Production method of polymer
By setting multiple inlets in the container, removing solvents with steam and recovering hot water, directly contacting the solvent with the solvent, the problems of high energy consumption and polymer loss in the water-definition condensation process are solved, and the energy consumption and loss are significantly reduced. , improves heat exchange efficiency.
Patent Information
- Application Number
- CN202411227368.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
The existing water-based condensation process has high energy consumption and polymer loss in the production of synthetic rubber, mainly due to the high solvent vaporization temperature and the large amount of gas-phase entrained glue, which leads to high energy consumption and partial polymer loss.
By setting multiple inlets in the container, the solvent is removed by steam and the hot water is recovered, the temperature of the solvent vapor phase is reduced, the water content is reduced, and the recycled hot water is directly in contact with the solvent vapor, improving heat exchange efficiency, reducing energy consumption and polymerization Loss of things.
It effectively reduces steam and energy consumption, reduces polymer loss, improves energy utilization efficiency, and significantly reduces the temperature of the solvent vapor phase and the amount of glue entrainment.
Smart Images

Figure CN119080986A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer preparation, and in particular relates to a method for producing a polymer. Background Art
[0002] At present, synthetic rubber is mostly prepared by solution polymerization, and the obtained synthetic rubber solution is separated from the polymer and solvent by a hydrolysis coagulation process (i.e., the solution is condensed by contact with steam and / or hot water). In this process, the evaporation separation of the solvent completely relies on steam and other heat sources, accounting for about 60% of the energy consumption in the production process of synthetic rubber.
[0003] In addition to synthetic rubber, polymer solutions obtained from other solution polymerization reactions also mostly use a water precipitation coagulation process to separate the polymer from the solvent. In this process, the polymer solution comes into contact with a heat source such as steam and / or hot water in a coagulation kettle, the solvent vaporizes, and the precipitated polymer particles are distributed in the water phase to form colloid water. The colloid water is then separated from the water by screening, extruder, etc. to obtain the polymer.
[0004] In order to improve the efficiency of heat and mass transfer, slow down or avoid the accumulation of glue in the coagulation kettle, and reduce energy consumption, the industry has made a variety of optimizations to the water separation and coagulation process, including the use of multiple kettles in series, differentiated operation of each kettle, and the recycling of hot water separated from the gel particles and water. Because the first kettle of the coagulation kettle bears the largest workload of organic solvent vaporization and separation, the optimization of the first kettle has been studied the most, including setting the polymer solution inlet position at the liquid phase or gas phase position of the coagulation kettle; setting the steam inlet at the gas phase or liquid phase position of the coagulation kettle, etc. At present, the more common setting of the first kettle of the coagulation kettle in the industry is: part of the steam is introduced into the liquid phase; the polymer solution and steam and circulating hot water are mixed and then sprayed downward from the gas phase of the coagulation kettle. Even so, the current water separation and coagulation kettle still has the problem of high temperature of the solvent volatilization gas phase carrying water vapor and high amount of glue entrained in the gas phase, resulting in high production energy consumption and partial polymer loss. Summary of the invention
[0005] In order to improve the above technical problems, the present invention provides a method for producing a polymer, which can effectively reduce energy consumption and reduce polymer loss. Specifically, the present invention provides the following solution:
[0006] A method for producing a polymer, the method comprising:
[0007] removing the solvent from the mixture containing the polymer and the solvent in a container under the action of steam to obtain a polymer / hot water mixture phase and a solvent gas phase;
[0008] Dehydrating the polymer / hot water mixture discharged from the container to obtain recycled hot water and a polymer / hot water mixture with reduced water content;
[0009] The recovered hot water is returned to the container, wherein part or all of the recovered hot water returned to the container directly contacts with the solvent gas.
[0010] According to an embodiment of the present invention, the method specifically comprises:
[0011] (1) adding a mixture containing a polymer and a solvent and steam into a container, removing the solvent under the action of the steam, and obtaining a polymer / hot water mixture phase and a solvent gas phase;
[0012] Wherein, the container comprises at least three inlets, the first inlet is arranged in the solvent gas phase for adding hot water; the second inlet is used for adding a mixture containing a polymer and a solvent, or a mixture containing a polymer, a solvent and water (from recycled hot water and / or steam); the third inlet is arranged in the polymer / hot water mixture phase for adding steam; the first inlet is located above the second inlet;
[0013] (2) dehydrating the polymer / hot water mixture discharged from the container to obtain recovered hot water and a polymer / hot water mixture with reduced water content;
[0014] (3) adding part or all of the recovered hot water in step (2) into the container from the first inlet so as to directly contact the hot water with the solvent gas.
[0015] According to an embodiment of the present invention, in step (3), when part of the recovered hot water is added to the container from the first inlet, another part of the recovered hot water is mixed with the mixture containing the polymer and the solvent and then added to the container from the second inlet.
[0016] According to an embodiment of the present invention, in the mixture containing a polymer and a solvent, the polymer content is 3-30wt%, for example, 3wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt% or 30wt%.
[0017] According to an embodiment of the present invention, the polymer is at least one of cis-1,4-dimethylbutyl rubber, solution-polymerized styrene-butadiene rubber, styrene-butadiene-styrene block copolymer or its hydrogenated product, styrene-isoprene-styrene block copolymer or its hydrogenated product, hydrogenated nitrile-butadiene rubber, halogenated butyl rubber, polyisoprene rubber, and acrylonitrile-butadiene-styrene. Exemplarily, it is selected from brominated butyl rubber.
[0018] According to an embodiment of the present invention, the solvent refers to an organic solvent having a boiling point below 100°C. For example, the solvent is selected from at least one of the following organic solvents having a boiling point below 100°C: saturated alkane solvents such as butane, pentane, cyclopentane, hexane, cyclohexane, heptane, halogenated hydrocarbons such as methyl chloride, dichloromethane, chloroform, ethyl chloride, and aromatic solvents such as benzene.
[0019] According to an embodiment of the present invention, part of the steam is mixed with the mixture containing the polymer and the solvent and then added to the container, and another part of the steam is added to the container alone. Exemplarily, in step (1), part of the steam is mixed with the mixture containing the polymer and the solvent and then added to the container from the second inlet, and another part of the steam is added to the container from the third inlet alone.
[0020] Alternatively, steam is added directly to the container. Exemplarily, in step (1), steam is added to the container from the third inlet.
[0021] According to an embodiment of the present invention, part of the recovered hot water is added to the container from the first inlet, another part of the recovered hot water, part of the steam and the mixture containing the polymer and the solvent are mixed and then added to the container from the second inlet, and another part of the steam is added to the container alone from the third inlet.
[0022] According to an embodiment of the present invention, the pressure of the steam entering the container is 0.2-4 MPa.
[0023] According to an embodiment of the present invention, in step (1), a distributor (specifically a porous distributor; illustratively, the shape of the porous distributor is selected from at least one of a shower head, a circular ring with uniform holes, or a cross shape) is provided at the end of the first inlet, and the end of the first inlet is located in the container, and the distributor is used to spray the recovered hot water.
[0024] According to an embodiment of the present invention, in step (1), the mass ratio of the mixture containing polymer and solvent or the mixture containing polymer, solvent and water entering the container from the second inlet to the recovered hot water added from the first inlet is 0.1-2.5:1.
[0025] According to an embodiment of the present invention, in step (1), the temperature of the water entering the container from the first inlet is 60-90°C.
[0026] According to an embodiment of the present invention, the temperature of the solvent gas phase is lower than 90° C. Preferably, the solvent gas phase includes solvent, water and a small amount of colloidal powder.
[0027] According to an embodiment of the present invention, in step (1), the second inlet is arranged in the solvent gas phase, or in the polymer / hot water mixture phase.
[0028] According to an embodiment of the present invention, the polymer / hot water mixture discharged from the container can be dehydrated by vibration and / or extrusion. Preferably, vibration is first used and then extrusion is used for dehydration. Preferably, the vibration method removes water through a vibrating screen. Preferably, the extrusion method is extrusion dehydration by an extrusion dehydrator. For example, in step (2), dehydration is performed by vibration and / or extrusion.
[0029] Exemplarily, step (2) is: first, the polymer / hot water mixture is passed through a vibrating screen to remove most of the hot water, thereby obtaining recovered hot water 1 and a polymer / hot water mixture with reduced water content; then, the polymer / hot water mixture with reduced water content is extruded and dehydrated by an extrusion dehydrator, thereby obtaining recovered hot water 2 and a polymer / hot water mixture with further reduced water content.
[0030] According to an embodiment of the present invention, the recovered hot water returned to the container and directly in contact with the solvent gas phase accounts for at least one third of the recovered hot water.
[0031] According to an embodiment of the present invention, the logistics in the solvent gas phase is discharged from the upper part of the container to recover the solvent therein. Preferably, the logistics in the solvent gas phase is discharged from the upper part of the container, cooled, and free water is separated to obtain the solvent therein, and the solvent can be further recycled.
[0032] According to an embodiment of the present invention, the polymer / hot water mixture in the polymer / hot water mixture phase is discharged from the bottom of the container.
[0033] According to an embodiment of the present invention, the temperature of the hot water recovered in step (3) is 5-10°C lower than the temperature of the water in the mixture containing the polymer, the solvent and the water (from the steam) in step (1).
[0034] Beneficial effects of the present invention:
[0035] The method of the present invention changes the way of reusing hot water recovered in the prior art. Specifically, part or all of the recovered hot water is directly contacted with the solvent gas phase, so that heat exchange occurs between the recovered hot water and the solvent gas phase, the amount of water carried by the solvent gas phase is reduced, the temperature of the solvent gas phase is lowered, and the problem of high temperature of the solvent gas phase is solved. In addition, the amount of rubber powder entrained in the gas phase is effectively reduced, which can significantly reduce steam and energy consumption and reduce polymer loss.
[0036] In the method of the present invention, the temperature of the recovered hot water is 5-10°C lower than the temperature of the water in the first condensation kettle containing a mixture of polymer, solvent and water (from steam). The recovered hot water with low temperature is first brought into contact with steam with high temperature, and then enters the container in the form of a mixture containing polymer, solvent and water. The recovered hot water is heated, thereby increasing the temperature of the returned recovered hot water and improving the energy utilization efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a production device diagram of the present invention;
[0038] Among them: 10. Hot water recovery pipeline, 11. distributor, 12. polymer and solvent mixture pipeline, 13. steam pipeline, 14. container, 15. agitator, 16. gas phase pipeline, 17. colloidal water pipeline. DETAILED DESCRIPTION
[0039] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0040] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0041] Example 1
[0042] like Figure 1 The device diagram shows that the container 14 is provided with an agitator 15, the top opening is connected to a gas phase pipeline 16 for discharging the solvent gas phase, and the bottom is connected to a colloidal water pipeline 17 for discharging the colloidal water (i.e., a polymer / hot water mixture). The container 14 includes three inlets, the first inlet is connected to a hot water recovery pipeline 10, and a distributor 11 (specifically a porous distributor, illustratively, the shape of the porous distributor is selected from at least one of a shower head, a ring with uniform holes, or a cross-shaped shape) is provided at the end of the hot water recovery pipeline 10 located in the container 14, and the distributor is used to spray the recovered hot water; the second inlet is connected to a polymer and solvent mixture pipeline 12 for passing a mixture containing a polymer and a solvent, or a mixture containing a polymer, a solvent, and water; the third inlet is connected to a steam pipeline 13 for passing steam.
[0043] The hot water recovery pipeline 10 is connected to the pipeline 12 for the mixture of polymer and solvent, and the steam pipeline 13 is connected to the pipeline 12 for the mixture of polymer and solvent.
[0044] The container contains a solvent gas phase and a polymer / hot water mixture phase.
[0045] The first inlet is disposed in the solvent gas phase in the container, and the first inlet is located higher than the second inlet;
[0046] The second inlet is arranged in the solvent gas phase, or in the polymer / hot water mixture phase;
[0047] The third inlet is located at the polymer / hot water mixture phase in the container.
[0048] Example 2
[0049] use Figure 1The container shown is a coagulation first kettle for preparing brominated butyl rubber. After mixing 50°C, 36t / h brominated butyl rubber n-hexane solution (containing 17wt% brominated butyl rubber and 83wt% n-hexane) from the bromination reaction unit and a certain amount of 0.7MPa steam, it enters the coagulation first kettle (or container) 14 from the second inlet of the container, and 116t / h of 85°C recycled hot water enters from the recycled hot water pipeline 10. The recycled hot water passes through the distributor 11 (i.e., the shower head) and is sprayed above the container 14. A certain amount of 0.7MPa steam is introduced from the steam pipeline 13, and the liquid phase temperature in the container is 95°C.
[0050] The n-hexane is heated and vaporized to obtain a mixture of brominated butyl rubber particles and water (i.e., particles water) and a gas containing n-hexane. The n-hexane-containing gas is recovered from the gas phase pipeline 16 out of the first condensation kettle. The temperature is 89°C, the pressure is 0.13MPa, and the flow rate is 34430kg / h. It contains 82wt% of n-hexane and 18wt% of water. The gas phase is condensed and separated to obtain n-hexane and water. The particles water at the bottom of the condensation kettle is sent to the next condensation kettle for further treatment. Compared with Comparative Example 1, the steam saving and the loss of rubber powder are shown in Table 1 below.
[0051] Example 3
[0052] The difference between Example 3 and Example 2 is that 77 t / h (about 2 / 3 of the recovered hot water) at 85°C is sprayed into the container from the shower head, and 39 t / h of the recovered hot water is mixed with a certain amount of steam and 36 t / h of brominated butyl rubber n-hexane solution (containing 17 wt% of brominated butyl rubber and 83 wt% of n-hexane) and then enters the container from the second inlet.
[0053] The gas phase pipeline 16 discharges a gas containing n-hexane at a pressure of 0.13 MPa, a temperature of 89.4° C., and a flow rate of 34653 kg / h, containing 81 wt% n-hexane and 19 wt% water. Compared with comparative example 1, the steam savings and the loss of rubber powder are shown in Table 1 below.
[0054] Example 4
[0055] The difference between Example 4 and Example 2 is that 58 t / h (about 1 / 2) of recovered hot water at 85°C is sprayed into the container from the shower head, and the recovered hot water 58 t / h is mixed with part of the steam and 36 t / h of brominated butyl rubber n-hexane solution (containing 17 wt% of brominated butyl rubber and 83 wt% of n-hexane) and then enters the container from the second inlet.
[0056] The gas phase pipeline 16 discharges a gas containing n-hexane at a pressure of 0.13 MPa, a temperature of 89.6° C., and a flow rate of 34785 kg / h, containing 80.8 wt% n-hexane and 18.2 wt% water. Compared with comparative example 1, the steam savings and the loss of rubber powder are shown in Table 1 below.
[0057] Example 5
[0058] The difference between Example 5 and Example 2 is that 39 t / h (about 1 / 3 of the recovered hot water) at 85°C is sprayed into the container from the shower head, and 77 t / h of the recovered hot water is mixed with part of the steam and 36 t / h of brominated butyl rubber n-hexane solution (containing 17 wt% of brominated butyl rubber and 83 wt% of n-hexane) and then enters the container from the second inlet.
[0059] The gas phase pipeline 16 discharges a gas containing n-hexane at a pressure of 0.13 MPa, a temperature of 89.6° C., and a flow rate of 34929 kg / h, containing 80.5 wt% n-hexane and 18.5 wt% water. Compared with comparative example 1, the steam savings and the loss of rubber powder are shown in Table 1 below.
[0060] Comparative Example 1
[0061] 116t / h of 85℃ circulating hot water, 36t / h of brominated butyl rubber hexane solution (containing 17wt% of brominated butyl rubber and 83wt% of n-hexane) and part of 0.7MPa steam are mixed and sprayed into the first condensation kettle from above the liquid surface, and part of 0.7MPa steam is introduced into the bottom of the liquid surface of the first condensation kettle. The n-hexane is vaporized by heat to obtain a mixture of brominated butyl rubber particles and water (i.e., particle water) and a gas containing n-hexane. The n-hexane-containing gas is discharged from the top of the first condensation kettle with a temperature of 95℃, a pressure of 0.13MPa and a flow rate of 35150kg / h. It contains 80wt% of n-hexane and 20wt% of water. The gas phase is decondensed to separate the n-hexane and water, and the particle water at the bottom of the kettle is sent to the next condensation kettle for further treatment.
[0062] The solvent gas phase coming out from the top of the condensation kettle is cooled, and the free water is separated and then enters the skimming pool to separate the rubber powder carried in it. Because the rubber powder contains obvious impurities, it can only be treated as waste rubber.
[0063] Table 1. Steam savings and amount of rubber residue recovered in skimming pool in Examples 2-5
[0064]
[0065]
[0066] In Table 1, "polymer content lost due to rubber dust" refers to the polymer content lost after the solvent gas phase is cooled and the free water is separated and then enters the skimming tank to separate the rubber dust carried therein. The obtained rubber dust content is the polymer content lost.
[0067] Comparing Examples 1-5 with Comparative Example 1, the top gas phase temperature of the polymer prepared by the method of the present application is significantly reduced, and the steam carried is also less, achieving the goal of saving steam. It can be seen from the above Table 1 that the method of the present invention can save steam to a great extent. In addition, in Comparative Example 1, the amount of rubber residue fished out of the skimming pool is 0.2kg / t of brominated butyl rubber, while in Examples 2, 3, 4, and 5, the rubber residue in the skimming pool is significantly less, or even no rubber residue appears.
[0068] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for producing a polymer, characterized in that: The method comprises: removing the solvent from the mixture containing the polymer and the solvent in a container under the action of steam to obtain a polymer / hot water mixture phase and a solvent gas phase; Dehydrating the polymer / hot water mixture discharged from the container to obtain recycled hot water and a polymer / hot water mixture with reduced water content; The recovered hot water is returned to the container, wherein part or all of the recovered hot water returned to the container directly contacts with the solvent gas.
2. The method according to claim 1, characterized in that The method specifically comprises: (1) adding a mixture containing a polymer and a solvent and steam into a container, removing the solvent under the action of the steam, and obtaining a polymer / hot water mixture phase and a solvent gas phase; The container comprises at least three inlets, wherein the first inlet is arranged at the solvent gas phase for adding hot water; the second inlet is used for adding a mixture containing a polymer and a solvent, or a mixture containing a polymer, a solvent and water; the third inlet is arranged at the polymer / hot water mixture phase for adding steam; wherein the first inlet is located above the second inlet; (2) dehydrating the polymer / hot water mixture discharged from the container to obtain recovered hot water and a polymer / hot water mixture with reduced water content; (3) adding part or all of the recovered hot water in step (2) into the container from the first inlet so as to directly contact the hot water with the solvent gas.
3. The method according to claim 2, characterized in that In step (3), when part of the recovered hot water is added to the container from the first inlet, another part of the recovered hot water is mixed with the mixture containing the polymer and the solvent and then added to the container from the second inlet.
4. The method according to any one of claims 1 to 3, characterized in that: In the mixture containing a polymer and a solvent, the content of the polymer is 3-30 wt%. Preferably, the polymer is at least one of cis-1,4-dibutyl rubber, solution-polymerized styrene-butadiene rubber, styrene-butadiene-styrene block copolymer or its hydrogenated product, styrene-isoprene-styrene block copolymer or its hydrogenated product, hydrogenated nitrile rubber, halogenated butyl rubber, polyisoprene rubber, and acrylonitrile-butadiene-styrene. Preferably, the solvent is an organic solvent with a boiling point below 100°C.
5. The method according to any one of claims 1 to 4, characterized in that: Part of the steam is mixed with the mixture containing the polymer and the solvent and then added to the container, and the other part of the steam is added to the container alone. Preferably, part of the recovered hot water is added to the container from the first inlet, another part of the recovered hot water, part of the steam and the mixture containing the polymer and the solvent are mixed and then added to the container from the second inlet, and another part of the steam is added to the container alone from the third inlet.
6. The method according to any one of claims 1 to 5, characterized in that: The pressure of steam entering the container is 0.2-4MPa. Preferably, in step (1), a distributor is provided at the end of the first inlet, and the end of the first inlet is located in the container. Preferably, in step (1), the mass ratio of the mixture containing polymer and solvent or the mixture containing polymer, solvent and water entering the container from the second inlet to the recovered hot water added from the first inlet is 0.1-2.5:
1. Preferably, in step (1), the temperature of the water entering the container from the first inlet is 60-90°C.
7. The method according to any one of claims 1 to 6, characterized in that: The temperature of the solvent gas phase is below 90°C. Preferably, in step (1), the second inlet is arranged in the solvent gas phase, or in the polymer / hot water mixture phase.
8. The method according to any one of claims 1 to 7, characterized in that: The recovered hot water returned to the container and in direct contact with the solvent vapor accounts for at least one third of the recovered hot water.
9. The method according to any one of claims 1 to 8, characterized in that: The material in the solvent gas phase is discharged from the upper part of the container and the solvent therein is recovered. Preferably, the polymer / hot water mixture in the polymer / hot water mixture phase is discharged from the bottom of the container.
10. The method according to any one of claims 1 to 9, characterized in that: The temperature of the hot water recovered in step (3) is 5-10° C. lower than the temperature of the water in the mixture containing the polymer, the solvent and water in step (1).