Ultrahigh-temperature tantalum-titanium-carbon ceramic precursor and preparation method thereof
The preparation of an ultra-high temperature tantalum-titanium-carbon ceramic precursor addresses processing difficulties and mechanical weaknesses of existing precursors by forming a solid solution, resulting in high strength and low viscosity materials for high-temperature applications.
Patent Information
- Application Number
- CN202411166519.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
AI Technical Summary
Existing multi-phase composite ceramic precursors, such as tantalum hafnium carbide, face challenges with high viscosity, difficult processing, low bending strength, and poor mechanical properties, making them unsuitable for high-temperature applications.
A method for preparing an ultra-high temperature tantalum-titanium-carbon ceramic precursor involves specific steps of reacting metallic sodium with cyclopentadiene, mixing tantalum pentachloride and organic solvents, and combining tantalum and titanium carbide precursors to form a solid solution, achieving a curing temperature of 170-190°C and improved mechanical properties.
The resulting ceramic precursor exhibits high bending strength, low viscosity, and resistance to ablation, suitable for high-temperature environments with yields of 38-46% at 1400-1600°C and mechanical strengths of 500-800MPa at 1600°C.
Smart Images

Figure CN119080498A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high temperature resistant ceramic materials, and in particular to an ultra-high temperature tantalum titanium carbon ceramic precursor and a preparation method thereof. Background Art
[0002] In recent years, ultra-high temperature ceramic precursors have developed from pure phase ceramic precursors to multiphase composite ceramic precursors. Compared with single-phase ceramic precursors, multiphase composite ceramic precursors have higher corrosion resistance and oxidation resistance. Among carbide ceramic precursors, tantalum carbide and titanium carbide have higher melting points (above 2000°C) and extremely low carbon diffusion permeability under ultra-high temperature environments. Under high temperature and oxygen conditions, tantalum carbide and titanium carbide are prone to oxidation reactions, and the resulting oxides can effectively block the inward diffusion of oxygen. Therefore, carbide ceramic precursors are of great significance for the design and use of high temperature resistant ceramic materials.
[0003] The existing multi-phase composite ceramic precursor is a tantalum hafnium carbide ceramic precursor, which is mainly prepared directly using the oxygen-containing principle. Therefore, the tantalum hafnium carbide ceramic precursor has high viscosity, is difficult to process, has a high curing temperature (reaching 260 degrees Celsius), has a low ablation rate, low bending strength, and poor mechanical properties. Summary of the invention
[0004] In view of this, one of the purposes of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a method for preparing an ultra-high temperature tantalum-titanium-carbon ceramic precursor. The ultra-high temperature tantalum-titanium-carbon ceramic precursor prepared by this preparation method is resistant to ablation, easy to process, has high bending strength and good mechanical properties.
[0005] One of the purposes of the present invention is to provide an ultra-high temperature tantalum-titanium-carbon ceramic precursor.
[0006] In order to achieve one of the above purposes, the present invention adopts the following technical solution:
[0007] A method for preparing an ultra-high temperature tantalum-titanium-carbon ceramic precursor, characterized in that the preparation method comprises the following steps:
[0008] Step S1, in a nitrogen atmosphere, dispersing metallic sodium and cyclopentadiene in an organic solvent, stirring, and reacting at a temperature of -10 to -5°C for 1.6 to 5.8 hours to obtain a sodium cyclopentadiene solution with a mass concentration of 5 to 17%;
[0009] The mass ratio of the sodium metal, cyclopentadiene and the organic solvent is 1:1-10:10-200;
[0010] Step S2, in a nitrogen atmosphere, tantalum pentachloride and an organic solvent are mixed and stirred evenly, a sodium cyclopentadienyl solution is added dropwise at a temperature of -10 to -5°C, and then distilled, and then a mixed solvent is added in batches for purification to obtain tantalum trichloride;
[0011] The mass ratio of sodium cyclopentadienyl to the organic solvent in the tantalum pentachloride and sodium cyclopentadienyl solution is 1:2-40:10-600;
[0012] The mixed solvent includes different first solvents and second solvents;
[0013] Step S3, in a nitrogen atmosphere, slowly adding the first reagent to a mixed solution of tantalum trichloride and an organic solvent at a temperature of -10 to -5°C, raising the temperature to 10 to 50°C after the addition is complete, reacting for 3.6 to 4.3 hours, and filtering to obtain a first tantalum intermediate;
[0014] The mass ratio of tantalum trichloride, the organic solvent and the first reagent is 1-25:2-125:1;
[0015] Step S4, in a nitrogen atmosphere, slowly adding the second reagent to the mixed solution of tantalum trichloride and the organic solvent at a temperature of -25 to -20°C, introducing hydrogen after the addition, continuing stirring for 2.6 to 5.3 hours, filtering, adding a polyolefin with a molecular weight of 2000 to 500000, slowly heating to 78 to 82°C, reacting for 1.8 to 2.2 hours, and continuing to heat to 90 to 100°C to recover the organic solvent to obtain a second tantalum intermediate;
[0016] The mass ratio of tantalum trichloride, organic solvent, polyolefin and second reagent is 1-60:2-250:1-4:1;
[0017] Step S5, mixing the organic solvent, the first tantalum intermediate and the second tantalum intermediate in a mass ratio of 2-15:1-3:1, and reacting at 57-61° C. for 3.7-4.2 hours to obtain a tantalum carbide ceramic precursor;
[0018] Step S6, dissolving titanium tetrachloride and phenolic resin 2402 in anhydrous ethanol, stirring evenly at a temperature of 63 to 77° C., and then drying at 82 to 118° C. for 16 to 21 hours to obtain a titanium carbide ceramic precursor;
[0019] The mass ratio of titanium tetrachloride, phenolic resin and anhydrous ethanol is 1-10:1:1-60;
[0020] Step S7, according to the mass ratio of 1-10:1:5-90, the tantalum carbide ceramic precursor, the titanium carbide ceramic precursor and the organic solvent are mixed, stirred and dispersed for 3.6-9.3 hours to obtain an ultra-high temperature tantalum titanium carbon ceramic precursor.
[0021] Furthermore, in step S1, the concentration of the sodium cyclopentadiene solution is 8% to 12%.
[0022] Further, the organic solvent is one or more of benzene, toluene, dichloromethane, tetrahydrofuran, DMF, and N-methylpyrrolidone;
[0023] The stirring rate is 500-1200 r / min;
[0024] Furthermore, the stirring rate is 800-900 r / min.
[0025] Further, in step S2, the number of batches includes 4 times, and the mass ratios of the first solvent and the second solvent in the 4 times are 1:1, 2:1, 3:1 and 4:1 respectively, and the mass ratio of the first solvent to the second solvent gradually increases;
[0026] The first solvent and the second solvent are respectively one of benzene, toluene, dichloromethane and tetrahydrofuran.
[0027] Furthermore, in step S3, the first reagent is one or more of formic acid, tetrahydrofuran, acetone, chloroform, dichloromethane, chloroform, N,N-dimethylacetamide, carbon tetrachloride, methanol, ethanol, isopropane, tert-butanol, toluene, and xylene.
[0028] Further, in step S4, the polyolefin is one or more of polyethylene, polypropylene, poly-1-butene, and poly-1-octene;
[0029] The second reagent is one or more of methyl lithium, ethyl lithium, propyl lithium, butyl lithium, n-butenyl magnesium bromide, isobutenyl magnesium bromide, and isopentenyl magnesium bromide.
[0030] Furthermore, the molecular weight of the polyolefin is 5,000 to 50,000, preferably 10,000.
[0031] In order to achieve the second objective above, the present invention adopts the following technical solution:
[0032] An ultra-high temperature tantalum-titanium-carbon ceramic precursor, characterized in that the ultra-high temperature tantalum-titanium-carbon ceramic precursor is prepared by the preparation method described above.
[0033] The beneficial effects of the present invention are:
[0034] The present invention uses a tantalum carbide ceramic precursor and a titanium carbide ceramic precursor, and adopts a transition metal Ti element to replace the Ta element to prepare a solid solution, so as to achieve stability at high temperature (the initial melting temperature is close to 2800°C), so that the composite material (i.e., the ultra-high temperature tantalum titanium carbon ceramic precursor) can be fractured from intergranular fracture to cascade fracture at high temperature, thereby achieving performance improvement at high temperature instead of reduction, and effectively improving the mechanical properties of the composite material at high temperature; the present invention uses a polymer precursor (tantalum carbide ceramic precursor and titanium carbide ceramic precursor) to achieve cross-linking and curing, and obtains a nitrogen-free and oxygen-free ultra-high temperature tantalum titanium carbon The ceramic precursor has broad application prospects in the field of high-temperature resistant high-entropy ceramics; the curing temperature of the ultra-high temperature tantalum titanium carbon ceramic precursor of the invention is 170-190°C, the viscosity is less than 150-170 mPa.s, the yield of the ultra-high temperature tantalum titanium carbon ceramic precursor at 1400°C is 45.15-46.27%, the yield of the ultra-high temperature tantalum titanium carbon ceramic precursor at 1600°C is 38.06-39.47%, the strength of the ultra-high temperature tantalum titanium carbon ceramic precursor at 1600°C is 600-800MPa, and the bending strength of the ultra-high temperature tantalum titanium carbon ceramic precursor at 900°C is 500-580MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a scanning electron microscope image of the 1400°C ceramic product of the ultra-high temperature tantalum-titanium-carbon ceramic precursor of Example 1;
[0036] Figure 2 This is a TGA curve diagram of the ultra-high temperature tantalum-titanium-carbon ceramic precursor of Example 1;
[0037] Figure 3 This is the DSC curve of the ultra-high temperature tantalum titanium carbon ceramic precursor of Example 3. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0039] Embodiment 1:
[0040] (1) Under a nitrogen atmosphere, sodium metal, cyclopentadiene and benzene are placed in a 250 mL three-necked flask in a mass ratio of 1:1 to 10:10 to 200, and stirred and dispersed at a stirring rate of 500 r / min at -10°C for 1.6 h to obtain an 8% sodium cyclopentadiene solution.
[0041] (2) Under nitrogen atmosphere, tantalum pentachloride and benzene were stirred into a suspension at a stirring rate of 500 r / min in a 250 mL three-necked flask, and a sodium cyclopentadienyl solution was added dropwise at -10°C, followed by distillation, and then purified by a gradient solvent (the gradient solvent was a mixed solvent of toluene and dichloromethane in a ratio of 1:1, 2:1, 3:1 and 4:1, respectively) to obtain tantalum trichloride. The mass ratio of tantalum pentachloride, sodium cyclopentadienyl and benzene was 1:10:100.
[0042] (3) Under nitrogen atmosphere, at a stirring rate of 500 r / min, tantalum trichloride and benzene were stirred and dispersed in a 250 mL three-necked flask, formic acid was slowly added dropwise at -10°C, then the temperature was raised to 10°C and the reaction was continued for 4 hours, and the first tantalum intermediate was obtained by suction filtration. The mass ratio of tantalum trichloride, benzene and formic acid was 1:2:1.
[0043] (4) Under nitrogen atmosphere, at -25°C, in a 250 mL three-necked flask, methyl lithium was dropped into a mixture of tantalum trichloride and benzene, hydrogen was introduced, and the mixture was stirred for 4 h at a stirring rate of 500 r / min until the reaction was complete. After filtration, polyethylene with a molecular weight of 50,000 was added, and the temperature was raised to 80°C for reaction for 2 h, and the second tantalum intermediate was obtained by adjusting the degree of polymerization. The mass ratio of tantalum trichloride, benzene, polyethylene and methyl lithium was 1:2:1:1.
[0044] (5) adding benzene, the first tantalum intermediate and the second tantalum intermediate into a reaction kettle in a mass ratio of 2:1:1, reacting at 57° C. for 3.7 hours to obtain a tantalum carbide ceramic precursor;
[0045] (6) Titanium tetrachloride and phenolic resin were dissolved in anhydrous ethanol in a mass ratio of 1:1:1, stirred at 63°C and a stirring rate of 500 r / min to obtain a titanium-containing gel, and then dried at 82°C for 16 hours to obtain a titanium carbide ceramic precursor.
[0046] (7) According to the mass ratio of 1:1:1, tantalum carbide ceramic precursor, titanium carbide ceramic precursor and benzene are added into the reaction kettle, and stirred and dispersed for 4 hours (3.6 to 9.3 hours) at a stirring rate of 800 r / min to obtain an ultra-high temperature tantalum titanium carbon ceramic precursor.
[0047] In an argon atmosphere, the ultrahigh temperature tantalum titanium carbon ceramic precursor prepared in this embodiment was cured and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yield under these conditions was calculated as shown in Table 1, the curing temperature and viscosity were shown in Table 2, and the mechanical properties were shown in Table 3. The scanning electron microscope image, TGA curve graph and DSC curve graph of the 1400°C ceramic product of the ultrahigh temperature tantalum titanium carbon ceramic precursor were shown in Table 3. Figure 1 , Figure 2 and 3 shown.
[0048] Embodiment 2:
[0049] (1) Under nitrogen atmosphere, sodium metal, cyclopentadiene and toluene were placed in a 250 mL three-necked flask in a mass ratio of 1:10:200, and the mixture was stirred and dispersed at a stirring rate of 800 r / min at -5°C for 5.8 h to obtain a 17% sodium cyclopentadiene solution.
[0050] (2) Under nitrogen atmosphere, tantalum pentachloride and toluene were stirred into a suspension at a stirring rate of 800 r / min in a 250 mL three-necked flask, and a sodium cyclopentadienyl solution was added dropwise at -5°C, followed by distillation, and then purified by a gradient solvent (the gradient solvent was a mixed solvent of benzene and toluene in a ratio of 1.5:1, 2.5:1, 3.5:1 and 4.5:1, respectively) to obtain tantalum trichloride. The mass ratio of tantalum pentachloride, sodium cyclopentadienyl and toluene was 1:2:10.
[0051] (3) Under nitrogen atmosphere, at a stirring rate of 800 r / min, tantalum trichloride and benzene were stirred and dispersed in a 250 mL three-necked flask, tetrahydrofuran was slowly added dropwise at -10°C, then the temperature was raised to 10°C and reacted for 4 hours, and then filtered to obtain a first tantalum intermediate. The mass ratio of tantalum trichloride, toluene and tetrahydrofuran was 25:125:1.
[0052] (4) Under nitrogen atmosphere, at -25°C, in a 250 mL three-necked flask, ethyl lithium was dropped into a mixture of tantalum trichloride and toluene, hydrogen was introduced, and the mixture was stirred at a stirring rate of 800 r / min for 4 h to complete the reaction. After filtration, polypropylene with a molecular weight of 2000 was added, and the temperature was raised to 80°C for reaction for 2 h, and the second tantalum intermediate was obtained by adjusting the degree of polymerization. The mass ratio of tantalum trichloride, toluene, polypropylene and ethyl lithium was 60:250:4:1.
[0053] (5) Toluene, the first tantalum intermediate and the second tantalum intermediate were added into a reactor in a mass ratio of 15:3:1, and reacted at 61° C. for 4.2 h to obtain a tantalum carbide ceramic precursor.
[0054] (6) Titanium tetrachloride and phenolic resin were dissolved in anhydrous ethanol at a mass ratio of 10:1:60, stirred at 77°C and a stirring rate of 800 r / min to obtain a titanium-containing gel, and then dried at 118°C for 16 h to obtain a titanium carbide ceramic precursor.
[0055] (7) Tantalum carbide ceramic precursor, titanium carbide ceramic precursor and toluene were added into a reactor at a mass ratio of 10:1:90, and stirred and dispersed for 3.6 hours at a stirring rate of 800 r / min to obtain an ultra-high temperature tantalum titanium carbon ceramic precursor.
[0056] In an argon atmosphere, the ultra-high temperature tantalum titanium carbon ceramic precursor prepared in this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yield under these conditions was calculated as shown in Table 1, the solidification temperature and viscosity were shown in Table 2, and the mechanical properties were shown in Table 3.
[0057] Embodiment 3:
[0058] (1) Under a nitrogen atmosphere, sodium metal, cyclopentadiene and dichloromethane were placed in a 250 mL three-necked flask in a mass ratio of 1:5:150, and the mixture was stirred and dispersed at -8°C at a stirring rate of 1200 r / min for 4.5 h to obtain a 5% sodium cyclopentadiene solution.
[0059] (2) Under nitrogen atmosphere, tantalum pentachloride and dichloromethane were stirred into a suspension in a 250 mL three-necked flask at a stirring rate of 1200 r / min, and a sodium cyclopentadienyl solution was added dropwise at -7°C, followed by distillation, and then purified by a gradient solvent (the gradient solvent was a mixed solvent of benzene and tetrahydrofuran in ratios of 1.5:1, 2.5:1, 3.5:1 and 4.5:1, respectively) to obtain tantalum trichloride. The mass ratio of tantalum pentachloride, sodium cyclopentadienyl and dichloromethane was 1:40:600.
[0060] (3) Under nitrogen atmosphere, at a stirring rate of 1200 r / min, tantalum trichloride and dichloromethane were stirred and dispersed in a 250 mL three-necked flask, acetone was slowly added dropwise at -10°C, and then the temperature was raised to 10°C to react for 4 hours, and filtered to obtain a first tantalum intermediate. The mass ratio of tantalum trichloride, dichloromethane and tetrahydrofuran was 10:100:1.
[0061] (4) Under nitrogen atmosphere, at -22°C, in a 250mL three-necked flask, propyl lithium was dripped into a mixture of tantalum trichloride and dichloromethane, hydrogen was introduced, and the mixture was stirred at a stirring rate of 1200r / min for 5.3h to complete the reaction. After filtration, poly-1-butene with a molecular weight of 500000 was added, and the temperature was raised to 82°C for reaction for 2.2h. The second tantalum intermediate was obtained by adjusting the degree of polymerization. The mass ratio of tantalum trichloride, dichloromethane, poly-1-butene and propyl lithium was 40:100:3:1.
[0062] (5) adding dichloromethane, the first tantalum intermediate and the second tantalum intermediate into a reaction kettle in a mass ratio of 15:3:1, reacting at 60° C. for 3.8 hours to obtain a tantalum carbide ceramic precursor;
[0063] (6) Titanium tetrachloride and phenolic resin were dissolved in anhydrous ethanol at a mass ratio of 8:1:40, stirred at 70°C and a stirring rate of 1200 r / min to obtain a titanium-containing gel, and then dried at 118°C for 21 hours to obtain a titanium carbide ceramic precursor.
[0064] (7) Tantalum carbide ceramic precursor, titanium carbide ceramic precursor and dichloromethane were added into a reactor at a mass ratio of 8:1:40, and stirred and dispersed for 3.6 hours at a stirring rate of 500 r / min to obtain an ultra-high temperature tantalum titanium carbon ceramic precursor.
[0065] In an argon atmosphere, the ultra-high temperature tantalum titanium carbon ceramic precursor prepared in this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yield under these conditions was calculated as shown in Table 1, the solidification temperature and viscosity were shown in Table 2, and the mechanical properties were shown in Table 3.
[0066] Embodiment 4:
[0067] (1) Under nitrogen atmosphere, sodium metal, cyclopentadiene and tetrahydrofuran were placed in a 250 mL three-necked flask in a mass ratio of 1:4:100, and stirred and dispersed at -6°C at a stirring rate of 900 r / min for 5 h to obtain a 5% sodium cyclopentadiene solution.
[0068] (2) Under nitrogen atmosphere, tantalum pentachloride and tetrahydrofuran were stirred into a suspension in a 250 mL three-necked flask at a stirring rate of 900 r / min, and a sodium cyclopentadienyl solution was added dropwise at -6°C, followed by distillation, and then purified by a gradient solvent (the gradient solvent was a mixed solvent of toluene and tetrahydrofuran in ratios of 1.5:1, 2.5:1, 3.5:1 and 4.5:1, respectively) to obtain tantalum trichloride. The mass ratio of tantalum pentachloride, sodium cyclopentadienyl and tetrahydrofuran was 1:30:300.
[0069] (3) Under nitrogen atmosphere, at a stirring rate of 1200 r / min, tantalum trichloride and tetrahydrofuran were stirred and dispersed in a 250 mL three-necked flask, chloroform was slowly added dropwise at -10°C, then the temperature was raised to 50°C and the reaction was continued for 3.8 hours, and the first tantalum intermediate was obtained by suction filtration. The mass ratio of tantalum trichloride, tetrahydrofuran and chloroform was 20:120:1.
[0070] (4) In a nitrogen atmosphere, at -25°C, in a 250 mL three-necked flask, butyl lithium was dropped into a mixture of tantalum trichloride and tetrahydrofuran, hydrogen was introduced, and the mixture was stirred at a stirring rate of 1200 r / min for 2.6 h to complete the reaction. After filtration, poly-1-octene with a molecular weight of 10,000 was added, and the temperature was raised to 78°C for reaction for 1.8 h. The second tantalum intermediate was obtained by adjusting the degree of polymerization. The mass ratio of tantalum trichloride, tetrahydrofuran, poly-1-octene and butyl lithium was 20:20:2:1.
[0071] (5) Tetrahydrofuran, the first tantalum intermediate and the second tantalum intermediate were added into a reaction kettle in a mass ratio of 10:2:1, and reacted at 58° C. for 4.2 h to obtain a tantalum carbide ceramic precursor.
[0072] (6) Titanium tetrachloride and phenolic resin were dissolved in anhydrous ethanol at a mass ratio of 8:1:40, stirred at 70°C and a stirring rate of 1200 r / min to obtain a titanium-containing gel, and then dried at 118°C for 21 hours to obtain a titanium carbide ceramic precursor.
[0073] (7) Tantalum carbide ceramic precursor, titanium carbide ceramic precursor and tetrahydrofuran were added into a reaction kettle at a mass ratio of 8:1:40, and stirred and dispersed for 3.6 hours at a stirring rate of 500 r / min to obtain an ultra-high temperature tantalum titanium carbon ceramic precursor.
[0074] In an argon atmosphere, the ultra-high temperature tantalum titanium carbon ceramic precursor prepared in this embodiment was solidified and then subjected to cracking tests at 1400°C and 1600°C, respectively. The ceramic yield under these conditions was calculated as shown in Table 1, the solidification temperature and viscosity were shown in Table 2, and the mechanical properties were shown in Table 3.
[0075] Table 1 Performance indicators of Examples 1 to 4.
[0076]
[0077]
[0078] Table 2 Curing temperature and viscosity of Examples 1 to 4
[0079] Example Curing temperature(℃) Viscosity (mPa.s) Example 1 180 165 Example 2 190 170 Example 3 170 150 Example 4 175 155
[0080] Table 3 Mechanical properties of Examples 1 to 4 (bending strength MPa)
[0081] Example 900℃ flexural strength (MPa) 1600℃ flexural strength (MPa) Example 1 520 614 Example 2 515 650 Example 3 580 800 Example 4 560 750
[0082] The above examples are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the best embodiment, a person skilled in the art should understand that the technical solution of the present invention can still be modified or replaced by equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing an ultra-high temperature tantalum-titanium-carbon ceramic precursor, characterized in that: The preparation method comprises the following steps: Step S1, in a nitrogen atmosphere, dispersing metallic sodium and cyclopentadiene in an organic solvent, stirring, and reacting at a temperature of -10 to -5°C for 1.6 to 5.8 hours to obtain a sodium cyclopentadiene solution with a mass concentration of 5 to 17%; The mass ratio of the sodium metal, cyclopentadiene and the organic solvent is 1:1-10:10-200; Step S2, in a nitrogen atmosphere, tantalum pentachloride and an organic solvent are mixed and stirred evenly, a sodium cyclopentadienyl solution is added dropwise at a temperature of -10 to -5°C, and then distilled, and then a mixed solvent is added in batches for purification to obtain tantalum trichloride; The mass ratio of sodium cyclopentadienyl to the organic solvent in the tantalum pentachloride and sodium cyclopentadienyl solution is 1:2-40:10-600; The mixed solvent includes different first solvents and second solvents; Step S3, in a nitrogen atmosphere, slowly adding the first reagent to a mixed solution of tantalum trichloride and an organic solvent at a temperature of -10 to -5°C, raising the temperature to 10 to 50°C after the addition is complete, reacting for 3.6 to 4.3 hours, and filtering to obtain a first tantalum intermediate; The mass ratio of tantalum trichloride, the organic solvent and the first reagent is 1-25:2-125:1; Step S4, in a nitrogen atmosphere, slowly adding the second reagent to the mixed solution of tantalum trichloride and the organic solvent at a temperature of -25 to -20°C, introducing hydrogen after the addition, continuing stirring for 2.6 to 5.3 hours, filtering, adding a polyolefin with a molecular weight of 2000 to 500000, slowly heating to 78 to 82°C, reacting for 1.8 to 2.2 hours, and continuing to heat to 90 to 100°C to recover the organic solvent to obtain a second tantalum intermediate; The mass ratio of tantalum trichloride, organic solvent, polyolefin and second reagent is 1-60:2-250:1-4:1; Step S5, mixing the organic solvent, the first tantalum intermediate and the second tantalum intermediate in a mass ratio of 2-15:1-3:1, and reacting at 57-61° C. for 3.7-4.2 hours to obtain a tantalum carbide ceramic precursor; Step S6, dissolving titanium tetrachloride and phenolic resin 2402 in anhydrous ethanol, stirring evenly at a temperature of 63 to 77° C., and then drying at 82 to 118° C. for 16 to 21 hours to obtain a titanium carbide ceramic precursor; The mass ratio of titanium tetrachloride, phenolic resin and anhydrous ethanol is 1-10:1:1-60; Step S7, according to the mass ratio of 1-10:1:5-90, the tantalum carbide ceramic precursor, the titanium carbide ceramic precursor and the organic solvent are mixed, stirred and dispersed for 3.6-9.3 hours to obtain an ultra-high temperature tantalum titanium carbon ceramic precursor.
2. The preparation method according to claim 1, characterized in that: In the step S1, the concentration of the sodium cyclopentadiene solution is 8% to 12%.
3. The preparation method according to claim 2, characterized in that: The organic solvent is one or more of benzene, toluene, dichloromethane, tetrahydrofuran, DMF, and N-methylpyrrolidone; The stirring rate is 500-1200 r / min.
4. The preparation method according to claim 3, characterized in that: The stirring speed is 800-900 r / min.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S2, the batching is performed 4 times, and the mass ratios of the first solvent and the second solvent in the 4 times are 1:1, 2:1, 3:1 and 4:1 respectively; The first solvent and the second solvent are respectively one of benzene, toluene, dichloromethane and tetrahydrofuran.
6. The preparation method according to claim 5, characterized in that: In step S3, the first reagent is one or more of formic acid, tetrahydrofuran, acetone, chloroform, dichloromethane, chloroform, N,N-dimethylacetamide, carbon tetrachloride, methanol, ethanol, isopropane, tert-butanol, toluene, and xylene.
7. The preparation method according to claim 6, characterized in that: In the step S4, the polyolefin is one or more of polyethylene, polypropylene, poly-1-butene, and poly-1-octene; The second reagent is one or more of methyl lithium, ethyl lithium, propyl lithium, butyl lithium, n-butenyl magnesium bromide, isobutenyl magnesium bromide, and isopentenyl magnesium bromide.
8. The preparation method according to claim 7, characterized in that: The molecular weight of the polyolefin is 5,000 to 50,000.
9. The preparation method according to claim 8, characterized in that: The molecular weight of the polyolefin is 10,000 to 30,000.
10. An ultra-high temperature tantalum-titanium-carbon ceramic precursor, characterized in that: The ultra-high temperature tantalum-titanium-carbon ceramic precursor is prepared by the preparation method described in claims 1 to 9.