Solid-waste-based low-carbon anti-cracking waterproof agent

By using sulfonated aramid fiber and cationic mullite fiber in waterproofing agents, the problem of insufficient crack resistance and anti-seepage performance of existing waterproofing agents in special environments is solved, and the early strength and anti-seepage performance of concrete are significantly improved. , extends service life.

CN119080430APending Publication Date: 2024-12-06JINHUA XINSHENG ZEOLITE DEV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411092727.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing waterproofing agents are difficult to meet the crack resistance and anti-seepage needs of concrete in special environments such as humid and rainy, and may affect the early strength of concrete, increase the risk of cracking, and affect durability.

Method used

The sulfonated aramid fiber and cationic mullite fiber are used as the main components, and the fiber structure with organic layer is formed through ultraviolet light and ultrasound technology, which enhances the strength and permeability of concrete and reduces the activation energy of hydration reaction. Improve the microstructure of hardened slurry and reduce the occurrence of microcracks.

Benefits of technology

It significantly improves the early strength and permeability of concrete, reduces the risk of cracking, extends the service life of concrete, and improves durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080430A_ABST
    Figure CN119080430A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of concrete admixtures, and discloses a solid-waste-based low-carbon anti-cracking waterproof agent, which is prepared from the following raw materials: sulfonated aramid fiber, cationic mullite fiber, fluorgypsum, blast furnace slag, aluminum slag powder, fly ash, calcium oxide, calcium sulphoaluminate, calcium formate and sodium methyl silicate. The sulfonated aramid fiber and the cationic mullite fiber are prepared and participate in the preparation process of the waterproof agent, so that the prepared waterproof agent can effectively improve the early strength of concrete without additionally adding a water reducing agent, and the anti-cracking performance and impermeability of the concrete are enhanced; the prepared concrete is high in strength and not prone to cracking and still has a good waterproof effect in a long-term humid and cloudy and rainy environment, the service life of the concrete is effectively prolonged, and the durability of the concrete is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete admixtures, in particular to a solid waste-based low-carbon anti-cracking waterproofing agent. Background Art

[0002] With the widespread use of concrete materials in construction projects, concrete leakage has become an important challenge facing the construction industry. There are pores of various shapes and sizes in concrete, including pores and capillaries. The presence of these pores increases the permeability of concrete, allowing water and gas to pass through the concrete more easily, which will reduce the strength of concrete, making it more likely to be damaged and cracked when bearing loads, affecting the service life of concrete.

[0003] Waterproofing agent is a widely used concrete admixture that can protect concrete structures from erosion and damage by moisture, improve the anti-seepage performance of concrete, and maintain its stability and durability. However, the current common waterproofing agents have average anti-cracking and anti-seepage capabilities, and are difficult to meet the requirements for concrete anti-seepage and anti-cracking in special environments such as humid and rainy environments. Therefore, people often make improvements on them when using them. For example, a patent with announcement number CN115160922B announces a high-penetration and anti-corrosion organosilicon waterproofing agent and its preparation method and application. The prepared organosilicon waterproofing agent has excellent permeability and can effectively penetrate into the concrete to form a protective layer on the surface of the steel bars to achieve both waterproof and anti-corrosion properties. However, the waterproofing agent prepared by this patent has average reinforcement effect. The addition of waterproofing agent may have an adverse effect on the early strength of concrete, resulting in an increased risk of concrete cracking, affecting the durability of concrete during actual use. Summary of the invention

[0004] The purpose of the present invention is to provide a solid waste-based low-carbon anti-cracking waterproofing agent, which solves the problem that the reinforcement, anti-cracking and anti-seepage performance of current waterproofing agents need to be improved.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A solid waste-based low-carbon anti-cracking waterproofing agent comprises the following raw materials in parts by weight: 6-8 parts of sulfonated aramid fiber, 8-12 parts of cationic mullite fiber, 35-50 parts of fluorinated gypsum, 20-35 parts of blast furnace slag, 8-18 parts of aluminum slag powder, 10-20 parts of fly ash, 8-15 parts of calcium oxide, 6-15 parts of calcium sulfoaluminate, 3-10 parts of calcium formate, and 6-12 parts of sodium methyl silicate.

[0007] Furthermore, the method for preparing the sulfonated aramid fiber comprises the following steps:

[0008] S1: immersing the aramid fiber in acetone, ultrasonically cleaning for 5-6 hours, filtering and drying, irradiating the aramid fiber under ultraviolet light for 8-10 minutes, collecting the product, and obtaining carboxylated aramid fiber;

[0009] S2: Take the composite catalyst and place it in anhydrous ethanol, add carboxylated aramid fiber, ultrasonically disperse for 8-10 minutes, then add p-aminobenzenesulfonic acid, react in a water bath at 60-65°C for 18-20 hours, wash, filter and vacuum dry to obtain sulfonated aramid fiber.

[0010] Through the above technical scheme, aramid fiber is irradiated with ultraviolet light to form carboxylated aramid fiber, and then the carboxyl group in the carboxylated aramid fiber structure reacts with the amino group in the p-aminobenzenesulfonic acid structure to obtain sulfonated aramid fiber. The sulfonated aramid fiber has an organic layer on its surface that can be evenly dispersed in a waterproofing agent. When the waterproofing agent is applied to concrete, its unique fiber structure can enhance the strength of the concrete, effectively disperse stress when the concrete is impacted or deformed, and maintain the integrity of the concrete structure. At the same time, the sulfonic acid group in its structure can reduce the activation energy of the hydration reaction, thereby accelerating the hydration rate, improving the microstructure of the concrete hardened slurry, relieving internal stress, improving the early strength of the concrete, and reducing the generation of microcracks, thereby improving the concrete's impermeability.

[0011] Furthermore, the UV intensity of the UV lamp in step S1 is 50-55 μW / cm 2 .

[0012] Furthermore, the composite catalyst in step S2 is dicyclohexylcarbodiimide and 4-dimethylaminopyridine in a mass ratio of 0.7-1:0.25-0.3.

[0013] Furthermore, the method for preparing the cationic mullite fiber comprises the following steps:

[0014] SS1: Place the silane coupling agent and mullite fiber in anhydrous ethanol, ultrasonically disperse for 15-20 minutes, add oxalic acid solution to adjust the pH to 4-5, heat to 70-75°C for reaction for 3-4 hours, filter, wash and dry to obtain amino-modified mullite fiber;

[0015] SS2: Place the aminated mullite fiber and sodium alginate in deionized water for ultrasonic dispersion for 20-30 minutes, let stand for 2-3 hours and then filter to collect the product to obtain modified mullite fiber;

[0016] SS3: The modified mullite fiber is fully mixed with a hydrochloric acid solution with a concentration of 1-2 mol / L, ultrasonically dispersed for 10-20 minutes, and then aniline is added. The mixture is fully stirred for 1-2 hours, and the initiator is added dropwise at a rate of 30-35 seconds per drop. The mixture is reacted in an ice bath at 0-4°C for 12-14 hours. After filtering, washing, and drying, the cationic mullite fiber is obtained.

[0017] Through the above technical scheme, a silane coupling agent is used to modify the mullite fiber to obtain an amino-modified mullite fiber, and then the positively charged amino groups on the surface of the mullite fiber interact with the negatively charged sodium alginate to form a negatively charged modified mullite fiber, and then aniline is in situ polymerized on the surface of the modified mullite fiber to obtain a cationic mullite fiber. The cationic mullite fiber is coated with an organic layer on the surface, which can be more evenly distributed in the waterproofing agent and is not easy to agglomerate; the sodium alginate coated on the surface has a hygroscopic effect, and produces a synergistic effect with the sulfonic acid group on the surface of the sulfonated aramid fiber, promoting the hydration of the concrete, so that it does not need to add an additional water reducer, and can effectively reduce the water-cement ratio of the concrete and improve the strength and durability of the concrete. At the same time, sodium alginate has good adhesion, which helps to fill and seal the tiny cracks and holes in the concrete structure, thereby reducing the possibility of water penetration and enhancing the concrete's impermeability. In actual use, the positively charged cationic mullite fiber interacts with the negatively charged sulfonated aramid fiber, approaches each other, produces an interwoven structure, and pulls each other to enhance the density of the concrete, effectively prevent concrete cracking, and improve the concrete's compressive strength and impermeability.

[0018] Furthermore, the mass fraction of the oxalic acid solution in step SS1 is 10%-12%.

[0019] Furthermore, the silane coupling agent described in step SS1 is any one of (3-aminopropyl)triethoxysilane, 3-(2-aminoethylamino)propylmethyldimethoxysilane, and [3-(6-aminohexylamino)propyl]trimethoxysilane.

[0020] Furthermore, the initiator described in step SS3 is an ammonium persulfate solution with a concentration of 0.1-0.2 mol / L.

[0021] Furthermore, the preparation method of the solid waste-based low-carbon anti-cracking waterproofing agent comprises the following steps:

[0022] Step 1: mixing fluorinated gypsum, blast furnace slag, aluminum slag powder, fly ash, calcium oxide, calcium sulfoaluminate, calcium formate, and sodium methyl silicate to obtain a mixture;

[0023] Step 2: placing sulfonated aramid fiber and cationic mullite fiber into a mixture, and stirring and mixing them thoroughly to obtain a waterproofing agent.

[0024] Beneficial effects of the present invention:

[0025] The present invention prepares sulfonated aramid fiber and cationic mullite fiber, and participates in the preparation process of the waterproofing agent, so that the prepared waterproofing agent can effectively improve the early strength of concrete, enhance the anti-cracking performance and anti-seepage ability of concrete, make the prepared concrete high in strength and not easy to crack, effectively improve the service life of concrete, and make it have excellent durability.

[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0028] Figure 1 1 is the zeta potential diagram of the amino-modified mullite fiber, the modified mullite fiber, and the cationic mullite fiber in the embodiments of the present invention. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] 1. Preparation of sulfonated aramid fiber

[0032] S1: 2.6 g of aramid fiber was immersed in 80 ml of acetone, and then ultrasonically cleaned for 5 h, filtered, and dried. 2 Irradiate under ultraviolet light for 8 minutes, collect the product, and obtain carboxylated aramid fiber;

[0033] S2: Take 0.7g of dicyclohexylcarbodiimide and 0.25g of 4-dimethylaminopyridine and place them in 100mL of anhydrous ethanol, add 3.2g of carboxylated aramid fiber, ultrasonically disperse for 8min, then add 3.8g of p-aminobenzenesulfonic acid, react in a 60℃ water bath for 18h, wash, filter and vacuum dry to obtain sulfonated aramid fiber.

[0034] The sulfur element in carboxylated aramid fiber and sulfonated aramid fiber was analyzed using a Thermo element analyzer. The carboxylated aramid fiber did not contain sulfur element, while the sulfur content in sulfonated aramid fiber was 3.5%. The appearance of sulfur element was due to the reaction between the carboxyl group in the carboxylated aramid fiber structure and the amino group in the p-aminobenzenesulfonic acid structure, which grafted the sulfonic acid group onto the surface of the aramid fiber.

[0035] 2. Preparation of cationic mullite fiber

[0036] SS1: 2.5 g (3-aminopropyl) triethoxysilane and 3 g mullite fiber were placed in 100 ml anhydrous ethanol, ultrasonically dispersed for 15 min, 10% oxalic acid solution was added to adjust the pH to 4, the temperature was raised to 70 ° C for 3 h, and the amino mullite fiber was obtained after filtration, washing and drying;

[0037] SS2: 3.5 g of amino-modified mullite fiber and 3 g of sodium alginate were ultrasonically dispersed in 120 ml of deionized water for 20 min. After standing for 2 h, the product was filtered and collected to obtain modified mullite fiber.

[0038] SS3: 3.6 g of modified mullite fiber was fully mixed with 180 ml of 1 mol / L hydrochloric acid solution, and after ultrasonic dispersion for 10 min, 4 g of aniline was added and stirred for 1 h. 4.2 ml of 0.1 mol / L ammonium persulfate solution was added dropwise at a rate of 30 s / drop. The mixture was reacted in an ice bath at 0°C for 12 h. After filtration, washing and drying, cationic mullite fiber was obtained.

[0039] The potential values ​​of amino-modified mullite fiber, modified mullite fiber and cationic mullite fiber were tested using SZ-100V2 Zeta potential analyzer. Figure 1 It can be seen that the potential value of the amino-modified mullite fiber is 4.4mv, which is caused by the positive charge on the surface of the mullite fiber after it is modified by the aminosilane coupling agent; the potential value of the modified mullite fiber is -2.6mv, which is caused by the negative charge on the modified mullite fiber after sodium alginate is adsorbed on the modified mullite fiber; the potential value of the cationic mullite fiber is 2.2mv, and the conversion of positive and negative charges is caused by the in-situ polymerization of aniline on the surface of the modified mullite fiber to coat it with positively charged polyaniline.

[0040] Preparation of waterproofing agent:

[0041] Step 1: Mix 35 g of fluorgypsum, 20 g of blast furnace slag, 8 g of aluminum slag powder, 10 g of fly ash, 8 g of calcium oxide, 6 g of calcium sulfoaluminate, 3 g of calcium formate, and 6 g of sodium methyl silicate to obtain a mixture;

[0042] Step 2: Add 6 g of sulfonated aramid fiber and 8 g of cationic mullite fiber into the mixture, stir and mix thoroughly to obtain a waterproofing agent.

[0043] Example 2

[0044] Preparation of waterproofing agent:

[0045] Step 1: Mix 40 g of fluorgypsum, 30 g of blast furnace slag, 12 g of aluminum slag powder, 15 g of fly ash, 10 g of calcium oxide, 10 g of calcium sulfoaluminate, 6 g of calcium formate, and 8 g of sodium methyl silicate to obtain a mixture;

[0046] Step 2: Add 7 g of sulfonated aramid fiber and 10 g of cationic mullite fiber into the mixture, stir and mix thoroughly to obtain a waterproofing agent.

[0047] The preparation method of the sulfonated aramid fiber and the cationic mullite fiber is consistent with that in Example 1.

[0048] Example 3

[0049] Step 1: Mix 50 g of fluorgypsum, 35 g of blast furnace slag, 18 g of aluminum slag powder, 20 g of fly ash, 15 g of calcium oxide, 15 g of calcium sulfoaluminate, 10 g of calcium formate, and 12 g of sodium methyl silicate to obtain a mixture;

[0050] Step 2: Add 8 g of sulfonated aramid fiber and 12 g of cationic mullite fiber into the mixture, stir and mix thoroughly to obtain a waterproofing agent.

[0051] The preparation method of the sulfonated aramid fiber and the cationic mullite fiber is consistent with that in Example 1.

[0052] Comparative Example 1

[0053] Preparation of waterproofing agent:

[0054] Step 1: Mix 40 g of fluorgypsum, 30 g of blast furnace slag, 12 g of aluminum slag powder, 15 g of fly ash, 10 g of calcium oxide, 10 g of calcium sulfoaluminate, 6 g of calcium formate, and 8 g of sodium methyl silicate to obtain a mixture;

[0055] Step 2: Place 10 g of cationic mullite fiber into the mixture, stir and mix thoroughly to obtain a waterproofing agent.

[0056] The preparation method of the cationic mullite fiber is consistent with that of Example 1.

[0057] Comparative Example 2

[0058] Preparation of waterproofing agent:

[0059] Step 1: Mix 40 g of fluorgypsum, 30 g of blast furnace slag, 12 g of aluminum slag powder, 15 g of fly ash, 10 g of calcium oxide, 10 g of calcium sulfoaluminate, 6 g of calcium formate, and 8 g of sodium methyl silicate to obtain a mixture;

[0060] Step 2: Place 7 g of sulfonated aramid fiber into the mixture, stir and mix thoroughly to obtain a waterproofing agent.

[0061] The preparation method of the sulfonated aramid fiber is consistent with that of Example 1.

[0062] Comparative Example 3

[0063] Preparation of waterproofing agent:

[0064] Step 1: Mix 40 g of fluorgypsum, 30 g of blast furnace slag, 12 g of aluminum slag powder, 15 g of fly ash, 10 g of calcium oxide, 10 g of calcium sulfoaluminate, 6 g of calcium formate, and 8 g of sodium methyl silicate to obtain a mixture;

[0065] Step 2: Add 7g of aramid fiber and 10g of cationic mullite fiber into the mixture, stir and mix them thoroughly to obtain a waterproofing agent.

[0066] The preparation method of the cationic mullite fiber is consistent with that of Example 1.

[0067] Comparative Example 4

[0068] Preparation of waterproofing agent:

[0069] Step 1: Mix 40 g of fluorgypsum, 30 g of blast furnace slag, 12 g of aluminum slag powder, 15 g of fly ash, 10 g of calcium oxide, 10 g of calcium sulfoaluminate, 6 g of calcium formate, and 8 g of sodium methyl silicate to obtain a mixture;

[0070] Step 2: Add 7 g of sulfonated aramid fiber and 10 g of modified mullite fiber into the mixture, stir and mix them thoroughly to obtain a waterproofing agent.

[0071] The preparation method of the sulfonated aramid fiber and the modified mullite fiber is consistent with that in Example 1.

[0072] Performance Testing

[0073] The waterproofing agents prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were used as samples for performance testing. The compressive strength of the samples was tested according to the reference standard GB / T50081-2002; the anti-cracking performance of the samples was tested according to the reference standard GB / T50082-2009; the anti-seepage performance and waterproof performance of the samples were tested according to the reference standard JC474-2008. The specific test results are shown in the following table:

[0074]

[0075] It can be seen from the above table that the waterproofing agents prepared in Examples 1 to 3 act on concrete, so that the concrete is completely hydrated, has high early strength, strong crack resistance, excellent anti-seepage effect, and good durability. The sample prepared in Comparative Example 1 does not add cationic mullite fiber, the sample prepared in Comparative Example 2 does not add sulfonated aramid fiber, the sample prepared in Comparative Example 3 does not add sulfonated aramid fiber but directly adds aramid fiber, and the sample prepared in Comparative Example 4 does not add cationic mullite fiber but adds modified mullite fiber. It can be seen that the samples prepared in Comparative Examples 1 to 4 are not as good as the performance of the samples in the embodiments.

[0076] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0077] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A solid waste-based low-carbon anti-cracking waterproofing agent, It is characterized in that The invention comprises the following raw materials in parts by weight: 6-8 parts of sulfonated aramid fiber, 8-12 parts of cationic mullite fiber, 35-50 parts of fluorinated gypsum, 20-35 parts of blast furnace slag, 8-18 parts of aluminum slag powder, 10-20 parts of fly ash, 8-15 parts of calcium oxide, 6-15 parts of calcium sulfoaluminate, 3-10 parts of calcium formate and 6-12 parts of sodium methyl silicate.

2. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 1, It is characterized in that The preparation method of the sulfonated aramid fiber comprises the following steps: S1: immersing the aramid fiber in acetone, ultrasonically cleaning for 5-6 hours, filtering and drying, irradiating the aramid fiber under ultraviolet light for 8-10 minutes, collecting the product, and obtaining carboxylated aramid fiber; S2: Take the composite catalyst and place it in anhydrous ethanol, add carboxylated aramid fiber, ultrasonically disperse for 8-10 minutes, then add p-aminobenzenesulfonic acid, react in a water bath at 60-65°C for 18-20 hours, wash, filter and vacuum dry to obtain sulfonated aramid fiber.

3. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 2, It is characterized in that The UV intensity of the UV lamp in step S1 is 50-55 μW / cm 2 .

4. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 2, It is characterized in that The composite catalyst in step S2 is dicyclohexylcarbodiimide and 4-dimethylaminopyridine in a mass ratio of 0.7-1:0.25-0.

3.

5. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 1, It is characterized in that The preparation method of the cationic mullite fiber comprises the following steps: SS1: Place the silane coupling agent and mullite fiber in anhydrous ethanol, ultrasonically disperse for 15-20 minutes, add oxalic acid solution to adjust the pH to 4-5, heat to 70-75°C for reaction for 3-4 hours, filter, wash and dry to obtain amino-modified mullite fiber; SS2: Place the aminated mullite fiber and sodium alginate in deionized water for ultrasonic dispersion for 20-30 minutes, let stand for 2-3 hours and then filter to collect the product to obtain modified mullite fiber; SS3: The modified mullite fiber is fully mixed with a hydrochloric acid solution with a concentration of 1-2 mol / L, ultrasonically dispersed for 10-20 minutes, and then aniline is added. The mixture is fully stirred for 1-2 hours, and the initiator is added dropwise at a rate of 30-35 seconds per drop. The mixture is reacted in an ice bath at 0-4°C for 12-14 hours. After filtering, washing, and drying, the cationic mullite fiber is obtained.

6. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 5, It is characterized in that The mass fraction of the oxalic acid solution in step SS1 is 10%-12%.

7. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 5, It is characterized in that The silane coupling agent described in step SS1 is any one of (3-aminopropyl)triethoxysilane, 3-(2-aminoethylamino)propylmethyldimethoxysilane, and [3-(6-aminohexylamino)propyl]trimethoxysilane.

8. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 5, It is characterized in that The initiator described in step SS3 is an ammonium persulfate solution having a concentration of 0.1-0.2 mol / L.

9. A solid waste-based low-carbon anti-cracking waterproofing agent according to claim 1, It is characterized in that The preparation method of the solid waste-based low-carbon anti-cracking waterproofing agent comprises the following steps: Step 1: mixing fluorinated gypsum, blast furnace slag, aluminum slag powder, fly ash, calcium oxide, calcium sulfoaluminate, calcium formate, and sodium methyl silicate to obtain a mixture; Step 2: placing sulfonated aramid fiber and cationic mullite fiber into a mixture, and stirring and mixing them thoroughly to obtain a waterproofing agent.