Asphalt anti-stripping agent as well as preparation method and application thereof
By using asphalt anti-flaking agents with components such as tailings powder, lime powder, fatty alcohol polyoxyethylene ether phosphate and organosilane, the problems of poor thermal stability and insufficient adhesion of asphalt anti-flaking agents in the prior art are solved, which significantly increases the problem of asphalt anti-flaking agents. The water stability and road performance of iron tailings asphalt mixture are improved, and the requirements of highway construction specifications are met.
Patent Information
- Application Number
- CN202310652488.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-05
AI Technical Summary
The existing asphalt anti-flaking agent has poor thermal stability and is difficult to significantly improve the adhesion between iron tailings aggregate and asphalt, resulting in water damage problems on the road surface.
Using an asphalt anti-flaking agent including tailings powder, lime powder, fatty alcohol polyoxyethylene ether phosphate, organosilane and composite modifier, the adhesion between asphalt and aggregate is enhanced by the combination of modifiers and enhanced Water stability of the mixture.
It significantly improves the water stability, thermal stability and low-temperature crack resistance of iron tailings asphalt mixture, meets the use indicators of the technical specifications for road asphalt pavement construction, and promotes the comprehensive utilization of tailings solid waste.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the field of asphalt additives, and in particular to an asphalt anti-stripping agent and a preparation method and application thereof. Background Art
[0002] Iron tailings are the part of iron ore with low content of valuable elements produced during the processing and utilization of iron ore. They are one of the important components of solid waste in mines and are also a valuable secondary resource. The world's iron tailings are mainly distributed in China, Brazil, Australia and other places. According to statistics, the annual cumulative increase in tailings in the world can reach 5 billion to 7 billion tons, and iron tailings account for about 1 / 2. At present, the stockpile of iron tailings in China and Brazil alone has exceeded 10 billion tons.
[0003] The chemical composition of iron tailings is mainly composed of oxides of silicon, aluminum, iron, calcium and magnesium, and the main minerals are mainly quartz and feldspar minerals, which are very close to the mineral composition of natural sand, which provides the necessary basis for iron tailings to become raw materials for building materials. New building materials are building materials with improved performance, improved or increased functions based on traditional building materials. They are characterized by high strength, light weight, energy saving and low environmental pollution. The application of iron tailings in the field of new building materials meets the dual needs of environmental and economic development.
[0004] Compared with conventional aggregates, the physical and mechanical properties of iron tailings aggregates meet the requirements of aggregate specifications. However, iron tailings are high-silicon stones with poor adhesion to asphalt, which can easily lead to loose, rough, pothole-like, pumping and other water damage on the road surface. The key to water damage is the insufficient adhesion between asphalt and aggregate, which causes the asphalt film to fall off the aggregate surface. Therefore, in order to use tailings aggregates and prevent the occurrence of water damage, it is crucial to improve the adhesion between asphalt and aggregate. The simplest and most effective way is to add an anti-stripping agent. However, at present, there is no anti-stripping agent specifically for tailings aggregates, and the commonly used anti-stripping agents are mostly amine compounds, which act directly on asphalt, have poor thermal stability, and easily lead to performance failure.
[0005] CN102174264A discloses a method for preparing a road asphalt anti-stripping agent and a preparation method thereof. The anti-stripping agent comprises the following components: 50-65 parts of polyethylene glycol; 10-30 parts of alkoxy aliphatic polyamines; 5-15 parts of alkylamines; 5-15 parts of polyamines; 1-2 parts of alcohol ether compounds; and 13-29 parts of diethanolamine. However, aliphatic amine anti-stripping agents have poor thermal stability and are mainly based on physical adsorption, which limits the use of amine anti-stripping agents.
[0006] CN108623207A discloses an asphalt anti-stripping agent containing phosphate salt and a method for using the same. The anti-stripping agent is composed of sodium dodecyl phosphate and octadecyl trimethyl ammonium chloride. When used, the anti-stripping agent needs to be evenly mixed with hot asphalt, but the aggregate is not modified. When the amount added is small, uneven dispersion is likely to result in limited anti-stripping effect.
[0007] In summary, developing an asphalt anti-stripping agent with good thermal stability and significantly improved adhesion to comprehensively utilize iron ore solid waste has important social and economic significance. Summary of the invention
[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an asphalt anti-stripping agent and its preparation method and application. The asphalt anti-stripping agent of the present invention can improve the adhesion between tailings aggregate and asphalt and improve the water stability of tailings asphalt mixture.
[0009] The first aspect of the present invention provides an asphalt anti-stripping agent, which comprises the following components in parts by weight:
[0010] Tailings powder: 100 parts;
[0011] Lime powder: 50-70 parts, preferably 55-70 parts;
[0012] Fatty alcohol polyoxyethylene ether phosphate: 3 to 15 parts, preferably 5 to 10 parts;
[0013] Organosilane: 2 to 8 parts, preferably 2 to 5 parts;
[0014] Composite modifier: 15 to 50 parts, preferably 20 to 40 parts.
[0015] The chemical composition of the tailings powder includes 55% to 60% SiO2, 10% to 18% Fe2O3, 10% to 15% Al2O3, and 6% to 13% CaO based on the mass of the tailings powder. The particle size of the tailings powder meets the following requirements: the passing rate of the standard square sieve of <0.075mm is 85% to 100%. The tailings powder is generally iron tailings powder after magnetic separation in the mining area.
[0016] The lime powder is industrial grade slaked lime powder, wherein Ca(OH)2>90wt% and the particle size is 80-500 meshes.
[0017] The fatty alcohol polyoxyethylene ether phosphate AEO-P has a general formula of RO(CH2CH2O)nPO3H2, where n is an integer of 3 to 9. The fatty alcohol ROH used in synthesizing the fatty alcohol polyoxyethylene ether phosphate is a normal fatty alcohol and / or an isomeric fatty alcohol selected from C8-18 alcohols, preferably one or more of isooctyl alcohol, lauryl alcohol, isomeric decanol, and cetyl alcohol.
[0018] The organosilane is a mixture of aminosilane and long-chain organosilane, wherein the aminosilane accounts for 30% to 50% of the total mass of the organosilane, and the long-chain organosilane accounts for 50% to 70% of the total mass of the organosilane.
[0019] The aminosilane is one or more of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane, N-[[[2-(trimethoxysilyl)ethyl]phenyl]methyl]-1,2-ethylenediamine, N-(6-aminohexyl)aminomethyltriethoxysilane, 3-(4-ureaamino)propyltriethoxysilane, and N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.
[0020] The long-chain organic silane is one or more of dodecyltrimethoxysilane, dodecyltriethoxysilane, dodecylmethyldimethoxysilane, hexadecyltrimethoxysilane and octadecyltrimethoxysilane.
[0021] The composite modifier comprises the following components by weight:
[0022] Nano silicon dioxide: 100 parts;
[0023] 3-glycidyloxypropylmethyldiethoxysilane (GPTMS): 3 to 8 parts, preferably 3 to 6 parts;
[0024] Polyethyleneimine (PEI): 3 to 10 parts, preferably 5 to 8 parts.
[0025] The nano silicon dioxide and 3-glycidyloxypropylmethyldiethoxysilane are both commercially available products.
[0026] The molecular weight of the polyethyleneimine is 1000-70000, preferably one or more of 1000, 20000 and 70000.
[0027] The second aspect of the present invention provides a method for preparing the above-mentioned asphalt anti-stripping agent, comprising:
[0028] (1) uniformly mixing fatty alcohol polyoxyethylene ether phosphate and organosilane to prepare a prefabricated mixed solution;
[0029] (2) preparing a composite modifier;
[0030] (3) mixing the tailings powder, lime powder and composite modifier uniformly to obtain a prefabricated mixed powder;
[0031] (4) The prefabricated mixed liquid obtained in step (1) is evenly sprayed on the prefabricated mixed powder obtained in step (3), and dried to obtain an asphalt anti-stripping agent.
[0032] In step (1), the fatty alcohol polyoxyethylene ether phosphate can be prepared by the following method: under nitrogen protection, first add 3 parts by weight of fatty alcohol polyoxyethylene ether AEO, preferably add 1 part by weight of P2O5 in batches while stirring, heat up and continue stirring, add and hydrolyze to obtain fatty alcohol polyoxyethylene ether phosphate. Wherein, the heating temperature is 80-90°C, the stirring time after heating is 3-6h, the hydrolysis temperature is consistent with the reaction temperature, the hydrolysis time is 1.5-3h, and the amount of water added is 3%-7% of the total product.
[0033] In step (1), the mixing temperature of the fatty alcohol polyoxyethylene ether phosphate and the organosilane is 45-65°C.
[0034] In step (2), the preparation process of the composite modifier is as follows:
[0035] Nano-silica and 3-glycidyloxypropylmethyldiethoxysilane (GPTMS) are mixed in anhydrous ethanol, reacted under a first heating reflux condition, polyethyleneimine (PEI) is added after the reaction is completed, reacted under a second heating reflux condition, filtered, washed and dried after cooling to obtain a composite modifier.
[0036] The first heating reflux reaction temperature is 90° C. to 130° C., preferably 100° C. to 115° C., and the reaction time is 12 to 18 hours.
[0037] The reaction temperature of the second heating reflux is 90° C. to 120° C., preferably 100° C. to 110° C., and the reaction time is 20 to 24 hours.
[0038] The first reflux temperature is preferably 3-10° C. higher than the second reflux temperature.
[0039] The filtering and washing can be performed in a conventional manner in the art.
[0040] The drying temperature is 80° C. to 120° C., and the drying time is 0.5 to 5 hours, preferably 3 to 5 hours.
[0041] The tailings powder in step (3) is obtained by drying and grinding the iron tailings slag, wherein the grinding to <0.075mm has a passing rate of 85-100%.
[0042] The iron tailings slag is dried at a temperature of 90 to 110° C. and for a drying time of 3 to 5 hours.
[0043] The drying temperature in step (4) is 100-105° C., and the drying time is 2-5 hours.
[0044] The third aspect of the present invention discloses a use of the above-mentioned asphalt anti-stripping agent in asphalt mixture.
[0045] The asphalt mixture is tailings aggregate asphalt mixture.
[0046] The application includes: adding the asphalt anti-stripping agent into the mineral powder of tailings aggregate asphalt mixture, wherein the amount of the asphalt anti-stripping agent added accounts for more than 80wt% of the mineral powder mass, preferably 80wt% to 90wt%, the coarse aggregate and fine aggregate in the tailings aggregate asphalt mixture are both iron ore waste rock, and the mineral powder is iron tailings powder after magnetic separation.
[0047] Compared with the prior art, the present invention has the following characteristics:
[0048] (1) The asphalt anti-stripping agent of the present invention plays multiple roles. The addition of slaked lime powder components, due to its strong alkalinity and high chemical adsorption energy, can not only improve the acidic environment on the aggregate surface, but also has a larger specific surface area and more sufficient asphalt adsorption. The fatty alcohol polyoxyethylene ether phosphate has different functional groups at both ends. One end undergoes hydrogen bond adsorption with the hydroxyl group on the aggregate surface, and the other end is entangled and cross-linked with the asphalt polymer, so that the overall adhesion of the asphalt mixture is enhanced. The aminosilane and long-chain organosilane in the organosilane cooperate synergistically to improve the connection ability of the acidic stone and the matrix asphalt, and enhance the adhesion of the asphalt to the aggregate.
[0049] (2) The composite modifier in the present invention is a modified nano-silica, which can not only be closely adsorbed and bonded with the aggregate, but the branched active groups introduced by the modification can also react with the hydroxyl group, carboxyl group, unsaturated bond, etc. in the asphalt, closely combining the asphalt and aggregate interface, thereby improving the anti-stripping performance of the asphalt mixture.
[0050] (3) The tailings asphalt mixture obtained by using the asphalt anti-stripping agent of the present invention not only significantly enhances the water stability, but also improves the high temperature stability and low temperature crack resistance, comprehensively improves the road performance of the mixture, and all road performances meet the road pavement usage index requirements in the "Technical Specifications for Highway Asphalt Pavement Construction" (JTG F40-2004), promotes the comprehensive utilization of tailings solid waste, and also provides a good foundation for the subsequent application of tailings asphalt mixture. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by way of examples, but these examples cannot limit the protection scope of the present invention, and the wt % involved is the mass fraction.
[0052] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, were purchased from conventional biochemical reagent stores.
[0053] The preparation method of the fatty alcohol polyoxyethylene ether phosphate used in the embodiments and comparative examples is as follows: under nitrogen protection, first add 3 parts by weight of fatty alcohol polyoxyethylene ether AEO (the fatty alcohol used to synthesize fatty alcohol polyoxyethylene ether is isooctyl alcohol, and n is 6), add 1 part by weight of P2O5 in batches while stirring, increase the temperature and continue stirring, and obtain fatty alcohol polyoxyethylene ether phosphate after hydrolysis, wherein the P2O5 batch addition time is 2h, the heating temperature is 80°C, the stirring time is 4h, the hydrolysis temperature is consistent with the reaction temperature, the hydrolysis time is 2h, and the amount of water added for hydrolysis is 4% of the total mass of the added material.
[0054] The tailings powder used in the embodiments and comparative examples has a chemical composition, based on the mass of the tailings powder, of 58% SiO2, 17% Fe2O3, 13% Al2O3, and 12% CaO.
[0055] The lime powder is industrial grade slaked lime powder, wherein the Ca(OH)2 content is 96.4wt% and the particle size is 120 meshes.
[0056] Example 1
[0057] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of a mixture of organosilane (N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane (wherein dodecyltrimethoxysilane accounts for 60 wt%) are mixed and stirred at 50° C. to obtain a prefabricated mixed solution.
[0058] (2) 100 parts of nano-silica and 5 parts of 3-glycidyloxypropylmethyldiethoxysilane (GPTMS) were mixed in anhydrous ethanol, heated under reflux at 110°C for 12 hours, and after the reaction, 6 parts of polyethyleneimine PEI with a molecular weight of 20,000 were added, and heated under reflux at 100°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain a composite modifier for use.
[0059] (3) Dry the iron tailings and grind them to a particle size of <0.075 mm with a passing rate of 90%. Mix 100 parts of tailings powder, 55 parts of lime powder, and 20 parts of a composite modifier to obtain a prefabricated mixed powder.
[0060] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 105° C. for 4 h to obtain asphalt anti-stripping agent A1.
[0061] Example 2
[0062] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 4 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane, wherein dodecyltrimethoxysilane accounts for 60 wt %) are mixed and stirred at 55° C. to obtain a prefabricated mixed solution.
[0063] (2) 100 parts of nano-silica and 5 parts of GPTMS were mixed in anhydrous ethanol, heated under reflux at 110°C for 12 hours, and after the reaction, 6 parts of PEI with a molecular weight of 20,000 were added, and heated under reflux at 100°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain a composite modifier for use.
[0064] (3) Dry the iron tailings and grind them to a particle size of <0.075 mm with a passing rate of 92%. Mix 100 parts of tailings powder, 55 parts of lime powder, and 25 parts of a composite modifier to obtain a prefabricated mixed powder.
[0065] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder and dried at 102°C for 5 h to obtain asphalt anti-stripping agent A2.
[0066] Example 3
[0067] (1) 8 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and hexadecyltrimethoxysilane, wherein the hexadecyltrimethoxysilane accounts for 70 wt %) are mixed and stirred at 55° C. to obtain a prefabricated mixed solution.
[0068] (2) 100 parts of nano-silica and 6 parts of GPTMS were mixed in anhydrous ethanol, heated under reflux at 110°C for 12 hours, and after the reaction, 7 parts of PEI with a molecular weight of 20,000 were added, and heated under reflux at 100°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain a composite modifier for use.
[0069] (3) Dry the iron tailings and grind them to a particle size of <0.075 mm with a passing rate of 90%. Mix 100 parts of tailings powder, 60 parts of lime powder, and 20 parts of a composite modifier to obtain a prefabricated mixed powder.
[0070] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder and dried at 105°C for 4 hours to obtain asphalt anti-stripping agent A3.
[0071] Example 4
[0072] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane, wherein dodecyltrimethoxysilane accounts for 60 wt %) are mixed and stirred at 60° C. to obtain a prefabricated mixed solution.
[0073] (2) 100 parts of nano-silica and 5 parts of GPTMS were mixed in anhydrous ethanol, heated under reflux at 110°C for 16 hours, and after the reaction, 3 parts of PEI with a molecular weight of 20,000 and 4 parts of PEI with a molecular weight of 70,000 were added, and heated under reflux at 105°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain a composite modifier for use.
[0074] (3) Dry the iron tailings and grind them to a particle size of <0.075 mm with a passing rate of 90%. Mix 100 parts of tailings powder, 55 parts of lime powder, and 20 parts of a composite modifier to obtain a prefabricated mixed powder.
[0075] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 105° C. for 4 h to obtain asphalt anti-stripping agent A4.
[0076] Example 5
[0077] (1) 6 parts of fatty alcohol polyoxyethylene ether phosphate and 3 parts of organosilane (a mixture of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane, wherein dodecyltrimethoxysilane accounts for 60 wt %) are mixed and stirred at 55° C. to obtain a prefabricated mixed solution.
[0078] (2) 100 parts of nano-silica and 5 parts of GPTMS were mixed in anhydrous ethanol, heated under reflux at 110°C for 16 hours, and after the reaction, 2 parts of PEI with a molecular weight of 20,000, 3 parts of PEI with a molecular weight of 70,000, and 2 parts of PEI with a molecular weight of 1,000 were added, and heated under reflux at 105°C for 24 hours. After the reaction, the mixture was filtered, washed, and dried at 100°C for 5 hours to obtain a composite modifier for use.
[0079] (3) Dry the iron tailings and grind them to a particle size of <0.075 mm with a passing rate of 95%. Mix 100 parts of tailings powder, 55 parts of lime powder, and 20 parts of a composite modifier to obtain a prefabricated mixed powder.
[0080] (4) The prefabricated mixed liquid was evenly sprayed on the prefabricated mixed powder, and dried at 105° C. for 4 h to obtain asphalt anti-stripping agent A5.
[0081] Comparative Example 1
[0082] The same as Example 1, except that lime powder is not added during the preparation process, to obtain asphalt mixture anti-stripping agent B1.
[0083] Comparative Example 2
[0084] The same as Example 1, except that nano silicon dioxide is directly used in place of modified nano silicon dioxide during the preparation process to obtain asphalt mixture anti-stripping agent B2.
[0085] Comparative Example 3
[0086] The same as Example 1, except that the preparation method of the modified nano-silica in the preparation process is as follows: 6 parts of the bionic material methacrylamide dopamine and 100 parts of nano-silica ethanol dispersion are mixed and stirred evenly for 5 minutes to obtain a mixture. After the reaction is completed, the mixture is filtered, washed, and dried at 100°C for 5 hours to obtain a modified nano-silica composite modifier for use, and finally an exfoliating agent B3 is obtained.
[0087] Comparative Example 4
[0088] The same as Example 1, except that the mixture of organic silane (N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane and dodecyltrimethoxysilane) was not added during the preparation process, to obtain asphalt mixture anti-stripping agent B4.
[0089] Comparative Example 5
[0090] The same as Example 1, except that no fatty alcohol polyoxyethylene ether phosphate was added during the preparation process, to obtain asphalt mixture anti-stripping agent B5.
[0091] Comparative Example 6
[0092] The same as Example 1, except that vinyl triethoxysilane is used instead of fatty alcohol polyoxyethylene ether phosphate in the preparation process to obtain anti-stripping agent B6.
[0093] According to the method of use, the asphalt anti-stripping agent of Examples 1 to 5 and Comparative Examples 1 to 6 was added to the mineral powder of the iron tailings aggregate asphalt mixture at an amount of 80wt% (accounting for 80wt% of the mineral powder mass), and then the asphalt mixture was prepared. The coarse aggregate and fine aggregate in the iron tailings aggregate asphalt mixture are both iron ore waste rock, the mineral powder is iron tailings powder, the matrix asphalt is Qilu 70A asphalt, and the asphalt mixture grading type is AC-20. The road performance of the asphalt mixture was evaluated.
[0094] The road performance of asphalt mixture was tested in accordance with the (JTG E20-2011) "Test Procedure for Asphalt and Asphalt Mixture in Highway Engineering". The water stability was investigated by the water residual stability MS0 of the immersion Marshall test (T 0709-2011) and the freeze-thaw splitting strength ratio TSR of the freeze-thaw splitting test (T0729-2000). The high temperature stability was investigated by the dynamic stability of the rutting test (T0719-2011). The low temperature crack resistance was investigated by the flexural tensile strength and maximum flexural tensile strain of the low temperature bending test (T0715-2011). The results are shown in Table 1.
[0095] Table 1 Performance of asphalt mixtures prepared in Examples 1 to 5 and Comparative Examples 1 to 6
[0096]
[0097] It can be seen from the results in Table 1 that the iron tailings asphalt mixture prepared by the asphalt anti-stripping agent prepared by the present invention has good water stability and high and low temperature performance, and various road performances meet the road pavement usage index requirements in (JTG F40-2004) "Technical Specifications for Highway Asphalt Pavement Construction".
Claims
1. An asphalt anti-stripping agent, characterized in that: By weight, it includes the following components: Tailings powder: 100 parts; Lime powder: 50-70 parts, preferably 55-70 parts; Fatty alcohol polyoxyethylene ether phosphate: 3 to 15 parts, preferably 5 to 10 parts; Organosilane: 2 to 8 parts, preferably 2 to 5 parts; Composite modifier: 15 to 50 parts, preferably 20 to 40 parts.
2. The asphalt anti-stripping agent according to claim 1, characterized in that Calculated by the mass of the tailings powder, the chemical composition of the tailings powder includes: 55% to 60% SiO2, 10% to 18% Fe2O3, 10% to 15% Al2O3, and 6% to 13% CaO.
3. The asphalt anti-stripping agent according to claim 1, characterized in that The fatty alcohol polyoxyethylene ether phosphate has the general formula RO(CH2CH2O)nPO3H2, where n is an integer of 3 to 9; wherein the fatty alcohol ROH used in synthesizing the fatty alcohol polyoxyethylene ether phosphate is a normal fatty alcohol and / or an isomeric fatty alcohol selected from C8-18 alcohol, preferably one or more of isooctyl alcohol, lauryl alcohol, isomeric decanol, and cetyl alcohol.
4. The asphalt anti-stripping agent according to claim 1, characterized in that: The organosilane is a mixture of aminosilane and long-chain organosilane, wherein the aminosilane accounts for 30% to 50% of the total mass of the organosilane, and the long-chain organosilane accounts for 50% to 70% of the total mass of the organosilane.
5. The asphalt anti-stripping agent according to claim 4, characterized in that: The aminosilane is one or more of N-(2-N-benzylaminoethyl)-3-aminopropyltrimethoxysilane, N-[[[2-(trimethoxysilyl)ethyl]phenyl]methyl]-1,2-ethylenediamine, N-(6-aminohexyl)aminomethyltriethoxysilane, 3-(4-ureaamino)propyltriethoxysilane, and N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane; and / or the long-chain organosilane is one or more of dodecyltrimethoxysilane, dodecyltriethoxysilane, dodecylmethyldimethoxysilane, hexadecyltrimethoxysilane, and octadecyltrimethoxysilane.
6. The asphalt anti-stripping agent according to claim 1, characterized in that: The composite modifier comprises the following components by weight: Nano silicon dioxide: 100 parts; 3-glycidyloxypropylmethyldiethoxysilane: 3 to 8 parts, preferably 3 to 6 parts; Polyethyleneimine: 3 to 10 parts, preferably 5 to 8 parts.
7. The method for preparing the asphalt anti-stripping agent according to any one of claims 1 to 6, comprising: (1) uniformly mixing fatty alcohol polyoxyethylene ether phosphate and organosilane to prepare a prefabricated mixed solution; (2) preparing a composite modifier; (3) mixing the tailings powder, lime powder and composite modifier uniformly to obtain a prefabricated mixed powder; (4) The prefabricated mixed liquid obtained in step (1) is evenly sprayed on the prefabricated mixed powder obtained in step (3), and dried to obtain an asphalt anti-stripping agent.
8. The preparation method according to claim 7, characterized in that: In step (1), the mixing temperature of the fatty alcohol polyoxyethylene ether phosphate and the organosilane is 45-65°C.
9. The preparation method according to claim 7, characterized in that: In step (2), the preparation process of the composite modifier is as follows: The nano-silicon dioxide and 3-glycidyloxypropylmethyldiethoxysilane are mixed in anhydrous ethanol, reacted under a first heating reflux condition, polyethyleneimine is added after the reaction is completed, reacted under a second heating reflux condition, filtered, washed and dried after cooling to obtain a composite modifier.
10. The preparation method according to claim 9, characterized in that: The reaction temperature of the first heating reflux is 90°C to 130°C, preferably 100°C to 115°C, and the time is 12 to 18 hours, and / or the reaction temperature of the second heating reflux is 90°C to 120°C, preferably 100°C to 110°C, and the time is 20 to 24 hours; preferably, the first reflux temperature is 3 to 10°C higher than the second reflux temperature.
11. The preparation method according to claim 7, characterized in that: The drying temperature in step (4) is 100-105° C., and the drying time is 2-5 hours.
12. Use of the asphalt anti-stripping agent according to any one of claims 1 to 6 or the asphalt prepared according to any one of claims 7 to 11 in asphalt mixture.
13. The use according to claim 12, characterized in that: The application includes: adding the asphalt anti-stripping agent into the mineral powder of tailings aggregate asphalt mixture, wherein the amount of the asphalt anti-stripping agent added accounts for more than 80wt% of the mineral powder mass, preferably 80wt% to 90wt%, the coarse aggregate and fine aggregate in the tailings aggregate asphalt mixture are both iron ore waste rock, and the mineral powder is iron tailings powder after magnetic separation.
Citation Information
Patent Citations
Aasphalt antistripping agent for pavement and preparation method thereof
CN102174264A
Phosphate-containing pitch anti-stripping agent and use method thereof
CN108623207A
Cationic pitch warm mixing agent and preparation method thereof
CN104559248A
Asphalt concrete used for highway engineering and preparation method of asphalt concrete
CN110342857A
Biomimetic material-containing asphalt anti-stripping agent and asphalt preparation method based on same
CN113652000A