Preparation method of novel light steel diagonal bracing wall body filling material

By using triethanolamine and dispersible latex powder to modify polystyrene particles in foam concrete and mixing them with recycled aggregate and gelling materials to form a filling material that wraps the cement slurry, the susceptibility of overflow and wall loss after pouring of foam concrete is solved. The problem of stability achieves a stable filling effect.

CN119080527APending Publication Date: 2024-12-06CHINA CONSTR SCI & IND WUHAN CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410991798.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional foam concrete is easily overflowed from the wire mesh after pouring, resulting in instability of the wall and cumbersome construction.

Method used

Using a new lightweight steel oblique wall filling material, the composite modifier is made by dissolving triethanolamine and dispersible latex powder in water, spraying it on the surface of polystyrene granule foam for hydrophilic modification, and Mix with recycled aggregate, gelling material and cellulose ether to form a mixed slurry that wraps the cement slurry to create a solid filler material.

Benefits of technology

This method makes the filling material not easy to overflow from the wire mesh, ensures the stability of the wall and the simplicity of construction, and meets the stability requirements of the filling material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080527A_ABST
    Figure CN119080527A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a novel light steel inclined strut wall body filling material, and relates to the technical field of building materials, the preparation method of the novel light steel inclined strut wall body filling material comprises the following steps: S10, dissolving triethanolamine and dispersible latex powder in 50% by mass of water to prepare a composite modifier, and adding the composite modifier into a stirrer to prepare the novel light steel inclined strut wall body filling material; uniformly spraying the mixture on the foam surface of the polyphenyl granules to perform hydrophilic modification on the surface of the polyphenyl granules, stirring for 1-3 minutes, adding the recycled aggregate, and stirring for 1-2 minutes to prepare mixed aggregate; s20, mixing a cementing material and cellulose ether in a stirrer for 1-3 minutes to prepare mixed powder, adding 50% by mass of the mixed powder into the mixed aggregate, and stirring for 1-3 minutes to wrap the surface of the aggregate with cement paste; s30, doping a water reducing agent into the residual 50% of water, and mixing the water reducing agent with the residual 50% of powder for 1-3 minutes to prepare mixed slurry; and S40, mixing the mixed slurry into the aggregate wrapped by the cement slurry, and stirring for 1-3 minutes to prepare the novel light steel diagonal bracing wall filling material. The preparation method has the beneficial effect that the stability of the prepared filling material is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and more particularly to a method for preparing a novel lightweight steel diagonal brace wall filling material. Background Art

[0002] Foamed concrete is a lightweight concrete that is characterized by the addition of stable foam (usually air foam) to the concrete, thus forming a large number of tiny pores. These pores can significantly reduce the density of foamed concrete, usually around 300kg / m 3 Up to 1600kg / m 3 This is much lighter than traditional concrete. Foam concrete has the characteristics of light weight, heat preservation, insulation, sound absorption and easy construction. It is suitable for occasions where it is necessary to reduce structural load or improve the thermal insulation and sound insulation performance of buildings. The main applications of foam concrete include but are not limited to:

[0003] Lightweight filling material: used to fill cavities such as walls, roofs, floors, etc.

[0004] Thermal and sound insulation materials: Due to its low density and good thermal insulation properties, it can be used for thermal and sound insulation layers of buildings.

[0005] Civil engineering applications: such as filling, filling deep pits, foundation reinforcement, etc.

[0006] Slope protection project: used for slope protection of river embankments, hillsides, etc.

[0007] However, traditional foam concrete slurry is prone to overflow from the mesh of the wire mesh after pouring, and its heavy weight can lead to problems such as wall instability. Summary of the invention

[0008] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a novel lightweight steel diagonal brace wall filling material, which solves the problem that the current foam concrete is easy to overflow from the mesh of the wire mesh after pouring, and the heavy weight causes the wall to become unstable and the construction is cumbersome, thereby ensuring the stability of the prepared filling material.

[0009] The technical solution adopted by the present invention to solve the technical problem is: a preparation method of a new type of lightweight steel diagonal brace wall filling material, the improvement of which is that the preparation method of the new type of lightweight steel diagonal brace wall filling material comprises the following steps:

[0010] S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, spraying the composite modifier evenly on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 1-3 minutes, and adding recycled aggregate and stirring for 1-2 minutes to prepare a mixed aggregate;

[0011] S20, mixing the gelling material and the cellulose ether in a mixer for 1-3 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to the mixed aggregate and stirring for 1-3 minutes to coat the surface of the aggregate with cement paste;

[0012] S30, adding the water reducing agent to the remaining 50% of the water, and mixing with the remaining 50% of the powder for 1-3 minutes to form a mixed slurry;

[0013] S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 1-3 minutes to prepare a new type of lightweight steel diagonal braced wall filling material.

[0014] Furthermore, in step S20, the cementitious material includes cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:1.

[0015] Furthermore, in step S10, the recycled aggregate is waste autoclaved aerated blocks and bricks that are crushed and screened by a crusher to obtain particles of less than 5 mm, the apparent density of the recycled aggregate is between 900 kg / m3 and 1100 kg / m3, and the mass ratio of the recycled aggregate to the cementitious material is 1:1.

[0016] Furthermore, the mass of the polystyrene particles accounts for 0.9%-1.4% of the mass of the gel material, and the particle size of the polystyrene particles is between 1-5 mm.

[0017] Furthermore, the mass of the polystyrene particles accounts for 1.0%-1.2% of the mass of the gel material, and the particle size of the polystyrene particles is between 1-5 mm.

[0018] Furthermore, in step S10, the mass of the triethanolamine accounts for 1%-3% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3%-4% of the mass of the polystyrene particles.

[0019] Furthermore, in step S10, the mass of the triethanolamine accounts for 2%-2.5% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3.2%-3.8% of the mass of the polystyrene particles.

[0020] Furthermore, in step S20, the cellulose ether is hydroxypropyl methyl cellulose ether, and the mass of the cellulose ether accounts for 0.5%-0.75% of the mass of the gelling material.

[0021] Furthermore, in step S20, the cellulose ether is hydroxypropyl methyl cellulose ether, and the mass of the cellulose ether accounts for 0.60%-0.70% of the mass of the gelling material.

[0022] Furthermore, in step S30, the water reducer is a polycarboxylic acid high-efficiency water reducer, and the mass of the water reducer accounts for 1%-2% of the mass of the cementitious material.

[0023] The beneficial effects of the present invention are as follows: triethanolamine and dispersible latex powder are first dissolved in 50% water by weight to prepare a composite modifier, which is evenly sprayed on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirred for 1-3 minutes, and recycled aggregate is added and stirred for 1-2 minutes to prepare a mixed aggregate; then, the gelling material and cellulose ether are mixed in a mixer for 1-3 minutes to prepare a mixed powder, and 50% of the mixed powder is added to the mixed aggregate and stirred for 1-3 minutes to coat the aggregate surface with cement slurry; then, the water reducer is added to the remaining 50% water and mixed with the remaining 50% powder for 1-3 minutes to prepare a mixed slurry; finally, the mixed slurry is added to the aggregate coated with cement slurry and stirred for 1-3 minutes to prepare a new lightweight steel diagonal brace wall filling material. The filling material prepared in this process can be formed in one time in combination with the steel wire mesh wall, and is not easy to overflow from the mesh of the steel mesh, thereby ensuring the stability of the prepared filling material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The present invention is an overall flow chart of a method for preparing a novel lightweight steel diagonal brace green grape filling material. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0026] The following will clearly and completely describe the concept, specific structure and technical effects of the present invention in combination with the embodiments and drawings, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. In addition, all the connection / connection relationships involved in the patent do not refer to the direct connection of components, but refer to the formation of a better connection structure by adding or reducing connection accessories according to the specific implementation situation. The various technical features in the invention can be combined interchangeably without conflicting with each other.

[0027] Embodiment 1:

[0028] Reference Figure 1 As shown, the present invention discloses a method for preparing a novel lightweight steel diagonal brace wall filling material, and the method for preparing the novel lightweight steel diagonal brace wall filling material comprises the following steps:

[0029] S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, spraying the composite modifier evenly on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 1-3 minutes, and adding recycled aggregate and stirring for 2 minutes to prepare a mixed aggregate; wherein the recycled aggregate is waste autoclaved aerated blocks and bricks that are crushed and screened by a crusher and have a particle size of less than 5 mm, and the apparent density of the recycled aggregate is 900 kg / m 3 -1100kg / m 3 The mass ratio of the recycled aggregate to the cementitious material is 1:1; the mass of the polystyrene particles accounts for 1.4% of the mass of the gel material, and the particle size of the polystyrene particles is between 1-5 mm; the mass of the triethanolamine accounts for 3% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 4% of the mass of the polystyrene particles.

[0030] S20, mixing a cementitious material and cellulose ether in a mixer for 2 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to a mixed aggregate and stirring for 2 minutes, so that the aggregate surface is coated with cement slurry; the cementitious material comprises cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:1; the cellulose ether is hydroxypropyl methylcellulose ether, and the mass of the cellulose ether accounts for 0.75% by weight of the cementitious material;

[0031] S30, adding a water reducer into the remaining 50% of the water, and mixing with the remaining 50% of the powder for 2 minutes to form a mixed slurry; the water reducer is a polycarboxylic acid high-efficiency water reducer, and the mass of the water reducer accounts for 2% of the mass of the cementitious material.

[0032] S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 2 minutes to prepare a new type of lightweight steel braced wall filling material.

[0033] In this embodiment, the material ratio is as follows: the cementitious material is 824.6g of cement, 247.4g of fly ash, and 82.5g of silica fume; the polystyrene particles account for 1.4% of the mass of the cementitious material; the cellulose ether accounts for 0.75% of the mass of the cementitious material, and the water reducer accounts for 2% of the mass of the cementitious material; the triethanolamine accounts for 3% of the mass of the polystyrene particles, and the dispersible latex powder accounts for 4% of the mass of the polystyrene particles; the filling material prepared by this ratio is subjected to a 28-day strength test, a mass water absorption test, and a density test, and the data obtained are: compressive strength 5MPa, mass water absorption 8.7%, and density 892kg / m 3 .

[0034] Embodiment 2:

[0035] Reference Figure 1As shown, the present invention discloses a method for preparing a novel lightweight steel diagonal brace wall filling material, and the method for preparing the novel lightweight steel diagonal brace wall filling material comprises the following steps:

[0036] S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, spraying the composite modifier evenly on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 2 minutes, and adding recycled aggregate and stirring for 2 minutes to prepare a mixed aggregate; wherein the recycled aggregate is waste autoclaved aerated blocks and bricks that are crushed and screened by a crusher to obtain particles of less than 5 mm, and the apparent density of the recycled aggregate is 900 kg / m 3 -1100kg / m 3 The mass ratio of the recycled aggregate to the cementitious material is 1:1; the mass of the polystyrene particles accounts for 1.0% of the mass of the gel material, and the particle size of the polystyrene particles is between 1-5 mm; the mass of the triethanolamine accounts for 1.5% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3.2% of the mass of the polystyrene particles.

[0037] S20, mixing a cementitious material and cellulose ether in a mixer for 2 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to a mixed aggregate and stirring for 2 minutes to coat the aggregate surface with cement slurry; the cementitious material comprises cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:1; the cellulose ether is hydroxypropyl methylcellulose ether, and the mass of the cellulose ether accounts for 0.55% by weight of the cementitious material;

[0038] S30, adding a water reducer into the remaining 50% of the water, and mixing with the remaining 50% of the powder for 2 minutes to form a mixed slurry; the water reducer is a polycarboxylic acid high-efficiency water reducer, and the mass of the water reducer accounts for 1.2% of the mass of the cementitious material.

[0039] S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 2 minutes to prepare a new type of lightweight steel braced wall filling material.

[0040] In this embodiment, the material ratio is as follows: the cementitious material is 824.6g of cement, 247.4g of fly ash, and 82.5g of silica fume; the polystyrene particles account for 1.0% of the mass of the cementitious material; the cellulose ether accounts for 0.55% of the mass of the cementitious material, and the water reducer accounts for 1.2% of the mass of the cementitious material; the triethanolamine accounts for 1.5% of the mass of the polystyrene particles, and the dispersible latex powder accounts for 3.2% of the mass of the polystyrene particles; the filling material prepared by this ratio is subjected to a 28-day strength test, a mass water absorption test, and a density test, and the data obtained are: compressive strength 9.2MPa, mass water absorption 6.6%, and density 988kg / m 3 .

[0041] Embodiment 3:

[0042] Reference Figure 1 As shown, the present invention discloses a method for preparing a novel lightweight steel diagonal brace wall filling material, and the method for preparing the novel lightweight steel diagonal brace wall filling material comprises the following steps:

[0043] S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, uniformly spraying the composite modifier on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 2 minutes, and adding recycled aggregate and stirring for 2 minutes to prepare a mixed aggregate; wherein the recycled aggregate is waste autoclaved aerated blocks and bricks crushed and screened by a crusher and having a size of less than 5 mm, the apparent density of the recycled aggregate is between 900kg / m3 and 1100kg / m3, and the mass ratio of the recycled aggregate to the gelling material is 1:1; the mass of the polystyrene particles accounts for 1.2% of the mass of the gelling material, and the particle size of the polystyrene particles is between 1 and 5 mm; the mass of the triethanolamine accounts for 2.0% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3.6% of the mass of the polystyrene particles.

[0044] S20, mixing a cementitious material and cellulose ether in a mixer for 2 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to a mixed aggregate and stirring for 2 minutes to coat the aggregate surface with cement slurry; the cementitious material comprises cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:1; the cellulose ether is hydroxypropyl methylcellulose ether, and the mass of the cellulose ether accounts for 0.60% by weight of the cementitious material;

[0045] S30, adding a water reducer into the remaining 50% of the water, and mixing with the remaining 50% of the powder for 2 minutes to form a mixed slurry; the water reducer is a polycarboxylic acid high-efficiency water reducer, and the mass of the water reducer accounts for 1.4% of the mass of the cementitious material.

[0046] S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 2 minutes to prepare a new type of lightweight steel braced wall filling material.

[0047] In this embodiment, the material ratio is as follows: the cementitious material is 824.6g of cement, 247.4g of fly ash, and 82.5g of silica fume; the polystyrene particles account for 1.2% of the mass of the cementitious material; the cellulose ether accounts for 0.60% of the mass of the cementitious material, and the water reducer accounts for 1.4% of the mass of the cementitious material; the triethanolamine accounts for 2.0% of the mass of the polystyrene particles, and the dispersible latex powder accounts for 3.6% of the mass of the polystyrene particles; the filling material prepared by this ratio is subjected to a 28-day strength test, a mass water absorption test, and a density test, and the data obtained are: compressive strength 8.8MPa, mass water absorption 7.3%, and density 948kg / m3 .

[0048] Embodiment 4:

[0049] Reference Figure 1 As shown, the present invention discloses a method for preparing a novel lightweight steel diagonal brace wall filling material, and the method for preparing the novel lightweight steel diagonal brace wall filling material comprises the following steps:

[0050] S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, uniformly spraying the composite modifier on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 2 minutes, and adding recycled aggregate and stirring for 2 minutes to prepare a mixed aggregate; wherein the recycled aggregate is waste autoclaved aerated blocks and bricks crushed and screened by a crusher and having a particle size of less than 5 mm, the apparent density of the recycled aggregate is between 900kg / m3 and 1100kg / m3, and the mass ratio of the recycled aggregate to the gelling material is 1:1; the mass of the polystyrene particles accounts for 1.3% of the mass of the gelling material, and the particle size of the polystyrene particles is between 1 and 5 mm; the mass of the triethanolamine accounts for 2.5% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3.8% of the mass of the polystyrene particles.

[0051] S20, mixing a cementitious material and cellulose ether in a mixer for 2 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to a mixed aggregate and stirring for 2 minutes to coat the aggregate surface with cement slurry; the cementitious material comprises cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:1; the cellulose ether is hydroxypropyl methylcellulose ether, and the mass of the cellulose ether accounts for 0.65% by weight of the cementitious material;

[0052] S30, adding a water reducer into the remaining 50% of the water, and mixing with the remaining 50% of the powder for 2 minutes to form a mixed slurry; the water reducer is a polycarboxylic acid high-efficiency water reducer, and the mass of the water reducer accounts for 1.8% of the mass of the cementitious material.

[0053] S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 2 minutes to prepare a new type of lightweight steel braced wall filling material.

[0054] In this embodiment, the material ratio is as follows: the cementitious material is 824.6g of cement, 247.4g of fly ash, and 82.5g of silica fume; the polystyrene particles account for 1.3% of the mass of the cementitious material; the cellulose ether accounts for 0.65% of the mass of the cementitious material, and the water reducer accounts for 1.8% of the mass of the cementitious material; the triethanolamine accounts for 2.5% of the mass of the polystyrene particles, and the dispersible latex powder accounts for 3.8% of the mass of the polystyrene particles; the filling material prepared by this ratio is subjected to a 28-day strength test, a mass water absorption test, and a density test, and the data obtained are: compressive strength 6.6MPa, mass water absorption 8.0%, and density 923kg / m 3 .

[0055] Embodiment 5:

[0056] Reference Figure 1 As shown, the present invention discloses a method for preparing a novel lightweight steel diagonal brace wall filling material, and the method for preparing the novel lightweight steel diagonal brace wall filling material comprises the following steps:

[0057] S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, uniformly spraying the composite modifier on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 2 minutes, and adding recycled aggregate and stirring for 2 minutes to prepare a mixed aggregate; wherein the recycled aggregate is waste autoclaved aerated blocks and bricks crushed and screened by a crusher and having a particle size of less than 5 mm, the apparent density of the recycled aggregate is between 900kg / m3 and 1100kg / m3, and the mass ratio of the recycled aggregate to the gelling material is 1:1; the mass of the polystyrene particles accounts for 0.9% of the mass of the gelling material, and the particle size of the polystyrene particles is between 1 and 5 mm; the mass of the triethanolamine accounts for 1% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3% of the mass of the polystyrene particles.

[0058] S20, mixing a cementitious material and cellulose ether in a mixer for 2 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to a mixed aggregate and stirring for 2 minutes to coat the aggregate surface with cement slurry; the cementitious material comprises cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:1; the cellulose ether is hydroxypropyl methylcellulose ether, and the mass of the cellulose ether accounts for 0.5% by weight of the cementitious material;

[0059] S30, adding a water reducer into the remaining 50% of the water and mixing it with the remaining 50% of the powder for 2 minutes to form a mixed slurry; the water reducer is a polycarboxylic acid high-efficiency water reducer, and the mass of the water reducer accounts for 1% of the mass of the cementitious material.

[0060] S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 2 minutes to prepare a new type of lightweight steel braced wall filling material.

[0061] In this embodiment, the material ratio is as follows: the cementitious material is 824.6g of cement, 247.4g of fly ash, and 82.5g of silica fume; the polystyrene particles account for 0.9% of the mass of the cementitious material; the cellulose ether accounts for 0.5% of the mass of the cementitious material, and the water reducer accounts for 1% of the mass of the cementitious material; the triethanolamine accounts for 1% of the mass of the polystyrene particles, and the dispersible latex powder accounts for 3% of the mass of the polystyrene particles; the filling material prepared by this ratio is subjected to a 28-day strength test, a mass water absorption test, and a density test, and the data obtained are: compressive strength 9.6MPa, mass water absorption 6.2%, and density 1045kg / m 3 .

[0062] When the present invention is specifically implemented, the traditional polystyrene particle foam concrete is also tested for 28-day strength, mass water absorption, and density, and the on-site pouring conditions are observed. The data obtained are: 28-day strength 7MPa, mass water absorption 7.6%, density 953kg / m3, and the physical properties meet the requirements of the specifications. However, during the pouring process, the slurry overflows from the mesh of the steel mesh, which cannot meet the use requirements. When the filling material is prepared using the ratios in Example 1 and Example 2, the steel mesh wall can be formed in one step, and it is not easy to overflow from the mesh of the steel mesh, thereby ensuring the stability of the prepared filling material.

[0063] The above is a specific description of the preferred implementation of the present invention, but the invention is not limited to the embodiments. Those skilled in the art can make various equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.

Claims

1. A method for preparing a novel lightweight steel braced wall filling material, characterized in that: The preparation method of the novel lightweight steel diagonal brace wall filling material comprises the following steps: S10, dissolving triethanolamine and dispersible latex powder in 50% by weight of water to prepare a composite modifier, spraying the composite modifier evenly on the surface of polystyrene particle foam to hydrophilically modify the surface of the polystyrene particle, stirring for 1-3 minutes, and adding recycled aggregate and stirring for 1-2 minutes to prepare a mixed aggregate; S20, mixing the gelling material and the cellulose ether in a mixer for 1-3 minutes to prepare a mixed powder, and adding 50% by weight of the mixed powder to the mixed aggregate and stirring for 1-3 minutes to coat the surface of the aggregate with cement paste; S30, adding the water reducing agent to the remaining 50% of the water, and mixing with the remaining 50% of the powder for 1-3 minutes to form a mixed slurry; S40, adding the mixed slurry into the aggregate wrapped by the cement slurry and stirring for 1-3 minutes to prepare a new type of lightweight steel diagonal braced wall filling material.

2. The method for preparing a lightweight steel braced wall filling material according to claim 1, characterized in that: In step S20, the cementitious material includes cement, fly ash and silica fume, and the mass ratio of the cement, fly ash and silica fume is 10:3:

1.

3. The method for preparing a lightweight steel braced wall filling material according to claim 2, characterized in that: In step S10, the recycled aggregate is waste autoclaved aerated blocks and bricks that are crushed and sieved by a crusher to obtain particles with a size of less than 5 mm. The apparent density of the recycled aggregate is 900 kg / m 3 -1100kg / m 3 The mass ratio of recycled aggregate to cementitious material is 1:

1.

4. The method for preparing a lightweight steel braced wall filling material according to claim 2, characterized in that: The mass of the polystyrene particles accounts for 0.9%-1.4% of the mass of the gel material, and the particle size of the polystyrene particles is between 1-5 mm.

5. The method for preparing a lightweight steel braced wall filling material according to claim 4, characterized in that: The mass of the polystyrene particles accounts for 1.0%-1.2% of the mass of the gel material, and the particle size of the polystyrene particles is between 1-5 mm.

6. The method for preparing a lightweight steel braced wall filling material according to claim 4, characterized in that: In step S10, the mass of the triethanolamine accounts for 1%-3% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3%-4% of the mass of the polystyrene particles.

7. The method for preparing a lightweight steel braced wall filling material according to claim 6, characterized in that: In step S10, the mass of the triethanolamine accounts for 2%-2.5% of the mass of the polystyrene particles; the mass of the dispersible latex powder accounts for 3.2%-3.8% of the mass of the polystyrene particles.

8. The method for preparing a light steel diagonal brace green grape filling material according to claim 1, characterized in that: In step S20, the cellulose ether is hydroxypropyl methyl cellulose ether, and the mass of the cellulose ether accounts for 0.5%-0.75% of the mass of the gelling material.

9. The method for preparing a light steel diagonal brace green grape filling material according to claim 8, characterized in that: In step S20, the cellulose ether is hydroxypropyl methyl cellulose ether, and the mass of the cellulose ether accounts for 0.60%-0.70% of the mass of the gelling material.

10. The method for preparing a lightweight steel braced wall filling material according to claim 1, characterized in that: In step S30, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent, and the mass of the water reducing agent accounts for 1%-2% of the mass of the cementitious material.

Citation Information

Patent Citations

  • Preparation method of modified waste EPS (expanded polystyrene) lightweight aggregate coated with silicate

    CN107954649A

  • Slurry-coated reinforced permeable recycled concrete and preparation method thereof

    CN113493333A

  • Anti-crack foam light soil and preparation method thereof

    CN113666682A

  • Recycled concrete of reinforced recycled aggregate based on composite slurry modification and preparation method of recycled concrete

    CN117088655A

  • Cement composition using regenerated aggregate

    JP1999180756A