PEGylated biological antifouling substrate as well as preparation method and application thereof
By forming a single molecular layer of silanized polyolefinic glycol methacrylate on the glass substrate, the problem of insufficient biocompatibility and protein resistance to protein adsorption function is solved, and PEGylated biofouling substrate is realized High hydrophilicity and stability, suitable for biological experiments.
Patent Information
- Application Number
- CN202411212537.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
Existing glass substrates have insufficient biocompatibility and protein-resistant adsorption functions in biological experiments, making it difficult to directly apply to cell culture and genetic testing fields.
After calcination and hydroxylation treatment, silanized polyolefinic glycol methacrylate reacts with the surface of the glass substrate to form a uniform monolayer containing oligoethylene glycol, improving its hydrophilicity and anti-protein adsorption Function, prepare PEGylated biofouling substrate.
It significantly improves the biocompatibility and protein adsorption function of glass substrates, provides excellent hydrophilicity and thermal stability, is suitable for cell culture, genetic testing and other fields, and is simple in preparation and low in cost, suitable for large-scale Production.
Smart Images

Figure HDA0005020659670000011
Abstract
Description
Technical Field
[0001] The present application relates to the field of biochip surface modification, and in particular to a PEGylated bio-antifouling substrate and a preparation method and application thereof. Background Art
[0002] Biochip generally refers to a microarray hybrid chip in which bioinformatics molecules are fixed at high density on a mutually supporting medium. Simply put, a biochip is to place a biological sample on a piece of glass, silicon wafer, polyacrylamide gel, nylon membrane and other materials, and then use an instrument to collect signals and a computer to analyze the data results. Like laboratory testing, the detection of blood sugar, protein, enzyme activity, etc. on a biochip is also based on the same biological reaction principle. Therefore, a biochip is a carrier platform. Gene detection is one of the application areas of biochips. Since biochips are usually made of glass, silicon wafers, polyacrylamide gel, nylon membranes, etc., glass materials are the most widely used. Glass slides without further surface modification cannot be directly used in cell culture, gene detection and other fields because of their poor biocompatibility or resistance to protein adsorption. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present application provides a PEGylated bio-antifouling substrate and its preparation method and application. The PEGylated bio-antifouling substrate prepared by the present application has excellent hydrophilicity, significantly improves the biocompatibility and anti-protein adsorption function of the glass substrate, and thus plays an important role in biological experiments. PEG has good biocompatibility, low toxicity, and electrical neutrality, and will not cause rejection reactions in the body. These characteristics make the PEGylated bio-antifouling substrate widely used in the fields of cell culture, gene detection, etc. In addition, the preparation method of the present application is simple, the reaction conditions are mild, the cost is low, and it is suitable for large-scale production.
[0004] In a first aspect, the present application provides a method for preparing a PEGylated bio-antifouling substrate, using the following technical scheme: A method for preparing a PEGylated bio-antifouling substrate comprises the following steps: S1, calcining the glass substrate at 400-500° C. for 2-3 hours to remove organic impurities on the surface, then washing with ultrapure water, and then performing hydroxylation treatment to obtain a hydroxylated glass substrate; S2. After adjusting the pH value to 2-3 by adding acid to 100 parts of 90% ethanol aqueous solution, add and mix evenly with 15 parts of silylated polymethacrylate oligoethylene glycol ester solution to obtain a mixed solution; then put the hydroxylated glass substrate into the mixed solution, react at 60-80°C in a water bath for 6-8 hours, and finally dehydrate at 90°C-100°C for 3-4 hours to obtain a PEGylated biofouling substrate.
[0005] By adopting the above technical scheme, S1, calcining the glass substrate at 400-500°C for 2-3h to remove organic impurities on the surface, then washing it with ultrapure water, and then performing hydroxylation treatment to obtain a hydroxylated glass substrate. The role of this step is to remove organic impurities on the surface of the glass substrate, improve its surface activity, and provide better conditions for subsequent reactions. S2, adding acid to 100 parts of 90% ethanol aqueous solution to adjust the pH value to 2-3, then adding and mixing with 15 parts of silanized polymethacrylate oligoethylene glycol ester solution to obtain a mixed solution; then placing the hydroxylated glass substrate into the mixed solution, reacting in a water bath at 60-80°C for 6-8 hours, and finally dehydrating at 90°C-100°C for 3-4h to obtain a PEGylated biofouling substrate. The role of this step is to form a uniform monolayer containing oligoethylene glycol on the surface of the hydroxylated glass substrate (silanized polymethacrylate oligoethylene glycol ester, one end of which is a siloxane group, which can be covalently bonded to the hydroxyl group of the glass substrate, and the other end is a PEG (actually oligoethylene glycol) segment, which can provide anti-cell adhesion. Using the molecular self-assembly method, the silanized polymethacrylate oligoethylene glycol ester can form a uniformly distributed monolayer containing oligoethylene glycol on the surface of the glass substrate), thereby giving the glass substrate excellent hydrophilicity, biocompatibility and anti-protein adsorption function. Through the synergistic effect of these steps, the PEGylated bio-antifouling substrate prepared by the present application has excellent properties, such as good hydrophilicity, biocompatibility, anti-protein adsorption function and thermal stability. These characteristics make the PEGylated bio-antifouling substrate play an important role in biological experiments, such as cell culture, gene detection and other fields have a wide range of applications. In addition, the preparation method of the present application is simple, the reaction conditions are mild, the cost is low, and it is suitable for large-scale production.
[0006] Preferably, in step S1, the process of hydroxylation treatment is: placing the glass substrate after washing with ultrapure water into a mixed solution of sodium hydroxide: water: isopropanol in a mass ratio of 3-4:18:21, ultrasonicating for 30-40 minutes, then washing with deionized water for 3 times, then washing with ethanol, and drying with nitrogen after washing.
[0007] By adopting the above technical scheme, the hydroxylation treatment process in step S1 is a key step in preparing the PEGylated biofouling-proof substrate, and its effects and synergistic effects are as follows: 1. Increasing hydroxyl groups: The cleaned glass substrate is placed in a mixed solution of sodium hydroxide, water and isopropanol for ultrasonic treatment to increase the number of hydroxyl groups on the surface of the glass substrate. Hydroxyl groups are the key groups for the combination of silylated poly(ethylene methacrylate oligomer) and the glass substrate, so the hydroxylation treatment can increase the grafting rate of silylated poly(ethylene methacrylate oligomer) on the glass substrate. 2. Improving hydrophilicity: The surface of the glass substrate after hydroxylation treatment has more hydroxyl groups, which can form hydrogen bonds with water molecules, thereby improving the hydrophilicity of the glass substrate. Hydrophilicity is one of the important factors for the PEGylated biofouling-proof substrate to have excellent anti-protein adsorption properties. 3. Promote the grafting of silylated poly(ethylene methacrylate oligomer) esters: The surface of the glass substrate after hydroxylation treatment has more hydroxyl groups, which can covalently bond with the siloxane groups of silylated poly(ethylene methacrylate oligomer) esters, thereby promoting the grafting of silylated poly(ethylene methacrylate oligomer) esters on the glass substrate. 4. Improve stability: The surface of the glass substrate after hydroxylation treatment has more hydroxyl groups, which can covalently bond with the siloxane groups of silylated poly(ethylene methacrylate oligomer) esters, thereby improving the stability of the PEGylated bio-antifouling substrate. In summary, the hydroxylation treatment process in step S1 plays a key role in the preparation of PEGylated bio-antifouling substrates. By increasing the number of hydroxyl groups on the surface of the glass substrate, the grafting rate of silylated poly(ethylene methacrylate oligomer) esters on the glass substrate is increased, thereby improving the anti-protein adsorption performance and stability of the PEGylated bio-antifouling substrate.
[0008] Preferably, in step S2, the method for preparing the silylated poly(ethylene glycol) methacrylate solution comprises the following steps: S31, after uniformly mixing the silane coupling agent, triethylamine and dichloromethane according to their mass fractions, cool the mixture to -5 to 0°C in an ice bath under nitrogen protection, and then slowly add the initiator thereto to carry out an amidation reaction for 6-8h, and vacuum dry the product at 50°C for 8-10h, and vacuum dry it at 48°C to obtain a silylation initiator; S32. According to the mass fractions, methacrylate oligoethylene glycol ester, catalyst and isopropanol are heated to 40-50° C. under nitrogen protection, and then a silylation initiator is added thereto to carry out an atom transfer radical polymerization reaction for 12-16 hours to obtain a silylated polymethacrylate oligoethylene glycol ester solution.
[0009] The function of the prepared silylated poly(ethylene glycol methacrylate) solution by adopting the above technical scheme is to combine the silylation initiator with the methacrylate oligo(ethylene glycol) through an atom transfer free radical polymerization reaction to form a polymer having a siloxane group and a PEG segment. This polymer can be covalently bonded to the hydroxyl group on the glass substrate to form a uniformly distributed monolayer containing oligo(ethylene glycol), thereby improving the hydrophilicity, biocompatibility and anti-protein adsorption function of the glass substrate.
[0010] Preferably, the mass ratio of the silane coupling agent, triethylamine, dichloromethane and initiator is 3.5:3.1:(42-48):3.
[0011] Preferably, the silane coupling agent is composed of 3-aminopropyltriethoxysilane, γ-chloropropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane in a mass ratio of 3:4:3.
[0012] By adopting the above technical scheme, the main role of the silane coupling agent in the present invention is to serve as a bridge connecting the glass substrate and the PEG segment. The combination of the three silane coupling agents, 3-aminopropyltriethoxysilane, γ-chloropropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, can provide a variety of reaction sites and functions, enhance the binding force with the glass substrate, and provide the necessary chemical groups for the subsequent grafting of PEG segments. 3-Aminopropyltriethoxysilane (APTES): This silane coupling agent contains an amino (-NH2) end, which can react with the hydroxyl group on the glass surface through this amino group to form a stable covalent bond. In addition, its ethoxysilane part can be hydrolyzed and react with the silanol group on the glass surface to further enhance the binding force. γ-Chloropropyltriethoxysilane (CPTES): This silane coupling agent provides a chloropropyl (-CH2CH2CH2Cl) end, which can react with other molecules through chlorine atoms, such as reacting with the hydroxyl groups on the PEG segment to achieve PEG fixation. N-β-(Aminoethyl)-γ-aminopropylmethyldimethoxysilane (a bifunctional silane coupling agent): This coupling agent has two different functional groups, one is amino and the other is methoxysilane, which allows it to react with the glass surface and PEG segments in different directions, increasing the diversity and stability of the binding. The synergistic effect is reflected in the fact that the different functional groups of these silane coupling agents can react with the glass surface and PEG segments in a complementary manner to form a multi-directional cross-linked network structure, which improves the stability and functionality of the PEGylated bio-antifouling substrate. Through this synergistic effect, a more uniform and stable PEG covering layer can be achieved, thereby effectively improving the anti-protein adsorption performance and biocompatibility of the substrate.
[0013] Preferably, the initiator is α-bromoisobutyryl bromide.
[0014] Preferably, the mass ratio of the methacrylate oligoethylene glycol ester, the catalyst, isopropanol and the silylation initiator is 95:4.8:(400-450):3.8.
[0015] Preferably, the catalyst is composed of cuprous bromide and 2,2-bipyridine in a mass ratio of 1:3.
[0016] In a second aspect, the present application provides a PEGylated bio-antifouling substrate, which adopts the following technical solution: As a general technical concept, the present application also provides a PEGylated bio-antifouling substrate prepared by the above-mentioned method for preparing a PEGylated bio-antifouling substrate.
[0017] In the third aspect, the present application provides an application of a PEGylated bio-antifouling substrate, adopting the following technical solution: As a general technical concept, the present application also provides the application of the above-mentioned PEGylated bio-antifouling substrate in drug carriers, protein detection chips, biological micro-electromechanical systems and biosensors.
[0018] In summary, the present application includes at least one of the following beneficial technical effects: 1. Excellent hydrophilicity and biocompatibility: The glass substrate treated with PEGylation exhibits significant hydrophilicity, which not only improves the biocompatibility of the substrate, but also enhances its anti-protein adsorption function. This is particularly important for biological experiments because it can reduce the adsorption of nonspecific proteins and obtain more accurate experimental results.
[0019] 2. Wide application fields: Due to the low toxicity, electrical neutrality and good biocompatibility of PEG, PEGylated bio-antifouling substrates have broad application prospects in the fields of cell culture, gene detection, etc. These characteristics make the substrates not cause rejection reactions in the body when used, providing a safe and effective platform for biomedical research.
[0020] 3. Simple and low-cost preparation method: The preparation method provided in this application is not only simple in steps and mild in reaction conditions, but also low in cost and suitable for large-scale production. This means that a large number of PEGylated bio-antifouling substrates can be efficiently produced to meet the growing market demand.
[0021] 4. Stable performance: Tests have shown that the PEGylated bio-antifouling substrate not only has good anti-protein adsorption performance, but also can maintain long-term stability under physiological conditions. This is particularly important for situations that require long-term observation or experiments, ensuring the reliability of experimental results.
[0022] 5. Molecular self-assembly to form a uniform monolayer: By utilizing the properties of silanized poly(ethylene glycol methacrylate) oligomers, a uniformly distributed monolayer containing oligoethylene glycol can be formed on the surface of the glass substrate. This uniform surface modification is crucial to improving the performance of the substrate because it ensures that the anti-cell adhesion effect of each area is consistent. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following is a brief introduction to the drawings used in the embodiments: Figure 1 3 is a graph showing the results of a fibrin adsorption test, in which a represents the hydroxylated glass substrate prepared in Example 3, b represents the PEGylated bio-antifouling substrate prepared in Example 3 before adsorbing fibrin, c represents the PEGylated bio-antifouling substrate prepared in Example 3 after adsorbing fibrin, and d represents the PEGylated bio-antifouling substrate prepared in Example 3 after being placed in a 1 mg / ml fibrin PBS buffer solution at 37°C for 28 days. DETAILED DESCRIPTION
[0024] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0025] In the following examples, 1 portion means 10 g.
[0026] Example 1 A method for preparing a PEGylated bio-antifouling substrate comprises the following steps: S1. calcining a glass substrate at 400° C. for 3 h to remove organic impurities on the surface, then washing with ultrapure water, and then performing a hydroxylation treatment. The hydroxylation treatment process is as follows: placing the glass substrate after washing with ultrapure water into a mixed solution of sodium hydroxide: water: isopropanol in a mass ratio of 3:18:21, ultrasonicating for 30 min, then washing with deionized water for 3 times, then washing with ethanol, and drying with nitrogen after washing to obtain a hydroxylated glass substrate; S2, adding acid to 100 parts of 90% ethanol aqueous solution to adjust the pH value to 2, then adding and mixing with 15 parts of silylated polymethacrylate oligoethylene glycol ester solution to obtain a mixed solution; then placing the hydroxylated glass substrate into the mixed solution, reacting at 60° C. in a water bath for 8 hours, and finally dehydrating at 90° C. for 4 hours to obtain a PEGylated biofouling substrate; the preparation method of the silylated polymethacrylate oligoethylene glycol ester solution comprises the following steps: S31. After uniformly mixing 3.5 parts of a silane coupling agent (the silane coupling agent is composed of 3-aminopropyltriethoxysilane, γ-chloropropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane in a mass ratio of 3:4:3), 3.1 parts of triethylamine and 42 parts of dichloromethane in parts by mass, the mixture is cooled to -5°C in an ice bath under nitrogen protection, and then 3 parts of α-bromoisobutyryl bromide are slowly added thereto to carry out an amidation reaction for 6 hours. The product is vacuum dried at 50°C for 8 hours and vacuum dried at 48°C to obtain a silylation initiator. S32. According to their mass fractions, 95 parts of methacrylate oligomer, 4.8 parts of catalyst (the catalyst is composed of cuprous bromide and 2,2-bipyridine in a mass fraction ratio of 1:3) and 400 parts of isopropanol are heated to 40°C under nitrogen protection, and then 3.8 parts of silylation initiator are added thereto to carry out atom transfer radical polymerization reaction for 16 hours to obtain a silylated polymethacrylate oligomer solution.
[0027] Example 2 A method for preparing a PEGylated bio-antifouling substrate comprises the following steps: S1. calcining a glass substrate at 500° C. for 3 h to remove organic impurities on the surface, then washing with ultrapure water, and then performing a hydroxylation treatment. The hydroxylation treatment process is as follows: placing the glass substrate after washing with ultrapure water into a mixed solution of sodium hydroxide: water: isopropanol in a mass ratio of 4:18:21, ultrasonicating for 40 min, then washing with deionized water for 3 times, then washing with ethanol, and drying with nitrogen after washing to obtain a hydroxylated glass substrate; S2, adding acid to 100 parts of 90% ethanol aqueous solution to adjust the pH value to 3, then adding and mixing with 15 parts of silylated polymethacrylate oligoethylene glycol ester solution to obtain a mixed solution; then placing the hydroxylated glass substrate into the mixed solution, reacting at 80° C. in a water bath for 6 hours, and finally dehydrating at 100° C. for 3 hours to obtain a PEGylated biofouling substrate; the preparation method of the silylated polymethacrylate oligoethylene glycol ester solution comprises the following steps: S31. After uniformly mixing 3.5 parts of a silane coupling agent (the silane coupling agent is composed of 3-aminopropyltriethoxysilane, γ-chloropropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane in a mass ratio of 3:4:3), 3.1 parts of triethylamine and 48 parts of dichloromethane in parts by mass, the mixture is cooled to 0° C. in an ice bath under nitrogen protection, and then 3 parts of α-bromoisobutyryl bromide are slowly added thereto to carry out an amidation reaction for 8 hours. The product is vacuum dried at 50° C. for 8 hours and vacuum dried at 48° C. to obtain a silylation initiator. S32. According to their mass fractions, 95 parts of methacrylate oligomer, 4.8 parts of catalyst (the catalyst is composed of cuprous bromide and 2,2-bipyridine in a mass fraction ratio of 1:3) and 450 parts of isopropanol are heated to 50°C under nitrogen protection, and then 3.8 parts of silylation initiator are added thereto to carry out atom transfer radical polymerization reaction for 12 hours to obtain a silylated polymethacrylate oligomer solution.
[0028] Example 3 A method for preparing a PEGylated bio-antifouling substrate comprises the following steps: S1. calcining the glass substrate at 450° C. for 2.5 h to remove organic impurities on the surface, then washing with ultrapure water, and then performing a hydroxylation treatment. The process of the hydroxylation treatment is as follows: placing the glass substrate after washing with ultrapure water into a mixed solution of sodium hydroxide: water: isopropanol in a mass ratio of 3.5:18:21, ultrasonicating for 35 min, then washing with deionized water for 3 times, then washing with ethanol, and drying with nitrogen after washing to obtain a hydroxylated glass substrate; S2, adding acid to 100 parts of 90% ethanol aqueous solution to adjust the pH value to 2.5, then adding and mixing with 15 parts of silylated polymethacrylate oligoethylene glycol ester solution to obtain a mixed solution; then placing the hydroxylated glass substrate into the mixed solution, reacting at 70° C. in a water bath for 7 hours, and finally dehydrating at 950° C. for 3.5 hours to obtain a PEGylated biofouling substrate; the preparation method of the silylated polymethacrylate oligoethylene glycol ester solution comprises the following steps: S31. After uniformly mixing 3.5 parts of a silane coupling agent (the silane coupling agent is composed of 3-aminopropyltriethoxysilane, γ-chloropropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane in a mass ratio of 3:4:3), 3.1 parts of triethylamine and 45 parts of dichloromethane in parts by mass, the mixture is cooled to -3°C in an ice bath under nitrogen protection, and then 3 parts of α-bromoisobutyryl bromide are slowly added thereto to carry out an amidation reaction for 7 hours. The product is vacuum dried at 50°C for 9 hours and vacuum dried at 48°C to obtain a silylation initiator. S32. According to their mass fractions, 95 parts of methacrylate oligomer, 4.8 parts of catalyst (the catalyst is composed of cuprous bromide and 2,2-bipyridine in a mass fraction ratio of 1:3) and 430 parts of isopropanol are heated to 45°C under nitrogen protection, and then 3.8 parts of silylation initiator are added thereto to carry out atom transfer radical polymerization reaction for 13 hours to obtain a silylated polymethacrylate oligomer solution.
[0029] Comparative Example 1 The same as Example 3, except that: the silane coupling agent is 3-aminopropyltriethoxysilane.
[0030] Comparative Example 2 The same as Example 3, except that: the silane coupling agent is γ-chloropropyltriethoxysilane.
[0031] Comparative Example 3 The same as Example 3, except that: the silane coupling agent is N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane.
[0032] Performance testing 1. The PEGylated bio-antifouling substrates prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were sampled and contact angles were tested. The test results are shown in Table 1. Contact angle: A contact angle tester (Kruss DSA100, Germany) was used at room temperature and a humidity of 85%. Ultrapure water was used as the test liquid. Three points on each substrate were measured in parallel and the average value was taken.
[0033] Table 1 Performance test project Contact angle / ° Example 1 20.6 Example 2 20.9 Example 3 20.2 Comparative Example 1 25.7 Comparative Example 2 25.3 Comparative Example 3 24.9 Analyzing the data in Table 1, we can see that: 1) The contact angles of the PEGylated bio-antifouling substrates prepared in Examples 1 to 3 were between 20.2 and 20.9, showing excellent hydrophilicity.
[0034] 2) The performance comparison analysis of the PEGylated biofouling substrates prepared in combination with Example 3 and Comparative Examples 1-3 shows that the silane coupling agent is composed of 3-aminopropyl triethoxysilane, γ-chloropropyl triethoxysilane and N-β-(aminoethyl)-γ-aminopropyl methyl dimethoxysilane in a mass ratio of 3:4:3. By utilizing the synergistic effect between them, the different functional groups of these silane coupling agents can react with the glass surface and the PEG chain segment in a complementary manner to form a multi-directional cross-linked network structure, thereby improving the hydrophilicity, stability and functionality of the PEGylated biofouling substrate. Through this synergistic effect, a more uniform and stable PEG covering layer can be achieved, thereby effectively improving the anti-protein adsorption performance and biocompatibility of the substrate.
[0035] 2. Fibrin adsorption test The PEGylated bio-antifouling substrate prepared in Example 3 and the hydroxylated glass substrate prepared in Example 3 were placed in a 1 mg / ml fibrin PBS buffer solution, then washed with deionized water for 30 seconds, and finally dried with nitrogen. XPS was used to quantitatively analyze the adsorbed fibrin on the above samples and the PEGylated bio-antifouling substrate prepared in Example 3 (the sample before being immersed in the fibrin PBS buffer solution); Stability test: The PEGylated biofouling substrate prepared in Example 3 was placed in a 1 mg / ml fibrin PBS buffer solution at 37°C for 28 days, then washed with deionized water for 30 seconds, and finally dried with nitrogen. The adsorbed fibrin was quantitatively analyzed using XPS.
[0036] The above results are Figure 1 As shown, from Figure 1 It can be seen that lines b and c show the N1S signals of the PEGylated bio-antifouling substrate before and after the adsorption of fibrin. Through comparative analysis, it can be found that basically no protein molecules are adsorbed on the PEGylated bio-antifouling substrate. Line d shows the N1S signal of the PEGylated bio-antifouling substrate monolayer after adsorption of fibrin after being placed in a fibrin PBS buffer solution with a concentration of 1 mg / ml for 28 days. Similarly, no adsorbed fibrin molecules were found. This shows that even after being immersed in a 1 mg / ml fibrin PBS buffer solution for 28 days, the PEGylated bio-antifouling substrate did not show obvious degradation, showing the good biocompatibility and stability of the PEGylated bio-antifouling substrate.
[0037] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a PEGylated bio-antifouling substrate, It is characterized in that The following steps are involved: S1, calcining the glass substrate at 400-500° C. for 2-3 hours to remove organic impurities on the surface, then washing with ultrapure water, and then performing hydroxylation treatment to obtain a hydroxylated glass substrate; S2. After adjusting the pH value to 2-3 by adding acid to 100 parts of 90% ethanol aqueous solution, add and mix evenly with 15 parts of silylated polymethacrylate oligoethylene glycol ester solution to obtain a mixed solution; then put the hydroxylated glass substrate into the mixed solution, react at 60-80°C in a water bath for 6-8 hours, and finally dehydrate at 90°C-100°C for 3-4 hours to obtain a PEGylated biofouling substrate.
2. A method for preparing a PEGylated bio-antifouling substrate according to claim 1, It is characterized in that In step S1, the hydroxylation process is as follows: the glass substrate washed with ultrapure water is placed in a mixture of sodium hydroxide: water: isopropanol in a mass ratio of 3-4:18:21, ultrasonicated for 30-40 minutes, then washed with deionized water for 3 times, then washed with ethanol, and dried with nitrogen after washing.
3. A method for preparing a PEGylated bio-antifouling substrate according to claim 1, It is characterized in that In step S2, the method for preparing the silylated poly(ethylene glycol) methacrylate solution comprises the following steps: S31, after uniformly mixing the silane coupling agent, triethylamine and dichloromethane according to their mass fractions, cool the mixture to -5 to 0°C in an ice bath under nitrogen protection, and then slowly add the initiator thereto to carry out an amidation reaction for 6-8h, and vacuum dry the product at 50°C for 8-10h, and vacuum dry it at 48°C to obtain a silylation initiator; S32. According to the mass fractions, methacrylate oligoethylene glycol ester, catalyst and isopropanol are heated to 40-50° C. under nitrogen protection, and then a silylation initiator is added thereto to carry out an atom transfer radical polymerization reaction for 12-16 hours to obtain a silylated polymethacrylate oligoethylene glycol ester solution.
4. A method for preparing a PEGylated bio-antifouling substrate according to claim 3, It is characterized in that The mass ratio of the silane coupling agent, triethylamine, dichloromethane and initiator is 3.5:3.1:(42-48):
3.
5. A method for preparing a PEGylated bio-antifouling substrate according to claim 3, It is characterized in that The silane coupling agent is composed of 3-aminopropyltriethoxysilane, γ-chloropropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane in a mass ratio of 3:4:
3.
6. A method for preparing a PEGylated bio-antifouling substrate according to claim 3, It is characterized in that The initiator is α-bromoisobutyryl bromide.
7. A method for preparing a PEGylated bio-antifouling substrate according to claim 3, It is characterized in that The mass ratio of the methacrylate oligoethylene glycol ester, the catalyst, isopropanol and the silylation initiator is 95:4.8:(400-450):3.
8.
8. A method for preparing a PEGylated bio-antifouling substrate according to claim 3, It is characterized in that The catalyst is composed of cuprous bromide and 2,2-bipyridine in a mass ratio of 1:
3.
9. A PEGylated bio-antifouling substrate, It is characterized in that The PEGylated bio-antifouling substrate is prepared by the preparation method of the PEGylated bio-antifouling substrate according to any one of claims 1-8.
10. Use of the PEGylated bio-antifouling substrate as claimed in claim 9 in drug carriers, protein detection chips, bio-MEMS and biosensors.
Citation Information
Patent Citations
Electronic grade glass fiber cloth surface conditioning agent and silane coupling agent preparation method
CN103911861A
Preparation method of three-dimensional biological chip substrate
CN104761745A
Far-infrared reflecting film, liquid dispersion for forming the far-infrared reflecting film, method for manufacturing the far-infrared reflecting film, far-infrared reflecting glass, and window
CN107209303A
Application of dihydroxy amino propyl silane coupling agent in glass surface modification
CN116217091A