Refractory material prepared from investment casting waste sand and preparation method
By using investment casting materials such as waste sand, combined with metallurgical slag and rice husk ash, refractory materials are prepared by using a multi-step process, which solves the problems of resource reuse and performance optimization, and achieves efficient environmental protection and cost reduction.
Patent Information
- Application Number
- CN202411483586.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the resource reuse of refractory materials is insufficient, resulting in high environmental pollution and production costs, and the performance of existing refractory materials is not optimized enough.
Using investment casting waste sand, metallurgical slag, rice husk ash and other materials, through crushing, magnetic separation, ball milling, drying, ultrasonic stirring and microwave sintering, refractory materials with high refractory resistance are prepared to improve resource utilization and performance. .
Waste reuse is achieved, environmental pollution and production costs are reduced, and the refractory resistance and mechanical strength of refractory materials are improved, which enhances its adaptability and thermal insulation properties.
Smart Images

Figure CN119080519A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refractory materials, and in particular to a refractory material prepared by using investment casting waste sand and a preparation method thereof. Background Art
[0002] The mold shell material used in investment casting is refractory. In investment casting, the mold shell must be resistant to high temperatures, thermochemically stable, have suitable thermal expansion performance, and the air permeability and shelling performance must meet the performance requirements of the casting. These requirements for the mold shell must be met by the refractory material used to manufacture the mold shell. A large amount of waste sand is discharged during the investment casting process, which directly affects the energy consumption, environmental pollution, quality of castings, production efficiency and cost.
[0003] Refractory materials refer to inorganic non-metallic materials with a refractoriness of not less than 1580℃. Refractoriness refers to the Celsius temperature at which a cone-shaped specimen of a refractory material can resist high temperature without softening and melting under no load. However, defining refractory materials only by refractoriness is not enough to fully describe refractory materials, and 1580℃ is not absolute. It is now defined as any material whose physical and chemical properties allow it to be used in a high temperature environment. Refractory materials are widely used in metallurgy, chemical industry, petroleum, machinery manufacturing, silicate, power and other industrial fields, and are used the most in the metallurgical industry.
[0004] In the prior art, there are many types of refractory materials, and the performance of different types of refractory materials is also different. However, due to the increasingly stringent national environmental protection policies at this stage, higher and higher requirements are placed on the environment and resource recycling of enterprises. How to reuse resources in the research and development of refractory materials has become a problem that needs to be solved at present. Therefore, the present invention proposes a refractory material prepared by using investment casting waste sand and a preparation method to solve the problems existing in the prior art. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to propose a refractory material and a preparation method prepared using investment casting waste sand. The refractory material and the preparation method prepared using investment casting waste sand have the advantage of waste recycling and solve the problems existing in the prior art.
[0006] To achieve the purpose of the present invention, the present invention is implemented through the following technical scheme: a refractory material prepared by using investment casting waste sand, comprising the following materials in parts by weight: 50-60 parts of investment casting waste sand, 20-30 parts of metallurgical slag, 5-15 parts of rice husk ash, 10-15 parts of quartz sand, 2-5 parts of potassium titanate, 1-3 parts of zinc borate, 5-10 parts of expanded perlite, 12-14 parts of mullite, 10-15 parts of binder, 2-3 parts of plasticizer, 1-2 parts of oxidant, 0.5-1 part of defoamer, and 1-2 parts of enhancer.
[0007] A further improvement is that the binder is silicate cement, the plasticizer is bentonite, the oxidant is sodium nitrate, the defoamer is silicone oil, and the reinforcing agent is ceramic fiber.
[0008] A method for preparing a refractory material using investment casting waste sand comprises the following steps:
[0009] Step 1: Preparation and processing of basic materials
[0010] Prepare investment casting waste sand, metallurgical slag and rice husk ash, crush the investment casting waste sand and metallurgical slag together with a crusher, and after crushing, screen and process through a magnetic separation device to obtain a mixed material, and then add the mixed material into a ball mill, add deionized water, perform a first mixing, mix for 2 to 3 hours, add rice husk ash, and perform a second mixing for 30 to 60 minutes to obtain a first mixed material;
[0011] Step 2: Preparation and processing of additive materials
[0012] Prepare quartz sand, potassium titanate, zinc borate, expanded perlite, and mullite, add the mullite and quartz sand into a crusher, crush them, sieve them after crushing, then add them together with potassium titanate and zinc borate into a dryer, add them into a dry mixer after drying, add the expanded perlite, mix them, and obtain a second mixture;
[0013] Step 3: Mixing of materials
[0014] The first mixed material is added into an ultrasonic mixer, and the second mixed material is added, and then silicate cement is added for mixing. After mixing for 8 to 12 minutes, bentonite, sodium nitrate, silicone oil and ceramic fiber are added, and the mixing is continued for 40 to 50 minutes to obtain a total mixed material, and then a preliminary heat treatment is performed to obtain a material to be formed;
[0015] Step 4: Material Forming
[0016] The material to be formed is placed in a microwave sintering device and subjected to high-temperature sintering at 1300-1500°C for 3-5 hours. After high-temperature sintering, a heat treatment is performed again to obtain a refractory material.
[0017] A further improvement is that in the step 1, during the first mixing process, the speed of the ball mill is 330-430 r / min, and during the second mixing process, the speed of the ball mill is 200-250 min.
[0018] A further improvement is that in step 2, the particle size of the material after screening is 6 to 10 mm.
[0019] A further improvement is that in step 2, the drying temperature is 120-140° C. and the drying time is 30-50 min.
[0020] A further improvement is that in the step three, the specific method of the preliminary heat treatment is: the total mixture is placed in a molding mold, and the mold is placed in an oven, kept at 120-150°C for 20-30 minutes, and then increased by 30°C each time and maintained for 30 minutes, until it is increased to 270°C and maintained for 3-6 hours.
[0021] A further improvement is that in step 4, cooling is performed after high-temperature sintering. After the material is cooled to 300-400°C, it is placed in an annealing device, heated to 1000-1200°C, maintained for 1-2 hours, and then cooled to room temperature with the device.
[0022] The beneficial effects of the present invention are as follows: the present invention uses investment casting waste sand as the cornerstone, and combines it with metallurgical slag and rice husk ash as auxiliary materials, so that the basic part of the refractory material introduces the principle of waste recycling, while ensuring the performance of the refractory material, avoiding the pollution of the environment caused by the discharge of waste materials, and improving the resource utilization rate. At the same time, it can bring a certain reduction in the material cost of production. In addition, by adding materials such as quartz sand and potassium titanate, the performance of the finished refractory material is improved and its adaptability is enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the steps of the present invention. DETAILED DESCRIPTION
[0024] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0025] The following materials were purchased from commercial sources.
[0026] Embodiment 1
[0027] according to Figure 1 As shown, this embodiment proposes a refractory material prepared by using investment casting waste sand, including the following materials in parts by weight: 60 parts of investment casting waste sand, 20 parts of metallurgical slag, 15 parts of rice husk ash, 10 parts of quartz sand, 2 parts of potassium titanate, 1 part of zinc borate, 5 parts of expanded perlite, 12 parts of mullite, 10 parts of silicate cement (binder), 2 parts of bentonite (plasticizer), 1 part of sodium nitrate (oxidant), 0.5 parts of silicone oil (defoaming agent), and 1 part of ceramic fiber (reinforcement agent).
[0028] A method for preparing a refractory material using investment casting waste sand comprises the following steps:
[0029] Step 1: Preparation and processing of basic materials
[0030] According to the formula of the above materials, firstly, the basic materials are prepared and processed. The basic materials are the cornerstone of the present invention. According to the formula, the waste sand of investment casting, metallurgical slag and rice husk ash are accurately weighed, and the waste sand of investment casting and the metallurgical slag are crushed together by a crusher. The particle size after crushing is 12 mm. During the crushing process, the two materials are in a state of preliminary mixing. After crushing, they are screened by magnetic separation equipment to remove ferromagnetic impurities. After screening, the mixed material is obtained. Then, the waste sand of investment casting, metallurgical slag and rice husk ash are prepared. The waste sand of investment casting and the metallurgical slag are crushed together by a crusher. After crushing, , screened by magnetic separation equipment to obtain a mixed material, then added the mixed material into a ball mill, and added deionized water for the first mixing, mixed for 3 hours, added rice husk ash, mixed for a second time for 60 minutes, and obtained a first mixed material. Added into a ball mill, with deionized water as the medium, and mixed for the first time. The weight ratio of deionized water to the mixed material was 3:10 and mixed for 3 hours. Rice husk ash was added and mixed for a second time for 60 minutes to obtain the first mixed material. During the first mixing process, the ball mill speed was 330 r / min, and during the second mixing process, the ball mill speed was 200 min.
[0031] Step 2: Preparation and processing of additive materials
[0032] After the basic materials are prepared, the additive materials are prepared. The role of the additive materials is to improve the performance of the refractory materials. Then quartz sand, potassium titanate, zinc borate, expanded perlite and mullite are prepared. First, mullite and quartz sand are added to the crusher for crushing. After crushing, they are screened. The particle size of the screened material is 10mm. In this process, the quartz sand has been pre-cleaned and impurities removed. Then it is added to the dryer together with potassium titanate and zinc borate. It is dried at a drying temperature of 120°C and a drying time of 50 minutes to remove moisture. Then it is added to a dry mixer, and the expanded perlite is added and mixed to obtain a second mixture.
[0033] Step 3: Mixing of materials
[0034] After the completion of step two, the first mixture is added into an ultrasonic mixer, and the second mixture is added, and then silicate cement is added for mixing. In this step, ultrasonic dispersion technology is introduced for mixing to improve the mixing effect. After mixing for 12 minutes, bentonite, sodium nitrate, silicone oil and ceramic fiber are added, and mixing is continued for 40 minutes. After uniform mixing, the total mixture is obtained, and then a preliminary heat treatment is performed. The function of the preliminary heat treatment is preheating and drying. The specific method is: the total mixture is placed in a molding mold, and the mold is placed in an oven, and kept at 120°C for 30 minutes, and then the temperature is increased by 30°C each time and kept for 30 minutes until it is increased to 270°C and kept for 3 hours to obtain the material to be molded.
[0035] Step 4: Material Forming
[0036] After step three is completed, the material is cooled to room temperature (25±5°C), and then kept for 1 hour. Then, the material is placed in a microwave sintering device and sintered at 1300°C for 5 hours. In this embodiment, microwave technology is used for sintering. Microwave sintering is a sintering technology that uses microwave energy to directly heat materials. It has the characteristics of fast heating speed, high energy utilization rate, and low sintering temperature. At the same time, the sintering efficiency will be improved to a certain extent. After high-temperature sintering, a heat treatment is performed again. Specifically, the material is cooled after high-temperature sintering. After the material is cooled to 400°C, it is placed in an annealing device, heated to 1200°C, maintained for 1 hour, and then cooled to room temperature with the device to obtain a refractory material. In this embodiment, after a short period of high temperature, a heat treatment is performed again to enhance the performance of the refractory material. At the same time, in this process, after high-temperature sintering, the material is not completely cooled, but cooled to a certain temperature, and then high-temperature annealing is performed, which reduces the time for preheating the material.
[0037] Embodiment 2
[0038] according to Figure 1 As shown, this embodiment proposes a refractory material prepared by using investment casting waste sand, including the following materials in parts by weight: 50 parts of investment casting waste sand, 30 parts of metallurgical slag, 5 parts of rice husk ash, 15 parts of quartz sand, 5 parts of potassium titanate, 3 parts of zinc borate, 10 parts of expanded perlite, 14 parts of mullite, 15 parts of silicate cement (binder), 3 parts of bentonite (plasticizer), 2 parts of sodium nitrate (oxidant), 1 part of silicone oil (defoaming agent), and 2 parts of ceramic fiber (reinforcement agent).
[0039] A method for preparing a refractory material using investment casting waste sand comprises the following steps:
[0040] Step 1: Preparation and processing of basic materials
[0041] According to the formula of the above materials, firstly, the basic materials are prepared and processed. The basic materials are the cornerstone of the present invention. According to the formula, the waste sand of investment casting, metallurgical slag and rice husk ash are accurately weighed, and the waste sand of investment casting and the metallurgical slag are crushed together by a crusher. The particle size after crushing is 8mm. During the crushing process, the two materials are in a state of preliminary mixing. After crushing, they are screened by magnetic separation equipment to remove ferromagnetic impurities. After screening, the mixed material is obtained. Then, the waste sand of investment casting, metallurgical slag and rice husk ash are prepared. The waste sand of investment casting and the metallurgical slag are crushed together by a crusher. After crushing, The material to be mixed is screened by magnetic separation equipment to obtain the material to be mixed, which is then added to a ball mill and deionized water for the first mixing. The material is mixed for 2 hours, and rice husk ash is added for the second mixing for 30 minutes to obtain the first mixture. The material to be mixed is added to a ball mill with deionized water as the medium for the first mixing. The weight ratio of deionized water to the material to be mixed is 3:10. The material is mixed for 2 hours, and rice husk ash is added for the second mixing for 30 minutes to obtain the first mixture. During the first mixing process, the speed of the ball mill is 430 r / min, and during the second mixing process, the speed of the ball mill is 250 min.
[0042] Step 2: Preparation and processing of additive materials
[0043] After the basic materials are prepared, the additive materials are prepared. The role of the additive materials is to improve the performance of the refractory materials. Then quartz sand, potassium titanate, zinc borate, expanded perlite and mullite are prepared. First, mullite and quartz sand are added to the crusher for crushing. After crushing, they are screened. The particle size of the screened material is 6 mm. In this process, the quartz sand has been pre-cleaned and impurities removed. Then it is added to the dryer together with potassium titanate and zinc borate. It is dried at a drying temperature of 140°C and a drying time of 30 minutes to remove moisture. Then it is added to a dry mixer, and the expanded perlite is added and mixed to obtain a second mixture.
[0044] Step 3: Mixing of materials
[0045] After the completion of step two, the first mixture is added into an ultrasonic mixer, and the second mixture is added, and then silicate cement is added for mixing. In this step, ultrasonic dispersion technology is introduced for mixing, which is beneficial to improve the mixing effect. After mixing for 8 minutes, bentonite, sodium nitrate, silicone oil and ceramic fiber are added, and mixing is continued for 50 minutes. After uniform mixing, the total mixture is obtained, and then a preliminary heat treatment is performed. The function of the preliminary heat treatment is preheating and drying. The specific method is: the total mixture is placed in a molding mold, and the mold is placed in an oven, and kept at 150°C for 20 minutes, and then the temperature is increased by 30°C each time, and kept for 30 minutes, until it is increased to 270°C, and kept for 6 hours to obtain the material to be molded.
[0046] Step 4: Material Forming
[0047] After step three is completed, the material is cooled to room temperature (25±5°C), and then kept for 1 hour. Then, the material is placed in a microwave sintering device and sintered at 1500°C for 3 hours. In this embodiment, microwave technology is used for sintering. Microwave sintering is a sintering technology that uses microwave energy to directly heat materials. It has the characteristics of fast heating speed, high energy utilization rate, and low sintering temperature. At the same time, the sintering efficiency will be improved to a certain extent. After high-temperature sintering, a heat treatment is performed again. Specifically, the material is cooled after high-temperature sintering. After the material is cooled to 300°C, it is placed in an annealing device, heated to 1000°C, maintained for 2 hours, and then cooled to room temperature with the device to obtain a refractory material. In this embodiment, after a short period of high temperature, a heat treatment is performed again to enhance the performance of the refractory material. At the same time, in this process, after high-temperature sintering, the material is not completely cooled, but cooled to a certain temperature, and then high-temperature annealing is performed, which reduces the preheating time of the material.
[0048] Combining Example 1 and Example 2, the prepared refractory materials were placed in an induction furnace for testing, and the refractoriness was greater than 1950°C. At the same time, the room temperature compressive strength was tested using the method described in GB / T5072-2008, and the fracture toughness was tested using the SENB method known in the art, as shown in the following table:
[0049]
[0050]
[0051] In the present invention, waste sand from investment casting is used as the main raw material, and metallurgical slag and rice husk ash are used as auxiliary materials. Metallurgical slag contains a large amount of oxides, such as iron oxide, calcium oxide, etc., which can improve the refractoriness and mechanical strength of refractory materials. At the same time, industrial by-products are utilized to achieve the recycling of resources. Rice husk ash is rich in silicon dioxide and has good refractory properties, which can improve the thermal insulation performance and refractoriness of refractory materials.
[0052] Quartz sand, potassium titanate, zinc borate, expanded perlite and mullite are used as fillers to enhance the performance of the refractory materials. Quartz sand provides high refractoriness and chemical stability, potassium titanate improves the refractoriness and corrosion resistance of the refractory materials, zinc borate acts as a flame retardant to improve the fireproof performance of the refractory materials, expanded perlite provides a lightweight and porous structure, which helps to improve the thermal insulation performance of the refractory materials, and mullite provides high refractoriness and good thermal stability, which helps to improve the refractory performance of the refractory materials.
[0053] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A refractory material prepared using investment casting waste sand, characterized in that: The invention comprises the following materials in parts by weight: 50-60 parts of investment casting waste sand, 20-30 parts of metallurgical slag, 5-15 parts of rice husk ash, 10-15 parts of quartz sand, 2-5 parts of potassium titanate, 1-3 parts of zinc borate, 5-10 parts of expanded perlite, 12-14 parts of mullite, 10-15 parts of binder, 2-3 parts of plasticizer, 1-2 parts of oxidant, 0.5-1 parts of defoamer and 1-2 parts of reinforcing agent.
2. A refractory material and preparation method using investment casting waste sand according to claim 1, characterized in that: The binder is silicate cement, the plasticizer is bentonite, the oxidant is sodium nitrate, the defoamer is silicone oil, and the reinforcing agent is ceramic fiber.
3. The method for preparing a refractory material using investment casting waste sand as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Preparation and processing of basic materials Prepare investment casting waste sand, metallurgical slag and rice husk ash, crush the investment casting waste sand and metallurgical slag together with a crusher, and after crushing, screen and process through a magnetic separation device to obtain a mixed material, and then add the mixed material into a ball mill, add deionized water, perform a first mixing, mix for 2 to 3 hours, add rice husk ash, and perform a second mixing for 30 to 60 minutes to obtain a first mixed material; Step 2: Preparation and processing of additive materials Prepare quartz sand, potassium titanate, zinc borate, expanded perlite, and mullite, add the mullite and quartz sand into a crusher, crush them, sieve them after crushing, then add them together with potassium titanate and zinc borate into a dryer, add them into a dry mixer after drying, add the expanded perlite, mix them, and obtain a second mixture; Step 3: Mixing of materials The first mixed material is added into an ultrasonic mixer, and the second mixed material is added, and then silicate cement is added for mixing. After mixing for 8 to 12 minutes, bentonite, sodium nitrate, silicone oil and ceramic fiber are added, and the mixing is continued for 40 to 50 minutes to obtain a total mixed material, and then a preliminary heat treatment is performed to obtain a material to be formed; Step 4: Material Forming The material to be formed is placed in a microwave sintering device and subjected to high-temperature sintering at 1300-1500°C for 3-5 hours. After high-temperature sintering, a heat treatment is performed again to obtain a refractory material.
4. The method for preparing a refractory material using investment casting waste sand according to claim 3, characterized in that: In the step 1, during the first mixing process, the speed of the ball mill is 330-430 r / min, and during the second mixing process, the speed of the ball mill is 200-250 min.
5. The method for preparing a refractory material using investment casting waste sand according to claim 3, characterized in that: In the step 2, the particle size of the material after screening is 6 to 10 mm.
6. The method for preparing a refractory material using investment casting waste sand according to claim 3, characterized in that: In the step 2, the drying temperature is 120-140° C., and the drying time is 30-50 minutes.
7. The method for preparing a refractory material using investment casting waste sand according to claim 3, characterized in that: In the step three, the specific method of the preliminary heat treatment is: put the total mixture into a molding mold, and put the mold into an oven, keep it at 120-150°C for 20-30 minutes, then increase it by 30°C each time and keep it for 30 minutes, until it reaches 270°C and keep it for 3-6 hours.
8. The method for preparing a refractory material using investment casting waste sand according to claim 3, characterized in that: In the step 4, the material is cooled after high-temperature sintering. After the material is cooled to 300-400° C., it is placed in an annealing device, heated to 1000-1200° C., maintained for 1-2 hours, and then cooled to room temperature with the device.