Additive composition for improving corrosion resistance and rust resistance of concrete
By using strong alkaline anion exchange resin, cationic polyacrylamide, expansion agent, internal curing agent, organosiloxane, activated diatomaceous earth and barium salt in the concrete, the chloride and sulfuric acid in the prior art are solved. The problem of salt corrosion has achieved the improvement of the efficient anti-corrosion and rust resistance of concrete, and met the protection needs of reinforced concrete in harsh environments.
Patent Information
- Application Number
- CN202411227966.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
Existing concrete anti-corrosion agents cannot effectively prevent the corrosion of chloride and sulfate in severe environments, and there are problems such as high amount, high cost and high toxicity. It is difficult to simultaneously inhibit the corrosion of chloride and sulfate, and to strengthen concrete The corrosion and rust resistance are not good.
Adopt an admixture composition, including a strong alkaline anion exchange resin, a cationic polyacrylamide, a composite of an expansion agent and an internal curing agent, an organosiloxane, activated diatomaceous earth and barium salts, and benzotriazoles, Through its synergistic action, it improves the compactness, hydrophobicity and corrosion resistance of concrete, and inhibits the transmission of harmful ions and corrosion electrochemical reactions.
It significantly improves the corrosion resistance and rust resistance of concrete, reduces the chloride ion migration coefficient and corrosion power, improves the corrosion resistance of sulfate, enhances the compactness and corrosion resistance of concrete, and meets GB/T 31296-2014 "Concrete corrosion resistance" Technical requirements in Rust Resistant.
Smart Images

Figure BDA0005025227320000021 
Figure BDA0005025227320000061 
Figure BDA0005025227320000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional admixture preparation, and specifically relates to an admixture composition for improving the anti-corrosion and rust-resistant performance of concrete. Background Art
[0002] Concrete is widely used in various projects due to its economical and high strength characteristics. However, in harsh environments such as saline soil, groundwater and marine areas, there are many corrosive media, such as sulfates and chlorides. The corrosion of these harmful ions is an important part of the research on concrete durability. It is also the most complex and harmful environmental water erosion, and is considered to be one of the main factors causing the durability degradation of concrete materials. In recent years, cases of concrete structures being corroded by sulfates and chlorides have been found in highways, bridges, hydraulic engineering and other projects, causing huge losses to the national economy. Therefore, it is crucial to improve the concrete's ability to resist sulfate and chloride corrosion.
[0003] At present, there are three main anti-corrosion measures commonly used for concrete: (1) reducing the water-cement ratio of concrete to improve its strength grade, but this method increases the cost of the project; (2) using anti-corrosion coatings to coat the surface of concrete structures, which is difficult to construct and the coating is easy to fall off; (3) using anti-sulfate cement, but anti-sulfate cement is expensive, and more importantly, anti-sulfate cement has poor resistance to chloride corrosion, and has poor anti-corrosion effect in an environment where chloride and sulfate coexist. The currently used anti-corrosion and rust inhibitors have problems such as high dosage, high cost, and high toxicity, and have almost no protective effect against corrosion caused by the coupling of sulfate and chloride. In anti-corrosion concrete projects, single-function admixtures have gradually failed to meet production needs. It can be seen that it is very necessary to develop an admixture that can simultaneously inhibit chloride and sulfate corrosion and has both anti-corrosion and rust-inhibiting functions. Summary of the invention
[0004] In view of the above problems and the shortcomings of the prior art, the purpose of the present invention is to provide an admixture composition that improves the anti-corrosion and rust-resistant properties of concrete, thereby solving the problem of severe corrosion of reinforced concrete when chlorides and sulfates coexist in harsh environments.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme to achieve: an admixture composition for improving the anti-corrosion and rust-resistant performance of concrete, which comprises the following components and proportions in terms of mass percentage:
[0006] Exchange resin 2~4%
[0007]
[0008] The exchange resin is a strongly alkaline anion exchange resin; the polyacrylamide is a cationic polyacrylamide with a molecular weight of 6 million to 8 million;
[0009] The dense component is a composite of an expansion agent and an internal curing agent, and the mass ratio of the composite is 100:1;
[0010] The organosiloxane is any one of n-octyltriethoxysilane and isooctyltriethoxysilane;
[0011] The diatomaceous earth is first ground for 15 minutes for mechanical activation and then calcined at 600°C for 2 hours for thermal activation;
[0012] The barium salt is any one of barium hydroxide and barium nitrate.
[0013] Compared with the prior art, the admixture composition disclosed in the present invention for improving the anti-corrosion and rust-resistant performance of concrete has the following advantages:
[0014] 1. The compacting component used in the present invention, in which the expansion agent has a compacting function, and the internal curing agent has two advantages. One advantage is that it has the function of repeated expansion, and the second advantage is that it has the function of releasing water and curing inside the concrete. Its internal curing function can further promote the expansion and compacting performance of the concrete, significantly improve the density of the concrete, and effectively inhibit the transmission of external harmful ions.
[0015] 2. The organosiloxane used in the present invention has good hydrophobic properties and can significantly reduce the water absorption rate of concrete. By inhibiting the transmission of water, the transmission of external harmful ions is indirectly inhibited.
[0016] 3. The activated diatomaceous earth used in the present invention has the characteristics of high active silicon dioxide content, good reaction activity, low cost, etc. It undergoes secondary hydration reaction with the hydration product calcium hydroxide, greatly consuming the content of the corroded product calcium hydroxide, and generating more hydrated calcium silicate gel, further improving the density and corrosion resistance of the concrete.
[0017] 4. The exchange resin used in the present invention has a good anion replacement effect, the cationic polyacrylamide used has a strong chemical adsorption effect on anions, and the barium salt used can further consume sulfate ions. Therefore, the combined effect of the three can significantly reduce the free harmful ions (Cl - 、SO4 2- )content.
[0018] 5. The benzotriazole used in the present invention forms a multi-layer protective film containing covalent bonds and coordination bonds on the surface of the steel bar, which can effectively block the corrosion of chloride ions and inhibit the electrochemical corrosion reaction. In addition, benzotriazole can also effectively promote the formation of hydrated calcium silicate gel, improve the density of concrete, and indirectly inhibit the occurrence of steel bar corrosion.
[0019] 6. In summary, the present invention utilizes the synergistic effects of improving the density and hydrophobicity of concrete, optimizing the composition of hydration products, replacing and adsorbing harmful ions inside concrete, and inhibiting corrosion electrochemical reactions to effectively inhibit the corrosion of reinforced concrete by chlorides and sulfates, and significantly improve the anti-corrosion and rust-resistant properties of reinforced concrete. DETAILED DESCRIPTION
[0020] In order to further illustrate the content of the present invention, the technical scheme of the present invention is further described through the following specific examples. The present invention evaluates the prepared product through technical parameters such as the compressive strength of concrete, chloride ion migration coefficient, sulfate corrosion resistance coefficient, and corrosion electricity.
[0021] Example 1
[0022] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0023] The mass percentage of each component is: 4% of strong alkaline anion exchange resin, 0.2% of polyacrylamide, 40.4% of expansion agent, 0.4% of internal curing agent, 4% of n-octyltriethoxysilane, 40% of diatomaceous earth, 1% of barium hydroxide, and 10% of benzotriazole.
[0024] Example 2
[0025] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0026] The mass percentage of each component is: 2% of strong alkaline anion exchange resin, 0.8% of polyacrylamide, 51.7% of expansion agent, 0.5% of internal curing agent, 2% of n-octyltriethoxysilane, 10% of diatomaceous earth, 3% of barium hydroxide, and 30% of benzotriazole.
[0027] Example 3
[0028] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0029] The mass percentage of each component is: 3% of strong alkaline anion exchange resin, 0.5% of polyacrylamide, 19.8% of expansion agent, 0.2% of internal curing agent, 3.5% of n-octyltriethoxysilane, 40% of diatomaceous earth, 3% of barium hydroxide, and 30% of benzotriazole.
[0030] Example 4
[0031] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0032] The mass percentage of each component is: 2% of strong alkaline anion exchange resin, 0.5% of polyacrylamide, 59.4% of expansion agent, 0.6% of internal curing agent, 4% of n-octyltriethoxysilane, 22.5% of diatomaceous earth, 1% of barium hydroxide, and 10% of benzotriazole.
[0033] Example 5
[0034] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0035] The mass percentage of each component is: 3% of strong alkaline anion exchange resin, 0.5% of polyacrylamide, 46% of expansion agent, 0.5% of internal curing agent, 3% of n-octyltriethoxysilane, 25% of diatomaceous earth, 2% of barium hydroxide, and 20% of benzotriazole.
[0036] Example 6
[0037] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0038] The mass percentage of each component is: 4% of strong alkaline anion exchange resin, 0.2% of polyacrylamide, 40.4% of expansion agent, 0.4% of internal curing agent, 4% of isooctyltriethoxysilane, 40% of diatomaceous earth, 1% of barium hydroxide, and 10% of benzotriazole.
[0039] Example 7
[0040] An admixture composition for improving the anti-corrosion and rust-resistant performance of concrete
[0041] The mass percentage of each component is: 2% of strong alkaline anion exchange resin, 0.8% of polyacrylamide, 51.7% of expansion agent, 0.5% of internal curing agent, 2% of n-octyltriethoxysilane, 10% of diatomaceous earth, 3% of barium nitrate, and 30% of benzotriazole.
[0042] Comparative Example 1
[0043] The benchmark group is concrete without the product prepared by the present invention.
[0044] Comparative Example 2
[0045] The method is basically the same as Example 1, except that the product does not contain strongly basic anion exchange resin and polyacrylamide, and the strongly basic anion exchange resin and polyacrylamide are replaced by cement in equal amounts.
[0046] Comparative Example 3
[0047] It is basically the same as Example 4, except that the product does not contain an expansion agent, an internal curing agent, or n-octyltriethoxysilane, and the expansion agent, the internal curing agent, and n-octyltriethoxysilane are replaced by an equal amount of cement.
[0048] Comparative Example 4
[0049] The method is basically the same as Example 1, except that the product does not contain diatomaceous earth, and the diatomaceous earth is replaced by an equal amount of cement.
[0050] Comparative Example 5
[0051] It is basically the same as Example 2, except that the product does not contain barium hydroxide, and the barium hydroxide is replaced by an equal amount of cement.
[0052] Comparative Example 6
[0053] The method is basically the same as Example 3, except that the product does not contain benzotriazole, and benzotriazole is replaced by an equal amount of cement.
[0054] Implementation Effect
[0055] In view of the serious corrosion problem of reinforced concrete when sulfate and chloride salt coexist in harsh environments, the present invention carries out functional design of the admixture composition from different technical dimensions, aiming to effectively improve the anti-corrosion and rust-resistant performance of reinforced concrete.
[0056] Anti-corrosion and rust resistance test: The test raw materials and mix ratio and other technical requirements are carried out in accordance with the provisions of GB / T 31296-2014 "Concrete Anti-corrosion and Rust Inhibitor". The cement uses standard cement, the natural sand fineness modulus is 2.7, the crushed stone is 5-10mm and 10-20mm, the water-cement ratio is 0.50, and the cement dosage is 420kg / m 3 The dosage of the products involved in the embodiments and comparative examples is 10%, that is, the cement is replaced by an equal amount. When testing the corrosion electricity, the sand ratio is 45%, and the slump is controlled at 50mm±10mm; when testing other items, the sand ratio is 38%, and the slump is controlled at 80mm±10mm. The slump is controlled by adjusting the dosage of the water reducing agent.
[0057] The compressive strength test was conducted in accordance with GB / T 50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Concrete"; the chloride ion migration coefficient and sulfate corrosion resistance coefficient test were conducted in accordance with GB / T 50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete", in which the sulfate corrosion test was conducted with 90 dry-wet cycles; the corrosion electricity was conducted in accordance with Appendix A of GB / T 31296-2014 "Concrete Anticorrosion and Rust Inhibitor". The results of the anticorrosion and rust resistance test are shown in Tables 1 and 2, and the test results in Table 2 are compared with the technical requirements of the main items of GB / T31296-2014 "Concrete Anticorrosion and Rust Inhibitor". It can be seen from the test results in Table 1 that, relative to Comparative Example 1, the chloride ion migration coefficients of Examples 1 to 7 are significantly reduced, the corrosion resistance coefficients are significantly improved, and the corrosion power is significantly reduced. The maximum reduction in the chloride ion migration coefficient is 29%, the maximum improvement in the corrosion resistance coefficient is 34%, and the maximum reduction in the corrosion power is 59%. Compared with Comparative Example 2, when Example 1 does not contain exchange resin and polyacrylamide, the corrosion resistance coefficient decreases by 20%, and the corrosion power increases by 19%. Compared with Comparative Example 4, when Example 1 does not contain diatomaceous earth, the chloride ion migration coefficient increases by 10%. The corrosion resistance coefficient of Example 2 increased by 14%, the corrosion resistance coefficient decreased by 18%, and the corrosion electricity increased by 8%; when Example 2 was compared with Comparative Example 5, the chloride ion migration coefficient was equivalent when barium salt was not contained, the corrosion resistance coefficient decreased by 12%, and the corrosion electricity was equivalent; when Example 3 was compared with Comparative Example 6, the chloride ion migration coefficient and the corrosion resistance coefficient were equivalent when benzotriazole was not contained, but the corrosion electricity increased by 17%; when Example 4 was compared with Comparative Example 3, the chloride ion migration coefficient increased by 30%, the corrosion resistance coefficient decreased by 5%, and the corrosion electricity increased by 20% when dense components and organic siloxane were not contained. In summary, the functional components involved in the present invention all have an impact on the anti-corrosion and rust-proof performance of concrete, among which the combination of exchange resin and polyacrylamide has a great influence on the sulfate corrosion resistance coefficient and the corrosion electricity, diatomaceous earth has a great influence on the sulfate corrosion resistance coefficient, benzotriazole has a great influence on the corrosion electricity, and the combination of dense components and organic siloxane has a great influence on the chloride ion migration coefficient and the corrosion electricity. It can be seen from the test results in Table 2 that the products prepared according to the present invention can well meet the technical requirements of GB / T 31296-2014 "Concrete Anticorrosion and Rust Inhibitors" in terms of anticorrosion and rust inhibition performance.
[0058] Table 1 Test results of anticorrosion and rust resistance performance of admixture composition
[0059]
[0060] Table 2 Comparison of anticorrosion and rust resistance performance of admixture composition with standard technical requirements
[0061]
[0062]
[0063] Although the present invention lists some embodiments as disclosed above, they are not intended to limit the present invention. Anyone familiar with this technology can make various changes or modifications without departing from the spirit and scope of the present invention. For example, adding or reducing a certain raw material component or process time may not have a substantial impact on the effect of the product. In this case, such changes also fall within the scope defined by the scope of protection of the claims of this application.
Claims
1. An admixture composition for improving the anti-corrosion and rust-resistant properties of concrete, Features: In terms of mass percentage, it includes the following components and proportions:
2. The admixture composition for improving the anti-corrosion and rust-resistant performance of concrete according to claim 1, Features: The exchange resin is a strongly basic anion exchange resin.
3. The admixture composition for improving the anti-corrosion and rust-resistant performance of concrete according to claim 1, Features: The polyacrylamide is cationic polyacrylamide, and its molecular weight is 6 million to 8 million.
4. The admixture composition for improving the anti-corrosion and rust-resistant performance of concrete according to claim 1, Features: The dense component is a composite of an expansion agent and an internal curing agent, and the mass ratio of the composite is 100:
1.
5. The admixture composition for improving the anti-corrosion and rust-resistant performance of concrete according to claim 1, Features: The organosiloxane is any one of n-octyltriethoxysilane and isooctyltriethoxysilane.
6. The admixture composition for improving the anti-corrosion and rust-resistant performance of concrete according to claim 1, Features: The diatomaceous earth is first ground for 15 minutes for mechanical activation and then calcined at 600° C. for 2 hours for thermal activation.
7. The admixture composition for improving the anti-corrosion and rust-resistant performance of concrete according to claim 1, Features: The barium salt is any one of barium hydroxide and barium nitrate.