Sulfur modified mesoporous carbon immobilized transition metal catalyst, preparation method thereof and application of sulfur modified mesoporous carbon immobilized transition metal catalyst in dicyclopentadiene polymerization reaction
By modifying the mesoporous carbon solid-load transition metal catalyst, the problem of two-component catalysts being easily deactivated in the air and low utilization rate of physically embedded catalysts is solved, and catalysis with high activity, high stability and high utilization rate is achieved Effectively, suitable for industrial production of dicyclopentadiene polymerization.
Patent Information
- Application Number
- CN202411415552.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
Existing two-component catalysts are prone to deactivate in air, have harsh usage conditions, and have low utilization rate of physically embedded catalysts, which affects the stability and properties of dicyclopentadiene polymerization.
The sulfur-modified mesoporous carbon solid-load transition metal catalyst is adopted to form a stable catalyst system to improve the activity and stability of the catalyst through the sulfur source modification of the mesoporous carbon support and transition metal oxychloride complex. The utilization rate of the catalyst is improved by the high specific surface area and pore structure of the mesoporous carbon support.
It achieves high activity, high stability and high utilization rate of the catalyst, is suitable for industrial production, and is stable to air and trace water, improving the mechanical properties of dicyclopentadiene polymerization.
Smart Images

Figure BDA0005079335290000161
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of supported catalysts, and specifically relates to a sulfur-modified mesoporous carbon-supported transition metal catalyst and a preparation method and application thereof, and in particular relates to the application of the sulfur-modified mesoporous carbon-supported transition metal catalyst in the polymerization reaction of dicyclopentadiene. Background Art
[0002] Dicyclopentadiene is a byproduct of petroleum cracking to produce ethylene and a light benzene fraction produced by coal coking. It contains two unsaturated double bonds in its structure, and both rings containing unsaturated double bonds can undergo ring-opening metathesis polymerization. Dicyclopentadiene has broad application prospects in the fields of fine chemicals and polymer chemistry. Its polymers have been widely used in industries such as energy conservation and environmental protection, and lightweight materials due to their excellent performance.
[0003] Ring-opening metathesis polymerization is a key step in the polydicyclopentadiene molding process. The catalyst is the core of ring-opening metathesis polymerization. The activity and stability of the catalyst will affect the structure and performance of the product and also determine the industrial application value of the catalyst.
[0004] The first catalyst to be used in the ring-opening metathesis polymerization of cycloolefins was a two-component catalyst. The two-component catalyst is mainly composed of a main catalyst and a co-catalyst. The main catalyst is a compound of certain transition metals such as W, Mo, Ta, Re, Ru, Ti, etc. The co-catalyst is a metal organic compound such as diethylaluminum monochloride and triethylaluminum. Among them, the main catalyst plays a decisive role in the formation of metal carbene. The co-catalyst can promote the accelerated formation of metal carbene, and different co-catalysts play a decisive role in the activity of metal carbene complexes. Since transition metal halides such as tungsten and molybdenum are easily oxidized in the air, substances such as phenols and alcohols with strong electron donating ability are often required. Among them, the transition metal provides an empty orbital, and the ligand can provide a considerable lone pair of electrons, using the hydroxyl group and the metal center to form a relatively stable complex. Due to the different steric hindrances and electron donating abilities of different ligands, the stability and activity of the catalyst are also different. Such stable complexes cannot catalyze the polymerization of the reaction alone, and a co-catalyst is required to expose the metal carbene active center through an in-situ reaction. The metathesis reaction of cycloolefins may release a large amount of heat, resulting in a sharp rise in temperature, which often leads to implosion, increasing the difficulty of industrial application and making the surface of the product less beautiful. In order to meet the requirements of industrial operation, a regulator is often added to the system to delay the reaction polymerization time.
[0005] The complexes of WCl6 and MoCl5 with substituted hindered phenols are the main catalysts currently used in industry, which can catalyze the ring-opening metathesis polymerization of dicyclopentadiene. The electronic effect and steric hindrance of substituted hindered phenol ligands are the key factors determining the activity and stability of the catalyst. After WCl6 and MoCl5 are coordinated with substituted hindered phenols, they can improve their own stability and the stability of the metal carbene complex, thereby improving the catalytic efficiency of the catalyst.
[0006] In the prior art, some researchers have used polystyrene and molecular sieve-loaded tungsten catalysts to catalyze the polymerization of dicyclopentadiene. The activity of polystyrene-loaded catalysts is higher than that of unloaded catalysts, and the stability is better. The catalysts loaded with molecular sieves also show higher activity. However, polystyrene-loaded tungsten catalysts are physically embedded, and the catalyst utilization rate is low. In addition, there are some problems with the dispersion of molecular sieves in dicyclopentadiene, which will affect the properties of polydicyclopentadiene.
[0007] The two-component catalyst is relatively cheap and highly active, and has been used as the main catalyst for the industrial production of polycycloolefin materials. However, since the two-component catalyst is easily deactivated when exposed to air, it is difficult for it to exist stably in the air, the use conditions are relatively harsh, and it is difficult to store it, which in turn increases the cost of catalyst application. And because it is difficult to determine the location of the metal carbene active center, there has been no major research progress in the bimetallic catalyst since its discovery. Summary of the invention
[0008] In view of this, the object of the present invention is to provide a sulfur-modified mesoporous carbon-supported transition metal catalyst and a preparation method and application thereof. The sulfur-modified mesoporous carbon-supported transition metal catalyst of the present invention is used as a main catalyst for catalyzing the polymerization of dicyclopentadiene, and the resulting catalyst system has high activity, good stability, high catalyst utilization rate, and good dispersibility in dicyclopentadiene.
[0009] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0010] A method for preparing a sulfur-modified mesoporous carbon-supported transition metal catalyst comprises the following steps:
[0011] (1) using a sulfur source to perform a doping modification pretreatment on the mesoporous carbon support to obtain a sulfur-modified mesoporous carbon support;
[0012] (2) Under oxygen-free and water-free conditions, utilizing the thiol groups on the surface of the sulfur-modified mesoporous carbon support to carry out a coordination treatment with an active component to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst;
[0013] The active component includes a transition metal oxychloride complex.
[0014] Preferably, the transition metal chloride is at least one of WCl6, MoCl5 and RuCl4.
[0015] Preferably, the mesoporous carbon carrier is prepared by a colloidal template method;
[0016] More preferably, the template substance used in the colloidal template method is aluminum salt, the carbon source is a soluble carbon-containing compound, and the mass ratio of the carbon source to the template substance is 0.1 to 20;
[0017] Particularly preferably, the aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride, and aluminum acetate; the carbon source is selected from at least one of soluble starch, sucrose, glucose, and fructose;
[0018] Most preferably, the preparation method of the mesoporous carbon carrier is:
[0019] S1. Take aluminum salt and dissolve it in distilled water to obtain an aluminum salt solution;
[0020] S2. Take a carbon source and dissolve it in distilled water to obtain a carbon source solution;
[0021] S3. Mix the aluminum salt solution and the carbon source solution, heat in a water bath at 80 to 100° C., and stir for 1 to 6 hours to obtain a mixed solution;
[0022] S4. The mixed solution is heated in a water bath at a temperature of 90 to 100° C. and evaporated to dryness to obtain a precursor;
[0023] S5. The precursor is first placed in a muffle furnace, calcined at 250-350°C for 4-6h, and then placed in a tube furnace, calcined at 750-850°C for 6-10h under an inert atmosphere to obtain a powder;
[0024] S6. The powder is placed in an acid solution, heated and stirred in an oil bath, the oil bath temperature is 100 to 120 ° C, the stirring time is 10 to 16 hours, and then filtered and dried in an oven at 80 to 120 ° C for 1 to 16 hours to obtain mesoporous carbon;
[0025] The acid solution is at least one of concentrated hydrochloric acid or concentrated nitric acid. In the acid solution, the molar ratio of the acid to distilled water is 1:0.5 to 1:1.5, and the mass ratio of the powder to the acid in the acid solution is 1:5 to 1:40.
[0026] Preferably, the process of step (1) is one of (1-1), (1-2), and (1-3):
[0027] (1-1) firstly, the sulfur source and the mesoporous carbon support are mixed and ground for 30 to 60 minutes, and then, under the protection of an inert atmosphere, the mixture is placed in a tube furnace and activated at 400 to 1000° C. for 2 to 8 hours to obtain a sulfur-modified mesoporous carbon support;
[0028] The sulfur source is at least one of sulfur, thiourea and sulfur trioxide, and the molar ratio of sulfur in the sulfur source to the mesoporous carbon carrier is 0.001 to 0.1:1;
[0029] (1-2) first placing the mesoporous carbon support in a tubular furnace and bubbling with an inert atmosphere to bring sulfur source vapor into the mesoporous carbon support bed to activate the mesoporous carbon support and obtain a sulfur-modified mesoporous carbon support;
[0030] The sulfur source is at least one of dimethyl sulfide, carbon disulfide, thiodiphenyl ether, diphenyl sulfide, thioethanol, ethyl sulfide, thioether, thiophenol, and mercaptan;
[0031] The bubbling time is 1 to 3 hours, the tube furnace temperature is 400 to 1000° C., and the activation time is 1 to 3 hours;
[0032] (1-3) placing the mesoporous carbon support in a tube furnace, mixing an inert atmosphere with a gaseous sulfur source, allowing the mixture to enter a mesoporous carbon support bed, activating the mesoporous carbon support, and obtaining a sulfur-modified mesoporous carbon support;
[0033] The sulfur source is at least one of sulfur dioxide, hydrogen sulfide, and carbon oxysulfide;
[0034] The volume ratio of the inert atmosphere to the gaseous sulfur source is 100:1 to 10:1, the temperature of the tube furnace is 400 to 1000° C., and the activation time is 2 to 8 hours.
[0035] Preferably, in step (2), the ligands of the transition metal oxychloride complex are independently a first ligand, a second ligand and a third ligand;
[0036] The first ligand includes at least one of trimethyl carbinol and 2,6-di-tert-butyl-p-cresol; the second ligand includes at least one of p-nonylphenol, 6-tert-butyl-2,4-dimethylphenol, diamylhydroquinone, polyphenol ligands, bisphenol ligands, 1,3-benzenediol and pyrogallol; the third ligand includes at least one of 2,3-pentanedione and diacetyl methane ester ligands;
[0037] More preferably, the process of step (2) is:
[0038] (2-1) Under the protection of an inert atmosphere, dissolving a transition metal chloride in a solvent to obtain a reaction solution;
[0039] The molar ratio of the transition metal chloride to the solvent is 1:8 to 1:14, and the solvent is at least one of carbon disulfide, benzene, butyl ether, and carbon tetrachloride;
[0040] (2-2) adding the first ligand, the second ligand and the third ligand to the reaction solution in sequence to obtain an active component mixed solution;
[0041] The molar ratio of the first ligand to the transition metal chloride is 0.1 to 1.5:1; the molar ratio of the second ligand to the transition metal chloride is 0.09 to 0.6:1; the molar ratio of the third ligand to the transition metal chloride is 0.09 to 0.6:1;
[0042] (2-3) adding a sulfur-modified mesoporous carbon support to the active component mixture, heating the mixture under inert atmosphere, the reaction temperature being 40 to 70° C., the reaction time being 0.5 to 3 h, to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst;
[0043] The mass ratio of the active component mixed solution to the sulfur-modified mesoporous carbon carrier is 15:1 to 1:1.
[0044] The present invention also provides a sulfur-modified mesoporous carbon-supported transition metal catalyst prepared by the above preparation method.
[0045] The present invention also provides a catalyst system for the polymerization of dicyclopentadiene, the catalyst system comprising a main catalyst and a co-catalyst, the main catalyst being a sulfur-modified mesoporous carbon-supported transition metal catalyst, and the co-catalyst being an organic aluminum compound.
[0046] The present invention also provides the use of the above catalyst system in the polymerization reaction of dicyclopentadiene, comprising the following steps:
[0047] (1) Under an inert atmosphere, the main catalyst and the co-catalyst are placed in the material to be polymerized to prepare material A and material B respectively;
[0048] The material to be polymerized includes cyclopentadiene monomer;
[0049] (2) mixing the material A and the material B and subjecting them to thermal polymerization to obtain polydicyclopentadiene;
[0050] The polymerization temperature is 60-90°C.
[0051] Preferably, the molar ratio of dicyclopentadiene to the co-catalyst in the A material is 7 to 20:1; the molar ratio of dicyclopentadiene to the main catalyst in the B material is 600 to 1100:1, and the molar amounts of the main catalyst and the co-catalyst are calculated based on the molar amounts of the metal elements.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] The present invention provides a method for preparing a sulfur-modified mesoporous carbon-supported transition metal catalyst, which comprises modifying a mesoporous carbon carrier with a sulfur source, mixing the obtained sulfur-modified mesoporous carbon carrier with an active component mixed solution for immobilization, and obtaining a sulfur-modified mesoporous carbon-supported transition metal catalyst. The present invention uses a sulfur source to perform a modification pretreatment on the mesoporous carbon carrier, so that sulfur doping is formed in the mesoporous carbon carrier. Such sulfur doping can form thiol groups, which can be chelated and coordinated with transition metal ions to form stable complexes, which is beneficial to improving the stability and catalytic activity of the catalyst; in addition, the specific surface area of the mesoporous carbon source prepared by the present invention is 1800 to 2000 m 2 / g. The surface has a large number of carbonyl, carboxyl, and pyrone groups that can act as Lewis bases and effectively regulate the electronic effect in the catalyst. Sulfur doping effectively regulates the electron cloud density around the transition metal active center, thereby regulating the activity of the catalyst, having a suitable polymerization operation window, and facilitating industrial production.
[0054] In the sulfur-modified mesoporous carbon-supported transition metal catalyst provided by the present invention, transition metal ions and thiol groups on the surface of the mesoporous carbon carrier form coordination bonds, and the obtained complex has a stable structure, thereby improving the activity and stability of the catalyst, while the ordinary supported tungsten catalyst is only physically embedded without chemical bonding, and the structure of the catalyst is unstable; furthermore, the mesoporous carbon carrier used in the present invention has a very high specific surface area, can load more active components, and has a high catalyst utilization rate, while the surface area of the ordinary supported catalyst is also small, and the catalyst utilization rate is low.
[0055] The sulfur-modified mesoporous carbon carrier of the present invention can play a role in regulating the electron cloud density and increase the operating window; further, the mesoporous carbon carrier provided by the present invention has a developed pore system, which is helpful for the monomer to be transmitted to the central ion, and further improves the utilization rate of the central ion. In addition, the dispersibility of the mesoporous carbon carrier in the dicyclopentadiene monomer is also much better than other carriers, and will not affect the properties of the polydicyclopentadiene product. Further, the sulfur-modified mesoporous carbon carrier can not only stabilize the metal center, but also effectively disperse active species, expose more active sites, improve the utilization rate of the catalyst, and improve the polymerization efficiency. Further, dicyclopentadiene can be polymerized in the pores of the mesoporous carbon carrier, and at this time, the mesoporous carbon carrier can play an overall supporting role, effectively improving the various mechanical properties of polydicyclopentadiene.
[0056] The sulfur-modified mesoporous carbon-supported transition metal catalyst system for dicyclopentadiene polymerization of the present invention comprises a main catalyst and a co-catalyst which are separately packaged, wherein the main catalyst is a sulfur-modified mesoporous carbon-supported transition metal catalyst. The sulfur-modified mesoporous carbon-supported transition metal catalyst provided by the present invention has high activity and stability, and is stable to air and a trace amount of water. When used as a main catalyst for dicyclopentadiene polymerization, it has a suitable polymerization operation window and is convenient for industrial production.
[0057] The method for preparing a dicyclopentadiene polymer material of the present invention comprises dispersing a main catalyst and a co-catalyst in an equal volume of a material to be polymerized containing a dicyclopentadiene monomer to obtain a component A and a component B, and then mixing the component A and the component B for polymerization. The method provided by the present invention is easy to operate, and the obtained product has high mechanical properties. DETAILED DESCRIPTION
[0058] In order to further understand the present invention, preferred embodiments of the present invention are described below. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0059] The method for preparing the sulfur-modified mesoporous carbon-supported transition metal catalyst of the present invention comprises the following steps:
[0060] (1) using a sulfur source to perform a doping modification pretreatment on the mesoporous carbon support to obtain a sulfur-modified mesoporous carbon support;
[0061] (2) Under oxygen-free and water-free conditions, the thiol groups on the surface of the sulfur-modified mesoporous carbon support are used to carry out a coordination treatment with the active component to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst;
[0062] The active component includes a transition metal oxychloride complex.
[0063] In the present invention, a mesoporous carbon carrier is prepared by a colloidal template method, the template material is an aluminum salt, and the carbon source is a soluble carbon-containing compound. The mass ratio of the carbon source to the template material is 0.1 to 20 times, preferably 1 to 5. The aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride, and aluminum acetate, preferably aluminum nitrate. The carbon source is at least one of soluble starch, sucrose, glucose, and fructose, preferably soluble starch. The aluminum salt and the carbon source are respectively configured into solutions and mixed evenly under a water bath, preferably taking the aluminum salt, dissolving it in 50 to 100 mL of distilled water, stirring for 1 to 3 hours, and obtaining an aluminum salt solution; preferably taking the carbon source, dissolving it in 50 to 100 mL of distilled water, stirring for 1 to 3 hours, and obtaining a carbon source solution; and obtaining a mixed solution. The water bath temperature is 80 to 100°C, preferably 90°C, and the stirring time is 3 to 6 hours, preferably 4 to 5 hours. The mixed solution is heated in a water bath and evaporated to dryness to obtain a precursor, and the water bath temperature is 90 to 100°C, preferably 95°C. The precursor is placed in a muffle furnace and calcined at 250-350°C for 4-6 hours, preferably at 280-310°C and for 5 hours. The precursor is placed in a tube furnace and calcined in an argon or high-purity nitrogen atmosphere, preferably in an argon atmosphere; the calcination temperature is 750-850°C, preferably 800°C; the calcination time is 6-10 hours, preferably 7-8 hours. The calcined powder is placed in an acid solution, heated and stirred in an oil bath, and dried to obtain a mesoporous carbon carrier; the mass ratio of the powder to the acid in the acid solution is 1:5-1:40, preferably 1:10-1:20; the acid solution is at least one of concentrated hydrochloric acid and concentrated nitric acid, preferably concentrated hydrochloric acid. In the acid solution, the molar ratio of acid to distilled water is 1:0.5-1:1.5, preferably 1:0.8-1:1.1; the oil bath temperature is 100-120°C, preferably 110-115°C; the stirring time is 10-16h, preferably 11-14h. The above sample is placed in an oven at 80-120°C for 1-16h, preferably the drying temperature is 110-120°C, and the drying time is 11-13h.
[0064] In the present invention, the mesoporous carbon carrier is doped and modified by using a sulfur source in three ways:
[0065] Method 1: First, the sulfur source and the mesoporous carbon carrier are mixed and ground, and then placed in a tube furnace under the protection of an inert atmosphere for activation for 2 to 8 hours to obtain a sulfur-modified mesoporous carbon carrier;
[0066] The molar ratio of the sulfur source to the mesoporous carbon carrier is 0.001 to 0.1:1, preferably 0.01 to 0.08:1; the sulfur source is at least one of sulfur, thiourea, and sulfur trioxide, preferably one of sulfur and thiourea; the mixing and grinding time is 30 to 60 minutes, preferably 40 to 50 minutes; the inert atmosphere is high-purity nitrogen or argon, preferably under argon protection; the activation temperature is 400 to 1000°C, preferably 700 to 900°C; the activation time is 2 to 8 hours, preferably 5 to 6 hours.
[0067] Method 2: firstly, the mesoporous carbon support is placed in a tubular furnace, and an inert atmosphere is used for bubbling to bring the sulfur source vapor into the mesoporous carbon support bed to activate the mesoporous carbon support, thereby obtaining a sulfur-modified mesoporous carbon support;
[0068] The sulfur source is at least one of dimethyl sulfide, carbon disulfide, thiodiphenyl ether, diphenyl sulfide, thioethanol, ethyl sulfide, thioether, thiophenol, and thiol; preferably one of dimethyl sulfide, carbon disulfide and thioether; the inert atmosphere is high-purity nitrogen or argon, preferably argon; the bubbling time is 1 to 3 hours, preferably 1.5 to 2.5 hours; the tube furnace temperature is 400 to 1000° C., preferably 700 to 850° C.; the activation time is 1 to 3 hours, preferably 1.5 to 2.5 hours;
[0069] Method three: placing a mesoporous carbon carrier in a tubular furnace, mixing an inert atmosphere with a gaseous sulfur source, allowing the mixture to enter a mesoporous carbon carrier bed, activating the mesoporous carbon carrier, and obtaining a sulfur-modified mesoporous carbon carrier; the inert atmosphere is high-purity nitrogen or argon, preferably argon; the sulfur source is at least one of sulfur dioxide, hydrogen sulfide, and carbon oxysulfide, preferably at least one of sulfur dioxide and carbon oxysulfide; the volume ratio of the inert atmosphere to the gaseous sulfur source is 100:1 to 10:1, preferably 50:1 to 30:1; the temperature of the tubular furnace is 400 to 1000°C, preferably 700 to 800°C; the activation time is 2 to 8 hours, preferably 2.5 to 4 hours.
[0070] In the present invention, the steps of using the thiol groups on the surface of the sulfur-modified mesoporous carbon carrier and the active components for a coordinated treatment to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst are as follows:
[0071] (1) Under the protection of an inert atmosphere, a transition metal chloride is dissolved in a solvent to obtain a reaction solution, wherein the transition metal chloride comprises one or more of WCl6, MoCl5 and RuCl4, preferably at least one of WCl6 and MoCl5; the solvent is one or more of carbon disulfide, benzene, butyl ether and carbon tetrachloride, preferably at least one of carbon disulfide and carbon tetrachloride; the molar ratio of the transition metal chloride to the solvent is 1:8 to 1:14, preferably 1:9 to 1:13.
[0072] (2) adding a first ligand, a second ligand, and a third ligand to the reaction solution in sequence to obtain an active component mixed solution;
[0073] The first ligand includes trimethyl carbinol and / or 2,6-di-tert-butyl-p-cresol, preferably 2,6-di-tert-butyl-p-cresol; the second ligand includes one or more of p-nonylphenol, 6-tert-butyl-2,4-dimethylphenol, diamylhydroquinone, polyphenol ligands, bisphenol ligands, 1,3-benzenediol and pyrogallol, preferably at least one of nonylphenol and 6-tert-butyl-2,4-dimethylphenol; the third ligand includes at least one of 2,3-pentanedione and diacetyl methane ester ligands;
[0074] The molar ratio of the first ligand to the transition metal chloride is 0.1 to 1.5:1, preferably 0.5 to 0.9:1; the molar ratio of the second ligand to the transition metal chloride is 0.09 to 0.6:1, preferably 0.09 to 0.3:1; the molar ratio of the third ligand to the transition metal chloride is 0.09 to 0.6:1, preferably 0.3 to 0.5:1;
[0075] In the present invention, the use of ligands to coordinate active metal species can appropriately reduce the intrinsic activity of transition metals. During use, the main catalyst can be appropriately prevented from directly initiating monomer polymerization and causing explosion polymerization, which promotes the improvement of catalyst stability.
[0076] (3) adding a sulfur-modified mesoporous carbon support to the active component mixture, and heating the mixture under an inert atmosphere to react to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst;
[0077] The mass ratio of the active component mixture to the sulfur-modified mesoporous carbon carrier is 15:1 to 1:1, preferably 9:1 to 1:1. The inert atmosphere is high-purity nitrogen or argon, preferably argon; the reaction temperature is 40 to 70°C, preferably 50 to 60°C; the reaction time is 0.5 to 3 hours, preferably 1.5 to 2 hours. During the reaction, the transition metal ions are chelated and coordinated with the thiol groups on the sulfur-modified mesoporous carbon carrier, thereby immobilizing the active metal species on the carrier surface. The mesoporous carbon carrier with a large specific surface area can also effectively disperse the active species and expose more active sites. Thus, a sulfur-modified mesoporous carbon immobilized transition metal catalyst with high activity and high stability is obtained.
[0078] In the present invention, the liquid obtained after the sulfur-modified mesoporous carbon carrier and the active component mixed solution are mixed and reacted is the suspension of the sulfur-modified carbon-based catalyst described in the present invention, which can be directly used as a catalyst.
[0079] The present invention also provides a sulfur-modified mesoporous carbon-supported transition metal catalyst prepared by the preparation method described in the above scheme, comprising a sulfur-modified mesoporous carbon carrier and an active component supported on the sulfur-modified mesoporous carbon carrier. The active component comprises a transition metal oxychloride complex; the ligands in the transition metal oxychloride complex comprise the first ligand, the second ligand and the third ligand described in the above scheme, and the metal central ion in the active component forms a stable complex structure with the thiol group on the surface of the mesoporous carbon carrier.
[0080] The present invention also provides a dicyclopentadiene polymerization catalyst system, which comprises a main catalyst and a co-catalyst, wherein the main catalyst is a sulfur-modified mesoporous carbon-supported transition metal catalyst, and the co-catalyst is an organic aluminum compound.
[0081] The present invention also provides an application of the above catalyst system in a polymerization reaction of dicyclopentadiene, comprising the following steps:
[0082] (1) Under an inert atmosphere, the main catalyst and the co-catalyst are placed in the material to be polymerized to prepare material A and material B respectively;
[0083] The material to be polymerized includes cyclopentadiene monomer;
[0084] (2) rapidly mixing the material A and the material B, transferring them to a mold at 70 to 85° C. under a pressure of 1 to 2 MPa within 20 to 40 seconds, and cross-linking and polymerizing the mixture within 1 to 5 minutes to obtain polydicyclopentadiene;
[0085] The polymerization temperature is preferably 70 to 85°C.
[0086] In the present invention, the inert atmosphere is high-purity nitrogen or argon, preferably argon. The molar ratio of dicyclopentadiene to the co-catalyst in material A is 7 to 20:1; the molar ratio of dicyclopentadiene to the main catalyst in material B is 600 to 1100:1; the molar amounts of the main catalyst and the co-catalyst are calculated based on the mass of the metal element.
[0087] The terms used in the present invention generally have the meanings commonly understood by those of ordinary skill in the art, unless otherwise specified. In order to enable those of ordinary skill in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with the embodiments. High purity in the present invention refers to a purity greater than 99.9%.
[0088] The present invention is further described below with reference to the examples.
[0089] Example 1
[0090] Weigh 24g of aluminum nitrate into a three-necked flask, add 50mL of distilled water, stir to dissolve, and obtain an aluminum nitrate solution. Weigh 10.5g of soluble starch, add 50mL of distilled water, stir to dissolve, and obtain a starch solution. Under 90℃ water bath conditions, drip the aluminum nitrate solution and starch solution into the three-necked flask in parallel, stir and react for 2h, and obtain a mixed solution.
[0091] The mixed solution was poured into a 200 mL ceramic dry pot and heated in a water bath at a temperature of 90-100° C. The mixture was stirred and evaporated to dryness to obtain a precursor.
[0092] The precursor was pre-calcined at 250 °C in a muffle furnace for 5 h and then ground into fine powder using an agate mortar.
[0093] Weigh 3 g of powder and place it in a tube furnace. Under argon protection, calcine it at 780°C for 6.5 h.
[0094] Weigh 1.5 g of the calcined powder and put it into a conical flask. Prepare a hydrochloric acid solution by mixing concentrated hydrochloric acid and distilled water in a molar ratio of 1:1.1. Weigh 30 g of the hydrochloric acid solution and add it into the conical flask, and stir at 115°C for 13 h.
[0095] Filter and wash with 6000 mL of distilled water.
[0096] The filter cake was placed in an oven at 115°C and dried for 12 hours to obtain mesoporous carbon C1. After testing, the specific surface area of the obtained mesoporous carbon was 1991m 2 / g.
[0097] Example 2
[0098] Weigh 24g of aluminum nitrate into a three-necked flask, add 50mL of distilled water, and stir to dissolve. Weigh 24g of soluble starch, add 100mL of distilled water, and stir to dissolve. In a 90℃ water bath, slowly drip the aluminum nitrate solution and starch solution into the three-necked flask in parallel, and stir to react for 2h.
[0099] The reaction solution was poured into a 200 mL ceramic dry pot, heated in a water bath, and evaporated to dryness.
[0100] The dried precursor was pre-calcined in a muffle furnace at 250 °C for 5 h and then ground into fine powder using an agate mortar.
[0101] After grinding, 3 g of the powder was weighed and placed in a tube furnace and calcined at 780 °C for 6.5 h under argon gas protection.
[0102] Weigh 1.5g of the calcined powder and put it into a conical flask. Prepare a hydrochloric acid solution by mixing concentrated hydrochloric acid and water in a molar ratio of 1:1.1. Weigh 30g of the hydrochloric acid solution and add it into the conical flask. Stir at 115℃ for 13h.
[0103] The above was filtered and washed with 6000 mL of distilled water.
[0104] The filter cake was placed in an oven at 115°C and dried for 12 hours to obtain mesoporous carbon C2. After testing, the specific surface area of the obtained mesoporous carbon was 1880 m 2 / g.
[0105] Example 3
[0106] Weigh 24g of aluminum nitrate into a three-necked flask, add 50mL of distilled water, and stir to dissolve. Weigh 36g of soluble starch, add 100mL of distilled water, and stir to dissolve. In a 90℃ water bath, slowly drip the aluminum nitrate solution and starch solution into the three-necked flask in parallel, and stir to react for 2h.
[0107] The reaction solution was poured into a 200 mL ceramic dry pot, heated in a water bath, and evaporated to dryness.
[0108] The dried precursor was pre-calcined in a muffle furnace at 250 °C for 5 h and then ground into fine powder using an agate mortar.
[0109] After grinding, 3 g of the powder was weighed and placed in a tube furnace and calcined at 780 °C for 6.5 h under argon gas protection.
[0110] Weigh 1.5g of the calcined powder and put it into a conical flask. Prepare a hydrochloric acid solution by mixing concentrated hydrochloric acid and water in a molar ratio of 1:1.1. Weigh 30g of the hydrochloric acid solution and add it into the conical flask. Stir at 115℃ for 13h.
[0111] The above was filtered and washed with 6000 mL of distilled water.
[0112] The filter cake was placed in an oven at 115°C and dried for 12 hours to obtain mesoporous carbon C3. After testing, the specific surface area of the obtained mesoporous carbon was 1845 m 2 / g.
[0113] Example 4
[0114] Weigh 0.65 g of sulfur and 5 g of mesoporous carbon C1, mix them evenly, and grind them in an agate mortar for 45 min.
[0115] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 700°C for 5 hours under argon protection.
[0116] Sulfur-modified mesoporous carbon SJKC1 was obtained.
[0117] Example 5
[0118] Weigh 0.65 g of sulfur and 5 g of mesoporous carbon C1, mix them evenly, and grind them in an agate mortar for 45 min.
[0119] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 800°C for 5 hours under argon protection.
[0120] Sulfur-modified mesoporous carbon SJKC2 was obtained.
[0121] Example 6
[0122] Weigh 0.65 g of sulfur and 5 g of mesoporous carbon C1, mix them evenly, and grind them in an agate mortar for 45 min.
[0123] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 900°C for 5 hours under argon protection.
[0124] Sulfur-modified mesoporous carbon SJKC3 was obtained.
[0125] Example 7
[0126] Weigh 0.9 g of sulfur and 5 g of mesoporous carbon C2, mix them evenly, and grind them in an agate mortar for 45 min.
[0127] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 800°C for 5 hours under argon protection.
[0128] Sulfur-modified mesoporous carbon SJKC4 was obtained.
[0129] Example 8
[0130] Weigh 0.65 g of thiourea and 5 g of mesoporous carbon C1, mix them evenly, and grind them in an agate mortar for 45 min.
[0131] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 700°C for 5 hours under argon protection.
[0132] Sulfur-modified mesoporous carbon SJKC5 was obtained.
[0133] Example 9
[0134] Weigh 0.65 g of thiourea and 5 g of mesoporous carbon C1, mix them evenly, and grind them in an agate mortar for 45 min.
[0135] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 800°C for 5 hours under argon protection.
[0136] Sulfur-modified mesoporous carbon SJKC6 was obtained.
[0137] Example 10
[0138] Weigh 0.65 g of thiourea and 5 g of mesoporous carbon C1, mix them evenly, and grind them in an agate mortar for 45 min.
[0139] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 900°C for 5 hours under argon protection.
[0140] Sulfur-modified mesoporous carbon SJKC7 was obtained.
[0141] Embodiment 11
[0142] Weigh 0.9 g of thiourea and 5 g of mesoporous carbon C3, mix them evenly, and grind them in an agate mortar for 45 min.
[0143] The mixed powder was placed in a quartz tube, which was placed in a tube furnace and calcined at 800°C for 5 hours under argon protection.
[0144] Sulfur-modified mesoporous carbon SJKC8 was obtained.
[0145] Example 12
[0146] Weigh 5 g of mesoporous carbon C1, put it in a quartz tube, and place it in a tube furnace.
[0147] Measure 2 mL of carbon disulfide and place it in a 10 mL two-necked bottle.
[0148] Argon was introduced into a two-necked bottle containing carbon disulfide at a flow rate of 10 mL / min, and the gas was exhausted from the other outlet and introduced into a quartz tube.
[0149] The tube furnace was programmed to heat up at a rate of 5°C / min and calcined at 800°C for 2h.
[0150] Sulfur-modified mesoporous carbon SJKC9 was obtained.
[0151] Embodiment 13
[0152] Weigh 5 g of mesoporous carbon C1, put it in a quartz tube, and place it in a tube furnace.
[0153] Adjust the sulfur dioxide gas flow rate to 1 mL / min. Adjust the argon gas flow rate to 40 mL / min.
[0154] The two gases flow into the quartz tube in parallel.
[0155] The tube furnace was programmed to heat up at a rate of 5°C / min and calcined at 800°C for 3h.
[0156] Sulfur-modified mesoporous carbon SJKC10 was obtained.
[0157] Embodiment 14
[0158] (1) Under argon protection, weigh 5g WCl6 and put it into a 100mL three-necked flask, add 5mL carbon tetrachloride and 10mL dehydrated toluene, heat and stir at 30℃ for 20min until it is completely dissolved.
[0159] (2) Add 2 g of 2,6-di-tert-butyl-p-cresol, 0.5 mL of nonylphenol, and 0.5 mL of 2,3-pentanedione to the above solution. Heat and stir at 50°C for 40 min.
[0160] (3) Add 2 g of sulfur-modified mesoporous carbon SJKC1 to the above solution, introduce argon at a flow rate of 20 mL / min, and heat to 55 °C for 2 h.
[0161] The sulfur-modified mesoporous carbon-supported W catalyst was obtained. The sulfur-modified mesoporous carbon-supported W catalyst was diluted to a tungsten content of 0.1 mol / L and named W-SJKC1.
[0162] According to the preparation method of this embodiment, the sulfur-modified mesoporous carbon-supported tungsten catalysts of embodiments 5-7 can be prepared respectively: W-SJKC2, W-SJKC3, and W-SJKC4.
[0163] Embodiment 15
[0164] (1) Under argon protection, weigh 5g WCl6 and put it into a 100mL three-necked flask, add 5mL carbon tetrachloride and 10mL dehydrated toluene, heat and stir at 30℃ for 20min until it is completely dissolved.
[0165] (2) Add 2 g of 2,6-di-tert-butyl-p-cresol, 0.5 mL of nonylphenol, and 0.5 mL of 2,3-pentanedione to the above solution. Heat and stir at 50°C for 40 min.
[0166] (3) Add 2 g of thiourea-modified mesoporous carbon SJKC5 to the above solution, introduce argon at a flow rate of 20 mL / min, and heat to 55 °C for 2 h.
[0167] The sulfur-modified mesoporous carbon-supported W catalyst was obtained. The sulfur-modified mesoporous carbon-supported W catalyst was diluted to a tungsten content of 0.1 mol / L and named W-SJKC5.
[0168] According to the preparation method of this embodiment, the thiourea-modified mesoporous carbon-supported tungsten catalysts of embodiments 9-11 can be prepared respectively: W-SJKC6, W-SJKC7, and W-SJKC8.
[0169] Example 16
[0170] (1) Under argon protection, weigh 5g WCl6 and put it into a 100mL three-necked flask, add 5mL carbon tetrachloride and 10mL dehydrated toluene, heat and stir at 30℃ for 20min until it is completely dissolved.
[0171] (2) Add 2 g of 2,6-di-tert-butyl-p-cresol, 0.5 mL of nonylphenol, and 0.5 mL of 2,3-pentanedione to the above solution. Heat and stir at 50°C for 40 min.
[0172] (3) Add 2 g of sulfur-modified mesoporous carbon SJKC9 to the above solution, introduce argon at a flow rate of 20 mL / min, and heat to 55 °C for 2 h.
[0173] The sulfur-modified mesoporous carbon-supported W catalyst was obtained. The sulfur-modified mesoporous carbon-supported W catalyst was diluted to a tungsten content of 0.1 mol / L and named W-SJKC9.
[0174] Embodiment 17
[0175] (1) Under argon protection, weigh 5g WCl6 and put it into a 100mL three-necked flask, add 5mL carbon tetrachloride and 10mL dehydrated toluene, heat and stir at 30℃ for 20min until it is completely dissolved.
[0176] (2) Add 2 g of 2,6-di-tert-butyl-p-cresol, 0.5 mL of nonylphenol, and 0.5 mL of 2,3-pentanedione to the above solution. Heat and stir at 50°C for 40 min.
[0177] (3) Add 2 g of sulfur-modified mesoporous carbon SJKC10 to the above solution, introduce argon at a flow rate of 20 mL / min, and raise the temperature to 55 °C for reaction for 2 h.
[0178] The sulfur-modified mesoporous carbon-supported W catalyst was obtained. The sulfur-modified mesoporous carbon-supported W catalyst was diluted to a tungsten content of 0.1 mol / L and named W-SJKC10.
[0179] Embodiment 18
[0180] Measure 3 mL of diethylaluminum monochloride, place it in a flat-bottom centrifuge tube, add 30 mL of dicyclopentadiene, seal it, and ultrasonicate it for 30 minutes to obtain material A.
[0181] 3 mL of the sulfur-modified mesoporous carbon tungsten-supported catalyst (W-SJKC1) prepared in Example 14 was weighed and placed in a flat-bottom centrifuge tube. 30 mL of dicyclopentadiene was added, and the tube was sealed and ultrasonicated for 30 min to obtain component B.
[0182] Material A and material B are mixed together, injected into a mold preheated to 70° C., and cured to form a cross-linked solid to obtain polydicyclopentadiene.
[0183] According to the preparation method of Example 18, the corresponding B materials are prepared with the sulfur-modified mesoporous carbon-supported W catalysts of other series prepared in Examples 14 to 17; the A materials are prepared according to the method of Example 18; and the corresponding polydicyclopentadiene is obtained by polymerization according to the polymerization method of Example 18. The mechanical properties of polydicyclopentadiene are shown in Table 1 (W-SJKC1-10).
[0184] According to the preparation method of material B in Example 18, material B was prepared with W-SJKC6 as a catalyst, and then exposed to air for 24 hours. Material A was prepared according to the method of preparing material A in Example 18. Dicyclopentadiene polymerization was carried out according to the polymerization method of Example 18. The mechanical properties of polydicyclopentadiene are shown in Table 1 (W-SJKC6-1).
[0185]
[0186] It can be seen from the above examples that the sulfur-modified mesoporous carbon-supported transition metal catalyst provided by the present invention has high activity and stability, and is used as a main catalyst to initiate the ring-opening metathesis polymerization of dicyclopentadiene, and the product has good mechanical properties. In addition, the sulfur-modified mesoporous carbon-supported transition metal catalyst provided by the present invention has a simple preparation method, low production cost, can be mass-produced, and has good application prospects.
[0187] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a sulfur-modified mesoporous carbon-supported transition metal catalyst, characterized in that: The following steps are involved: (1) using a sulfur source to perform a doping modification pretreatment on the mesoporous carbon support to obtain a sulfur-modified mesoporous carbon support; (2) Under oxygen-free and water-free conditions, utilizing the thiol groups on the surface of the sulfur-modified mesoporous carbon support to carry out a coordination treatment with an active component to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst; The active component includes a transition metal oxychloride complex.
2. The method for preparing the sulfur-modified mesoporous carbon-supported transition metal catalyst according to claim 1, characterized in that: The transition metal chloride is at least one of WCl6, MoCl5 and RuCl4; And / or, the ligands of the transition metal oxychloride complex are independently a first ligand, a second ligand and a third ligand; The first ligand includes at least one of trimethylcarbinol and 2,6-di-tert-butyl-p-cresol; the second ligand includes at least one of p-nonylphenol, 6-tert-butyl-2,4-dimethylphenol, diamylhydroquinone, polyphenol ligands, bisphenol ligands, 1,3-benzenediol and pyrogallol; the third ligand includes at least one of 2,3-pentanedione and diacetyl methane ester ligands.
3. The method for preparing the sulfur-modified mesoporous carbon-supported transition metal catalyst according to claim 1, characterized in that: The mesoporous carbon carrier is prepared by a colloidal template method; The template material used in the colloidal template method is an aluminum salt, and the aluminum salt is selected from at least one of aluminum nitrate, aluminum chloride, and aluminum acetate; The carbon source used in the colloidal template method is a soluble carbon-containing compound, and the carbon source is selected from at least one of soluble starch, sucrose, glucose, and fructose; The mass ratio of the carbon source to the template material is 0.1-20.
4. The method for preparing the sulfur-modified mesoporous carbon-supported transition metal catalyst according to claim 3, characterized in that: The preparation method of the mesoporous carbon carrier is: S1. Take aluminum salt and dissolve it in distilled water to obtain an aluminum salt solution; S2. Take a carbon source and dissolve it in distilled water to obtain a carbon source solution; S3. Mix the aluminum salt solution and the carbon source solution, heat in a water bath at 80 to 100° C., and stir for 1 to 6 hours to obtain a mixed solution; S4. The mixed solution is heated in a water bath at a temperature of 90 to 100° C. and evaporated to dryness to obtain a precursor; S5. The precursor is first placed in a muffle furnace, calcined at 250-350°C for 4-6h, and then placed in a tube furnace, calcined at 750-850°C for 6-10h under an inert atmosphere to obtain a powder; S6. The powder is placed in an acid solution, heated and stirred in an oil bath, the oil bath temperature is 100 to 120 ° C, the stirring time is 10 to 16 hours, and then filtered and dried in an oven at 80 to 120 ° C for 1 to 16 hours to obtain mesoporous carbon; The acid solution is at least one of concentrated hydrochloric acid or concentrated nitric acid. In the acid solution, the molar ratio of the acid to distilled water is 1:0.5 to 1:1.5, and the mass ratio of the powder to the acid in the acid solution is 1:5 to 1:
40.
5. The method for preparing the sulfur-modified mesoporous carbon-supported transition metal catalyst according to claim 1, characterized in that: The process of step (1) is one of (1-1), (1-2), and (1-3): (1-1) firstly, the sulfur source and the mesoporous carbon support are mixed and ground for 30 to 60 minutes, and then, under the protection of an inert atmosphere, the mixture is placed in a tube furnace and activated at 400 to 1000° C. for 2 to 8 hours to obtain a sulfur-modified mesoporous carbon support; The sulfur source is at least one of sulfur, thiourea and sulfur trioxide, and the molar ratio of sulfur in the sulfur source to the mesoporous carbon carrier is 0.001 to 0.1:1; (1-2) first placing the mesoporous carbon support in a tubular furnace and bubbling with an inert atmosphere to bring sulfur source vapor into the mesoporous carbon support bed to activate the mesoporous carbon support and obtain a sulfur-modified mesoporous carbon support; The sulfur source is at least one of dimethyl sulfide, carbon disulfide, thiodiphenyl ether, diphenyl sulfide, thioethanol, ethyl sulfide, thioether, thiophenol, and mercaptan; The bubbling time is 1 to 3 hours, the tube furnace temperature is 400 to 1000° C., and the activation time is 1 to 3 hours; (1-3) placing the mesoporous carbon support in a tube furnace, mixing an inert atmosphere with a gaseous sulfur source, allowing the mixture to enter a mesoporous carbon support bed, activating the mesoporous carbon support, and obtaining a sulfur-modified mesoporous carbon support; The sulfur source is at least one of sulfur dioxide, hydrogen sulfide, and carbon oxysulfide; The volume ratio of the inert atmosphere to the gaseous sulfur source is 100:1 to 10:1, the temperature of the tube furnace is 400 to 1000° C., and the activation time is 2 to 8 hours.
6. The method for preparing the sulfur-modified mesoporous carbon-supported transition metal catalyst according to claim 1, characterized in that: The process of step (2) is as follows: (2-1) Under the protection of an inert atmosphere, dissolving a transition metal chloride in a solvent to obtain a reaction solution; The molar ratio of the transition metal chloride to the solvent is 1:8 to 1:14, the solvent is at least one of carbon disulfide, benzene, butyl ether, and carbon tetrachloride; the transition metal chloride is at least one of WCl6, MoCl5, and RuCl4; (2-2) adding the first ligand, the second ligand and the third ligand to the reaction solution in sequence to obtain an active component mixed solution; The first ligand includes at least one of trimethyl carbinol and 2,6-di-tert-butyl-p-cresol; the second ligand includes at least one of p-nonylphenol, 6-tert-butyl-2,4-dimethylphenol, diamylhydroquinone, polyphenol ligands, bisphenol ligands, 1,3-benzenediol and pyrogallol; the third ligand includes at least one of 2,3-pentanedione and diacetyl methane ester ligands; The molar ratio of the first ligand to the transition metal chloride is 0.1 to 1.5:1; the molar ratio of the second ligand to the transition metal chloride is 0.09 to 0.6:1; the molar ratio of the third ligand to the transition metal chloride is 0.09 to 0.6:1; (2-3) adding a sulfur-modified mesoporous carbon support to the active component mixture, heating the mixture under inert atmosphere, the reaction temperature being 40 to 70° C., the reaction time being 0.5 to 3 h, to obtain a sulfur-modified mesoporous carbon-supported transition metal catalyst; The mass ratio of the active component mixed solution to the sulfur-modified mesoporous carbon carrier is 15:1 to 1:
1.
7. A sulfur-modified mesoporous carbon-supported transition metal catalyst prepared according to the preparation method according to any one of claims 1 to 6.
8. A catalyst system for the polymerization of dicyclopentadiene, the catalyst system comprising a main catalyst and a co-catalyst, characterized in that: The main catalyst is the sulfur-modified mesoporous carbon-supported transition metal catalyst as described in claim 7, and the co-catalyst is an organic aluminum compound.
9. Use of the catalyst system for dicyclopentadiene polymerization according to claim 8 in dicyclopentadiene polymerization reaction, characterized in that: The following steps are involved: (1) Under an inert atmosphere, the main catalyst and the co-catalyst are placed in the material to be polymerized to prepare material A and material B respectively; The material to be polymerized includes cyclopentadiene monomer; (2) mixing the material A and the material B and performing thermal polymerization to obtain polydicyclopentadiene; The polymerization temperature is 60-90°C.
10. Use of the catalyst system for dicyclopentadiene polymerization according to claim 9 in the preparation of dicyclopentadiene polymeric materials, characterized in that: The molar ratio of dicyclopentadiene to the co-catalyst in the A material is 7-20:1; the molar ratio of dicyclopentadiene to the main catalyst in the B material is 600-1100:1, and the molar amounts of the main catalyst and the co-catalyst are calculated based on metal elements.