of the first complexing agent to the second complexing agent is 1:0.1-2. For example, a mixed solution of oxalic acid and ammonia water is used as the complexing agent solution, wherein the molar ratio of oxalate ions to ammonium ions is 1:0.5-1.5. When two or more complexing agents are used, by adjusting the ratio of each complexing agent, the number of first grains in the material and the thickness of the first grains and the second crystals can be regulated, thereby increasing the specific surface area and tap density of the material.

[0083] In some specific embodiments, the molar concentration of the precipitant in the precipitant solution is 9.8-11.8 mol / L, including but not limited to any point value of 9.8 mol / L, 10 mol / L, 10.3 mol / L, 10.5 mol / L, 10.8 mol / L, 11 mol / L, 11.2 mol / L, 11.5 mol / L, 11.8 mol / L or a range value between any two of them.

[0084] In some specific embodiments, the precipitant solution comprises a sodium hydroxide solution.

[0085] In some specific embodiments, after the coprecipitation reaction is completed and before the solid-liquid separation, an aging step is also included.

[0086] In some specific embodiments, the aging is performed under an inert atmosphere such as a nitrogen atmosphere.

[0087] In some specific implementations, the aging time is 3 to 6 hours.

[0088] In some specific embodiments, after the solid-liquid separation, the steps of washing, drying and screening are further included.

[0089] In some specific embodiments, the mixing and the coprecipitation reaction are carried out under an inert atmosphere to prevent the oxidation of the slurry from affecting the physical and chemical properties of the precursor particles. A liquid seal may also be provided at the nitrogen outlet of the reactor to further prevent oxygen from entering and reduce the escape of ammonia into the environment.

[0090] In some specific embodiments, the inert atmosphere includes but is not limited to a nitrogen atmosphere.

[0091] In some specific embodiments, the coprecipitation reaction specifically includes: the first stage (granulation): controlling the pH of the reaction system to be 11.0-13.0 (including but not limited to any one of 11, 11.3, 11.5, 11.8, 12, 12.3, 12.5, 12.8, 13 or a range between any two of them), and the ammonium ion concentration to be 2-5 g / L (including but not limited to any one of 2 g / L, 3 g / L, 4 g / L, 5 g / L or a range between any two of them), and conducting a first coprecipitation reaction, wherein the time of the first coprecipitation reaction is 10-90 min (including but not limited to any one of 10 min, 30 min, 40 min, 60 min, 80 min, 90 min or a range between any two of them). The second stage (growth): increasing the feed rate of the nickel-iron-manganese mixed salt solution to 1.2 to 3.0 times (including but not limited to 1.2 times, 1.5 times, 1.8 times, 2 times, 2.3 times, 2.5 times, 2.8 times, 3 times any one of the point values ​​or any range values ​​between two of them) of the feed rate of the nickel-iron-manganese mixed salt solution during the first coprecipitation reaction, and increasing the feed rate of the copper-ammonia solution to 1.2 to 3.0 times (including but not limited to 1.2 times, 1.5 times, 1.8 times, 2 times, 2.3 times, 2.5 times, 2.8 times, 3 times any one of the point values ​​or any range values ​​between two of them) of the feed rate of the copper-ammonia solution during the first coprecipitation reaction. The present invention adopts a one-step method to prepare nickel-copper-iron-manganese precursor, and the operation is relatively simple. Among them, increasing the feed flow rate of the complexing agent solution to 1.5 to 4.0 times (including but not limited to 1.5 times, 1.8 times, 2 times, 2.3 times, 2.5 times, 2.8 times, 3 times, 3.5 times, 4 times any one of the point values ​​or the range value between any two) of the feed flow rate of the complexing agent solution during the first coprecipitation reaction, and adjusting the pH of the reaction system to 9.5 to 12.0 (including but not limited to 9.5, 10, 10.5, 11, 11.3, 11.5, 11.8, any one of the point values ​​or the range value between any two), and performing a second coprecipitation reaction until the particles grow to the desired particle size. The present invention adopts a one-step method to prepare nickel-copper-iron-manganese precursor, and the operation is relatively simple. Among them, increasing the feed flow rate of the nickel-iron-manganese mixed salt solution is beneficial to increasing the yield of the material per unit time.

[0092] In some specific embodiments, the first stage (granulation) specifically includes: under the protection of an inert atmosphere, deionized water, a precipitant solution and a complexing agent solution are introduced into the reactor, and the pH of the mixed material in the reactor is adjusted to 11.0-13.0 and the ammonium ion concentration is adjusted to 2.0-5.0 g / L. Then, the reactor stirring system and the heating device are turned on, and nitrogen is introduced into the reactor at the same time. After ventilation for 1-2 hours and the temperature of the reactor is stable, the nickel-iron-manganese mixed salt solution, the copper-ammonia solution, the precipitant solution and the complexing agent solution are added to the reactor at the same time, and the reaction is carried out for 10-90 minutes.

[0093] In some specific embodiments, the second stage (growth) specifically includes: increasing the feed flow rate of the nickel-iron-manganese mixed salt solution and the copper-ammonia solution to 1.2 to 3.0 times that of the first stage, adjusting the feed flow rate of the complexing agent solution to 1.5 to 4.0 times that of the first stage, and adjusting the amount of the precipitant solution to make the pH of the reaction system 9.5 to 12.0 until the precursor particle size meets the requirements.

[0094] In some specific embodiments, the reaction system temperature of the first coprecipitation reaction is 40-50° C. The reaction system temperature of the second coprecipitation reaction is 60-70° C.

[0095] In a third aspect, the present invention provides a positive electrode material, which is mainly formed by mixing the nickel-copper-iron-manganese precursor with a sodium source and then sintering the mixture.

[0096] Wherein, the positive electrode material has a single crystal morphology.

[0097] The positive electrode material provided by the present invention has a single crystal morphology with a smooth surface. The positive electrode material with a single crystal structure helps to reduce stress and inhibit cracks. In addition, the material itself has no pores and can withstand greater forces without breaking during the calendering process. Therefore, the positive electrode material has good electrochemical properties after being assembled into a battery, and its first effect and cycle performance are good.

[0098] In some specific embodiments, the sintering is performed in an air atmosphere and / or an oxygen atmosphere.

[0099] In some specific embodiments, the sintering method includes: heating to 400-600° C. at a heating rate of 1-5° C. / min and keeping warm for 4-8 hours, then heating to 800-1000° C. at a heating rate of 1-5° C. / min and keeping warm for 12-24 hours.

[0100] In some specific embodiments, the molar ratio of the nickel-copper-iron-manganese precursor to the sodium element in the sodium source is 1:1.03-1.06.

[0101] In some specific embodiments, the sodium source includes any sodium-containing compound commonly used in the art, such as sodium carbonate, but not limited thereto.

[0102] In a fourth aspect, the present invention provides a positive electrode sheet comprising the positive electrode material.

[0103] The positive electrode sheet has high initial efficiency and excellent cycle performance.

[0104] In some specific implementations, the positive electrode sheet further includes a binder and a conductive agent, which is not limited in the present invention.

[0105] In a fifth aspect, the present invention provides a sodium ion battery comprising the positive electrode sheet.

[0106] The sodium-ion battery has high initial coulombic efficiency and good cycle performance.

[0107] In some specific embodiments, the sodium ion battery further includes a negative electrode sheet, a separator and an electrolyte, which is not limited in the present invention.

[0108] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0109] Example 1

[0110] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 The preparation method of (OH)2 comprises the following steps:

[0111] (1) According to the molar ratio of nickel, iron and manganese elements being 6:5:8, the sulfates of nickel, iron and manganese are weighed to prepare a mixed sulfate solution with a total molar concentration of metal elements of 1.5 mol / L. A sodium hydroxide solution with a molar concentration of 9.8 mol / L is prepared. A 1.5 mol / L complexing agent solution is prepared using ammonia water. Copper sulfate is weighed and mixed with ammonia water to prepare a copper ammonia solution with a pH of 10.3 and a copper ion molar concentration of 0.5 mol / L, and a stabilizer sulfosalicylic acid is added thereto to a concentration of 0.05 mol / L.

[0112] (2) Add deionized water and sodium hydroxide solution to the reactor, adjust its pH to 11.2, open the nitrogen valve to introduce nitrogen into the system, and the ventilation time is 1 hour. Add ammonia water to the reactor, adjust the ammonium ion concentration to 3.5g / L, and adjust the reactor temperature to 40°C. Add the prepared mixed sulfate solution, copper ammonia solution, sodium hydroxide solution, and complexing agent solution to the reactor in parallel for coprecipitation reaction (control the reaction system pH to 11.0-11.3, and the ammonium ion concentration to 3.0-4.0g / L; wherein, the reaction system pH and ammonium ion concentration cannot be guaranteed to be stable at a fixed value, and there will be fluctuations, so it is a range value). The reaction time of the first stage is controlled at 30min.

[0113] After the reaction time is reached, the reaction temperature is raised to 60°C, the feed flow rates of the mixed sulfate solution and the copper ammonia solution are increased to 2.0 times and 2.0 times of the first stage respectively, and the feed flow rate of the complexing agent solution is increased to 3.0 times of the first stage. By adjusting the feed flow rate of the sodium hydroxide solution, the pH of the reaction system is controlled to be 10.7-11.0 (the pH of the reaction system cannot be guaranteed to be stable at a fixed value and will fluctuate, so it is a range value). When the particle size D of the slurry in the reactor is 50 After reaching 5 μm, the feed was stopped.

[0114] (3) After stopping the feeding, the stirring speed is reduced to 50% and the stirring is continued, while ensuring that nitrogen is introduced for aging. After stirring for 4 hours, the slurry is transferred out, washed, dried, and sieved to obtain a nickel-copper-iron-manganese precursor.

[0115] The positive electrode material NaNi provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 The preparation method of O2 includes the following steps: grinding the above-obtained nickel-copper-iron-manganese precursor and sodium carbonate in a mortar at a molar ratio of 1:1.04 between the precursor and the sodium element to make the two fully mixed; then, in an oxygen atmosphere, heating the temperature to 500°C at a heating rate of 3°C / min and keeping it for 6 hours, then heating the temperature to 900°C at a heating rate of 2°C / min and keeping it for 14 hours, naturally cooling to room temperature, and then sieving to obtain a single crystal nickel-copper-iron-manganese positive electrode material.

[0116] The SEM image of the nickel-copper-iron-manganese precursor prepared in this example is shown in Figure 2As shown. It can be seen that the primary grains in the secondary particles of the nickel-copper-iron-manganese precursor are arranged radially. The primary grains include a framework (first grain) and bricks (second grain), and the framework (first grain) and bricks (second grain) are stacked alternately, and the larger gaps in the framework are filled by bricks, thereby increasing the specific surface area of ​​the precursor. The shapes of the first grain and the second grain are both flaky, and the size of the first grain is larger than that of the second grain. The shape of the secondary particle is spherical. The number of first grains in the secondary particle is 6-9, the thickness of the first grain is 0.4-0.9μm, and the thickness of the second grain is 0.03-0.07μm.

[0117] The SEM image of the positive electrode material prepared in this embodiment is shown in Figure 3 As shown. It can be seen that the cathode material as a whole presents a single crystal structure, with a smooth surface and relatively uniform particle size.

[0118] Example 2

[0119] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.04 Fe 0.26 Mn 0.40 The preparation method of (OH)2 is basically the same as the preparation method of the precursor in Example 1, except that: in step (1), the molar ratio of nickel, iron and manganese elements is replaced by 15:13:20, and the stabilizer is replaced by succinic acid. In addition, the complexing agent solution is replaced by a mixed solution of oxalic acid and ammonia water, wherein the molar ratio of oxalate ion to ammonium ion is 1:0.75.

[0120] The number of first grains in the secondary particles of the nickel-copper-iron-manganese precursor prepared in this embodiment is 7-9, the thickness of the first grains is 0.5-0.8 μm, and the thickness of the second grains is 0.01-0.06 μm.

[0121] Further, referring to the preparation method of the positive electrode material in the embodiment, the nickel-copper-iron-manganese precursor prepared in this embodiment is prepared into a positive electrode material NaNi 0.30 Cu 0.04 Fe 0.26 Mn 0.40 O2.

[0122] Example 3

[0123] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.03 Fe 0.27 Mn 0.40The preparation method of (OH)2 is basically the same as the preparation method of the precursor in Example 1, except that in step (1), the molar ratio of nickel, iron and manganese elements is replaced by 30:27:40, the stabilizer is replaced by acetylacetone, and the complexing agent solution is replaced by oxalic acid solution.

[0124] The number of first grains in the secondary particles of the nickel-copper-iron-manganese precursor prepared in this embodiment is 7-10, the thickness of the first grains is 0.4-0.7 μm, and the thickness of the second grains is 0.01-0.06 μm.

[0125] Further, referring to the preparation method of the positive electrode material in the embodiment, the nickel-copper-iron-manganese precursor prepared in this embodiment is prepared into a positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 O2.

[0126] Example 4

[0127] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 The preparation method of O2 is basically the same as that of Example 1, except that in step (1), the stabilizer is replaced by tartaric acid.

[0128] Example 5

[0129] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 The preparation method of O2 is basically the same as that of Example 1, except that in step (1), the stabilizer is replaced by ethylenediaminetetraacetic acid.

[0130] Example 6

[0131] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27Mn 0.40 The preparation method of O2 is basically the same as that in Example 1, except that in step (1), the pH of the copper ammonia solution is adjusted to 9.9.

[0132] Example 7

[0133] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 The preparation method of O2 is basically the same as that of Example 1, except that in step (1), the molar concentration of copper ions in the copper ammonia solution is adjusted to 0.8 mol / L.

[0134] Example 8

[0135] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.03 Fe 0.27 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 The preparation method of O2 is basically the same as that of Example 3, except that: in step (1), the nickel-iron-manganese mixed salt solution also includes an antioxidant vitamin C (i.e., vitamin C is dissolved in a mixed sulfate solution), and the molar concentration of the antioxidant vitamin C in the nickel-iron-manganese mixed salt solution is controlled to be 0.05 mol / L.

[0136] Example 9

[0137] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 The preparation method of (OH)2 comprises the following steps:

[0138] (1) According to the molar ratio of nickel, iron and manganese elements being 6:5:8, the sulfates of nickel, iron and manganese are weighed to prepare a mixed sulfate solution with a total molar concentration of metal elements of 2.0 mol / L. A sodium hydroxide solution with a molar concentration of 10.5 mol / L is prepared. A 2.0 mol / L complexing agent solution is prepared using ammonia water. Copper sulfate is weighed and mixed with ammonia water to prepare a copper ammonia solution with a pH of 10.5 and a copper ion molar concentration of 0.7 mol / L, and a stabilizer sulfosalicylic acid is added thereto to a concentration of 0.1 mol / L.

[0139] (2) Add deionized water and sodium hydroxide solution to the reactor, adjust its pH to 11.6, open the nitrogen valve to introduce nitrogen into the system, and the ventilation time is 2 hours. Add ammonia water to the reactor, adjust the ammonium ion concentration to 4.3g / L, and adjust the reactor temperature to 45°C. Add the prepared mixed sulfate solution, copper ammonia solution, sodium hydroxide solution, and complexing agent solution to the reactor in parallel for coprecipitation reaction (control the reaction system pH to 11.5-11.7, and the ammonium ion concentration to 4.0-4.5g / L; wherein, the reaction system pH and ammonium ion concentration cannot be guaranteed to be stable at a fixed value, and there will be fluctuations, so it is a range value). The reaction time of the first stage is controlled at 20min.

[0140] After the reaction time is reached, the reaction temperature is raised to 70°C, the feed flow rates of the mixed sulfate solution and the cuprammonia solution are increased to 1.5 times and 1.5 times of the first stage respectively, and the feed flow rate of the complexing agent solution is increased to 2.0 times of the first stage. By adjusting the feed flow rate of the sodium hydroxide solution, the pH of the reaction system is controlled to be 11.0-11.3; when the particle size D of the slurry in the reactor is 50 After reaching 5.0 μm, the feed was stopped.

[0141] (3) After stopping the feeding, the stirring speed is reduced to 50% and the stirring is continued, while ensuring that nitrogen is introduced for aging. After stirring for 4 hours, the slurry is transferred out, washed, dried, and sieved to obtain a nickel-copper-iron-manganese precursor.

[0142] The nickel-copper-iron-manganese precursor prepared in this embodiment was used to prepare the positive electrode material according to the method for preparing the positive electrode material provided in Example 1. 0.30 Cu 0.05 Fe 0.25 Mn 0.40 Preparation of O2 positive electrode materials.

[0143] Example 10

[0144] The nickel-copper-iron-manganese precursor Ni provided in this embodiment 0.30 Cu 0.05 Fe 0.25 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 The preparation method of O2 is basically the same as that of Example 1, except that no stabilizer is added to the copper ammonia solution.

[0145] Comparative Example 1

[0146] The nickel-copper-iron-manganese precursor Ni provided in this comparative example 0.30 Cu 0.05 Fe0.25 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.03 Fe 0.27 Mn 0.40 The preparation method of O2 is basically the same as that of Example 1, except that the copper ammonia solution is replaced by a copper sulfate solution with an equimolar concentration to that of copper ions.

[0147] Comparative Example 2

[0148] The nickel-copper-iron-manganese precursor Ni provided in this comparative example 0.30 Cu 0.04 Fe 0.26 Mn 0.40 (OH)2 and positive electrode material NaNi 0.30 Cu 0.04 Fe 0.26 Mn 0.40 The preparation method of O2 is basically the same as that of Example 2, except that the copper ammonia solution is replaced by a copper sulfate solution with an equimolar concentration to that of copper ions.

[0149] The tap density, specific surface area and sulfur content of the nickel-copper-iron-manganese precursors prepared in the above embodiments and comparative examples were respectively tested, and the results are shown in Table 1.

[0150] The positive electrode materials prepared in each embodiment and each comparative example were mixed with carbon black conductive agent (SP) and polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1, and N-methylpyrrolidone (NMP) was used as solvent. After homogenization-coating-drying-slicing, a positive electrode sheet was prepared, which was mixed with electrolyte sodium hexafluorophosphate and metal sodium sheet to prepare sodium ion half-cell. Then the electrochemical performance of each half-cell was tested respectively: 0.1C charge and discharge in the first cycle; 0.1C charge and 1C discharge in the second cycle, and 50 cycles of testing; the test voltage was 2.0 4.0V.

[0151] Table 1 Physical and chemical indicators of nickel-copper-iron-manganese precursors and electrochemical test results of batteries

[0152]

[0153] It can be seen from Table 1 above that the tap density and specific surface area of ​​the precursors prepared in each embodiment are relatively high, wherein the tap density is 1.4 g / cm 3 Above, the specific surface area is 30m 2 / g or more, it can be seen that the precursor has the characteristics of high tap compaction and large specific surface area. At the same time, the sulfur impurity content in the precursor prepared in each embodiment is low.

[0154] Moreover, the positive electrode material obtained after solid-phase sintering of the precursors prepared in each embodiment has a high initial efficiency and a high capacity retention rate, which are better than those of the comparative examples, indicating that the positive electrode material provided by the present invention has better structural stability.

[0155] Furthermore, by comparing Example 1, Example 6 and Example 7, it can be seen that the pH of the copper ammonia solution and the molar concentration of copper ions will have a certain effect on the tap density and specific surface area of ​​the nickel-copper-iron-manganese precursor.

[0156] By comparing Example 3 and Example 8, it can be seen that the antioxidant will have a certain effect on the tap density and capacity of the nickel-copper-iron-manganese precursor.

[0157] By comparing Example 1 and Example 10, it can be seen that whether or not to add a stabilizer will have a certain impact on the sulfur impurity content in the nickel-copper-iron-manganese precursor.

[0158] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A nickel-copper-iron-manganese precursor, characterized in that: The chemical formula of the nickel-copper-iron-manganese precursor is Ni x Cu 1-x-y- x Fe y Mn z (OH)2, where 0.1≤x≤0.6, 0.1≤y≤0.5, 0.1≤z≤0.5, 0.01≤1-xyx≤0.2; The nickel-copper-iron-manganese precursor comprises secondary particles formed by radially stacked primary crystal grains; wherein the primary crystal grains comprise first crystal grains having a framework structure, and second crystal grains radially filled between the first crystal grains; the first crystal grains and the second crystal grains are both in the shape of flakes; The tap density of the nickel-copper-iron-manganese precursor is ≥1.4 g / cm 3 ; The specific surface area of ​​the nickel-copper-iron-manganese precursor is>30m 2 / g.

2. The nickel-copper-iron-manganese precursor according to claim 1, characterized in that: At least one of the following conditions is met: (1) In each of the secondary particles, the number of the first crystal grains is ≥ 6; (2) The thickness of the first crystal grain is 0.3 to 1.5 μm; (3) The thickness of the second grain is ≤0.1 μm; (4) The shape of the secondary particles includes spherical and / or quasi-spherical shapes; (5) The particle size D of the nickel-copper-iron-manganese precursor 50 3~15μm.

3. The nickel-copper-iron-manganese precursor according to claim 1, characterized in that: The sulfur content in the nickel-copper-iron-manganese precursor is less than 600 ppm.

4. The method for preparing the nickel-copper-iron-manganese precursor according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: mixing a nickel-iron-manganese mixed salt solution, a complexing agent solution, a precipitant solution and a cuprammonia solution and carrying out a coprecipitation reaction, and then performing solid-liquid separation to obtain the nickel-copper-iron-manganese precursor.

5. The method for preparing the nickel-copper-iron-manganese precursor according to claim 4, characterized in that: At least one of the following conditions is met: (1) The molar concentration of copper ions in the copper ammonia solution is 0.2 to 1.0 mol / L; (2) The pH of the copper ammonium solution is 9.5 to 13.0; (3) The copper ammonia solution also includes a stabilizer, the complexing ability of the stabilizer for copper ions and / or iron ions is greater than the complexing ability of the complexing agent solution for copper ions and / or iron ions, and the stabilizer includes at least one of acetylacetone, oxalic acid, citric acid, ethylenediaminetetraacetic acid, sulfosalicylic acid, tartaric acid and succinic acid; the molar concentration of the stabilizer in the copper ammonia solution is 0.01 to 0.1 mol / L.

6. The method for preparing the nickel-copper-iron-manganese precursor according to claim 4, characterized in that: At least one of the following conditions is met: (1) The total molar concentration of metal elements in the nickel-iron-manganese mixed salt solution is 1.5 to 3.0 mol / L; (2) The nickel-iron-manganese mixed salt solution also includes an antioxidant, the antioxidant includes vitamin C, and the molar concentration of the antioxidant in the nickel-iron-manganese mixed salt solution is 0.01 to 0.1 mol / L; (3) The molar concentration of the complexing agent in the complexing agent solution is 0.5 to 2.0 mol / L; (4) the complexing agent solution comprises at least one of an aqueous ammonia solution, an oxalic acid solution, a citric acid solution, an ethylenediaminetetraacetic acid solution and a tartaric acid solution; (5) The molar concentration of the precipitant in the precipitant solution is 9.8 to 11.8 mol / L; (6) The precipitant solution includes a sodium hydroxide solution; (7) After the coprecipitation reaction is completed and before the solid-liquid separation, an aging step is also included; (8) After the solid-liquid separation, the steps of washing, drying and screening are also included; (9) The mixing and the coprecipitation reaction are carried out under an inert atmosphere.

7. The method for preparing the nickel-copper-iron-manganese precursor according to claim 4, characterized in that: The coprecipitation reaction specifically includes: first controlling the pH of the reaction system to 11.0-13.0 and the ammonium ion concentration to 2-5 g / L, and performing a first coprecipitation reaction, wherein the time of the first coprecipitation reaction is 10-90 min; then increasing the feed flow rate of the nickel-iron-manganese mixed salt solution to 1.2-3.0 times the feed flow rate of the nickel-iron-manganese mixed salt solution during the first coprecipitation reaction, increasing the feed flow rate of the copper-ammonia solution to 1.2-3.0 times the feed flow rate of the copper-ammonia solution during the first coprecipitation reaction, and increasing the feed flow rate of the complexing agent solution to 1.5-4.0 times the feed flow rate of the complexing agent solution during the first coprecipitation reaction, and adjusting the pH of the reaction system to 9.5-12.0, and performing a second coprecipitation reaction until the particles grow to the desired particle size.

8. A positive electrode material, characterized in that It is mainly formed by mixing the nickel-copper-iron-manganese precursor described in any one of claims 1 to 3 with a sodium source and then sintering; the positive electrode material has a single crystal morphology.

9. A positive electrode sheet, characterized in that: Comprising the positive electrode material as claimed in claim 8.

10. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 9.