Water-based acrylic emulsion, preparation method thereof and application of water-based acrylic emulsion in automobile lamp antifogging coating

Through the use of aqueous acrylic emulsion, the sag and high VOC problems of anti-fog coating of the headlights are solved, and good adhesion and long-term anti-fog effect are achieved on the headlights, which meets the high adhesion and durability of the headlight industry. Require.

CN119080996APending Publication Date: 2024-12-06HUNAN SONGJING ADVANCED SURFACE TREATMENT & FUNCTIONAL COATING RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411416719.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing anti-fog coatings of the headlights have problems with sagging and high VOC content, and are difficult to adhere to the headlights, which cannot meet the requirements of long-term anti-fog and high adhesion.

Method used

Using aqueous acrylic emulsion as the main composition of anti-fog coating, the combination of specific monomers and emulsifiers provides good adhesion and anti-fog properties to the plastic substrate, and controls the VOC content through the solvent-free synthesis process to ensure coating. uniformity and durability of the layer.

Benefits of technology

It realizes anti-fog effect without sag on the headlights, meets the performance requirements for long-term use, and reduces the VOC content, providing good adhesion to the headlights and high gloss transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005079653720000081
    Figure BDA0005079653720000081
  • Figure BDA0005079653720000111
    Figure BDA0005079653720000111
  • Figure BDA0005079653720000121
    Figure BDA0005079653720000121
Patent Text Reader

Abstract

The invention relates to the technical field of car lamp glass, in particular to a water-based acrylic emulsion, a preparation method thereof and application of the water-based acrylic emulsion in car lamp antifogging paint. The water-based acrylic emulsion is prepared from the following raw materials in parts by weight: 3 to 7 parts of acrylic acid, 60 to 100 parts of methyl methacrylate, 5 to 15 parts of hydroxyethyl methylacrylate, 5 to 20 parts of N-hydroxy acrylamide, 1 to 4 parts of sodium vinylsulfonate, 1 to 2 parts of emulsifier, 5 to 15 parts of water, 10 to 3 parts of acrylamide and 20 to 30 parts of tetrahydrofuran acrylate. By adopting the thought, the VOC of the anti-fog coating can be zero, no surfactant exists, the anti-fog performance is lasting, meanwhile, no small molecules are separated out in the using process, the sagging phenomenon is avoided, and the performance requirement for long-term use of automobile lamps can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a water-based acrylic emulsion and a preparation method thereof and application thereof in anti-fog coating for vehicle lamps. Background Art

[0002] Anti-fog coatings are widely used in car lights. Since car lights are special-shaped products, there are many problems with UV curing, such as incomplete curing in some areas. The thermosetting anti-fog products for car lights currently on the market mainly include Nippon Ink, Fujikura and South Korea's KCC. However, the products on the market are all solvent-based coatings, such as NOF's 5000 series. This type of coating has a low solid content of only about 10%, and the remaining components are organic solvents, so the VOC content is relatively high. Similar situations also exist in the following existing technologies:

[0003] Patent CN 114867793A discloses an anti-fog coating composition capable of forming the following anti-fog coating film, wherein the anti-fog coating film does not cause appearance changes such as water marks, is firmly attached to the surface of various substrates including plastic substrates, and exerts an anti-fog effect for a long time. The invention provides an anti-fog coating composition, which contains: elongated colloidal silica; and a silane derivative compound mixture, which at least contains a silane derivative compound having a polyethylene glycol chain in the molecule and a silane derivative compound having an epoxy group in the molecule. However, the patent still uses a large amount of solvents, and the VOC content is relatively high.

[0004] Patent CN114015317A discloses a method for preparing an anti-fog coating in the field of automotive glass. The raw materials for preparing the anti-fog coating of the patent include: a hydrophilic copolymer, an epoxy resin, a coupling agent, a curing agent and a first solvent; the raw materials for preparing the hydrophilic copolymer include: a hydrophilic monomer, an initiator and a second solvent; the solubility of the epoxy resin in water is greater than or equal to 90%; the solubility of the hydrophilic copolymer in water is greater than or equal to 90%. The anti-fog coating of the invention can be directly coated on the glass substrate in a single layer, which simplifies the production process, reduces production costs, and has a good anti-fog effect and is not easy to peel off. However, due to the difference between the glass substrate and the headlight substrate, the anti-fog coating that can be attached to the glass is difficult to attach to the headlight. In addition, a large amount of solvents are used in the preparation process of the hydrophilic copolymer, which cannot solve the problem of VOC.

[0005] Patent CN1263815C discloses an anti-fog coating composition for forming an anti-fog coating film without producing water flow marks, comprising a block or graft copolymer and an acidic alkyl phosphate, wherein the copolymer comprises a hydrophilic polymer part formed by a vinyl monomer having a cross-linking functional group and a water-soluble vinyl monomer, and a hydrophobic polymer part formed by a non-water-soluble vinyl monomer. The patent adopts a large amount of hydrophilic monomers to provide an anti-fog effect. Although the increase of hydrophilic monomers will provide anti-fog performance, it also brings about the negative effect of poor coating film performance. For example, the anti-fog performance test of water vapor in the patent is 40°C water vapor and the waterproof performance is only soaked in 40°C water for 1 hour. These conditions are relatively simple and easy to meet, but they cannot meet the current requirements of 80°C fumigation and 40°C water resistance for 240 hours in the automotive lighting industry.

[0006] Patent CN118459652A discloses a long-lasting super hydrophilic anti-fog self-cleaning polyacrylate emulsion and its preparation method and application. The preparation method of the polyacrylate emulsion is to first prepare a pre-emulsion, then mix and disperse an anionic emulsifier, a nonionic emulsifier and water evenly, add 10% to 20% of the total mass of the pre-emulsion, mix evenly, heat to 75°C to 85°C, add an initiator; then drop the remaining pre-emulsion and the initiator solution accounting for 0.2% to 0.6% of the total monomer amount into the system for reaction, cool to 25 to 60°C, add a nanoparticle dispersion, adjust the pH to 7 to 8, then add a second external cross-linking monomer, mix evenly, filter, and obtain a long-lasting super hydrophilic anti-fog self-cleaning polyacrylate emulsion. The invention can achieve a long-lasting anti-fog self-cleaning effect without any hydrophilic additives. The coating also has good mechanical properties and no VOC, and the comprehensive performance is excellent. However, during the implementation of the invention, a variety of cross-linked monomers are used and chelated with inorganic materials to obtain long-lasting anti-fog performance, but the durability of the anti-fog can only be maintained for about 6 months, which is difficult to meet the 3-year anti-fog effectiveness requirement of the automotive lighting industry. Summary of the invention

[0007] The purpose of the present invention is to provide a water-based acrylic emulsion that does not produce sagging, a preparation method thereof, and an application of the emulsion in anti-fog coatings for vehicle lamps.

[0008] In order to achieve the above object, the technical solution of the present invention is as follows:

[0009] A water-based acrylic emulsion, the raw materials of which are measured by weight: 3-7 parts of acrylic acid, 60-100 parts of methyl methacrylate, 5-15 parts of hydroxyethyl methacrylate, 5-20 parts of N-hydroxyacrylamide, 1-4 parts of sodium vinyl sulfonate, 1-2 parts of emulsifier, 5-15 parts of water, 10-3 parts of acrylamide and 20-30 parts of tetrahydrofuran acrylate.

[0010] In one preferred embodiment, the raw materials of the aqueous acrylic emulsion include, by weight, 5 parts of acrylic acid, 80 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 7.5 parts of N-hydroxyacrylamide, 2.5 parts of sodium vinyl sulfonate, 1.5 parts of emulsifier, 10 parts of water, 20 parts of acrylamide and 25 parts of tetrahydrofuran acrylate.

[0011] In a preferred embodiment, the N-hydroxyacrylamide is one or both of N-hydroxymethylacrylamide and N-hydroxyethylacrylamide.

[0012] In a preferred embodiment, the acrylamide is one or both of acrylamide and methacrylamide.

[0013] In a preferred embodiment, the acrylic acid is one or both of acrylic acid and methacrylic acid.

[0014] Methyl methacrylate monomer provides adhesion to plastic substrates; tetrahydrofuran acrylate monomer provides adhesion to PC.

[0015] In a preferred embodiment, the emulsifier is a phosphate surfactant.

[0016] The phosphate surfactant is used as an emulsifier. On the one hand, 1. the monomer contains a double bond, which can react to the main chain of the molecule during the synthesis process; 2. the phosphate surfactant can provide a good anti-fog effect; 3. the monomer contains only one double bond, which will not cause explosion during the synthesis process to cause product gelation.

[0017] In a preferred embodiment, the phosphate ester surfactant is a phosphate ester of aliphatic ethoxyethanol with a double bond.

[0018] In a preferred embodiment, the phosphate ester surfactant is Rhodafac RS-710.

[0019] Other phosphates available on the market contain more double bonds, which will not only cause explosion during the synthesis process but also lead to gelation of the product.

[0020] Based on the same inventive concept, the present invention also claims a method for preparing the aqueous acrylic emulsion, comprising the following steps:

[0021] S1. In a protective gas atmosphere, add water, sodium vinyl sulfonate, acrylic acid, part of methyl methacrylate, hydroxyethyl methacrylate, and N-hydroxymethyl acrylamide, mix well, and heat to 40-60°C;

[0022] S2, adding part of the initiator, reacting at 75-85°C for 20-40 minutes to obtain emulsion 1;

[0023] S3, dropping an emulsifier, acrylamide, a mixed solution of the remaining methyl methacrylate and tetrahydrofuran acrylate into emulsion 1, and simultaneously dropping the remaining initiator; and then reacting at 75-85° C. for 2-3 hours to obtain the aqueous acrylic emulsion.

[0024] The hydrophilic resin obtained by the above process is solvent-free and can well control the VOC content of the coating.

[0025] In a preferred embodiment, the protective gas is nitrogen.

[0026] In a preferred embodiment, the part of methyl methacrylate is 20-30 wt % of methyl methacrylate.

[0027] Experiments have shown that, in the present invention, adding methyl methacrylate all at once will lead to too high a reactivity ratio and uneven polymerization; adding methyl methacrylate in portions can effectively avoid the problem of too high a reactivity ratio and make various monomers more evenly distributed on the molecular chain.

[0028] In a preferred embodiment, the initiator is sodium persulfate solution.

[0029] In one preferred embodiment, the initiator is a 0.5-1.5 wt % sodium persulfate aqueous solution.

[0030] In one preferred embodiment, the amount of the initiator added is 45-55 parts.

[0031] In one preferred embodiment, the portion of initiator is 15-25 wt % of the initiator.

[0032] In view of the stepwise addition of the monomers, the initiator is also added stepwise to improve the uniformity of the distribution of the polymerization monomers.

[0033] Based on the same inventive concept, the present invention also claims to protect the use of the aqueous acrylic emulsion in the preparation of anti-fog coatings.

[0034] Based on the same inventive concept, the present invention also claims to protect the use of the aqueous acrylic emulsion in the preparation of anti-fog coating for vehicle lamps.

[0035] An anti-fog coating for vehicle lamps comprises the water-based acrylic emulsion.

[0036] In one of the preferred embodiments, the anti-fog coating for vehicle lamps further comprises, by weight: 0.05-0.15 parts of a wetting agent and 0.05-0.15 parts of a leveling agent.

[0037] Based on the same inventive concept, the present invention also claims to protect a method for preparing the anti-fog coating for vehicle lamps, comprising: dispersing a water-based acrylic emulsion, a wetting agent, and a leveling agent at 800-1000R / min for 30-40min to obtain the anti-fog coating for vehicle lamps.

[0038] The method for using the anti-fog coating for vehicle lamps is as follows: spraying the anti-fog coating for vehicle lamps on a vehicle lamp substrate with a wet film thickness of 20-30 microns, and baking the coating at 100-140° C. for 20-30 minutes after spraying to obtain an anti-fog vehicle lamp.

[0039] In one preferred embodiment, the vehicle light substrate is PC or PMMA.

[0040] The present invention will be further explained below:

[0041] In the resin formula, N-hydroxymethyl acrylamide provides cross-linking during heat curing, thereby improving the mechanical properties of the coating. Methyl methacrylate and tetrahydrofuran acrylate provide adhesion to plastic substrates, such as PC, PMMA, etc. Monomer phosphate surfactants and SVS can provide good anti-fog performance, and acrylamide can provide absorption of water vapor during fumigation, thereby increasing the water content of the anti-fog coating and forming a uniform water film. The hydrophilic groups of methacrylic acid and HEMA can supplement the anti-fog performance. Through the overall design of the resin molecular structure, the monomers that provide anti-fog performance are uniformly reacted to the main chain of the acrylic resin, thereby avoiding the free surfactant in the anti-fog coating from dissolving in the water film during the fumigation process, which brings about the flow mark problem after the anti-fog water film dries, thereby affecting the appearance of the anti-fog coating.

[0042] The beneficial effects of the present invention are:

[0043] (1) Using water-based acrylic emulsion resin as the main composition of anti-fog coating can achieve good adhesion to plastic substrates such as PC to meet the long-term use standards of the automotive lighting industry. On the other hand, the acrylic emulsion synthesis process can be completely water-based and solvent-free, thereby effectively controlling VOC. Finally, acrylic resin can provide better transparency and high gloss to meet the requirements of transparency of automotive lighting.

[0044] (2) The anti-fog coating obtained by the design concept of the present invention is free of surfactants and has long-lasting anti-fog performance. At the same time, no small molecules are precipitated during use, so no sagging phenomenon occurs, which can meet the performance requirements of long-term use of automobile lamps. DETAILED DESCRIPTION

[0045] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0047] the term

[0048] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:

[0049] The optional scope of the terms "and / or", "or / and", and "and / or" used in this article includes any one of two or more related listed items, and also includes any and all combinations of the related listed items, said any and all combinations include any combination of any two related listed items, any more related listed items, or all related listed items.

[0050] Herein, "one or several" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0051] As used herein, "combination thereof", "any combination thereof", "any combination thereof" etc. include all suitable combinations of any two or more of the listed items.

[0052] Herein, “preferred” is only used to describe an implementation method or example with better effects, and it should be understood that it does not constitute a limitation on the scope of protection of the present invention.

[0053] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0054] In the present invention, reference to a numerical range includes both endpoints of the numerical range unless otherwise specified.

[0055] The percentage content involved in the present invention, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.

[0056] The percentage concentrations involved in the present invention, unless otherwise specified, refer to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.

[0057] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.

[0058] The "solubility" referred to in the present invention, unless otherwise specified, refers to the mass of a solute dissolved in water at 20°C when the solute reaches a saturated state.

[0059] Example 1

[0060] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0061] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 10 g of hydroxyethyl methacrylate, 7.5 g of N-hydroxymethyl acrylamide, and 2.5 g of hydrophilic monomer sodium vinyl sulfonate (SVS) into the reactor, start stirring, and slowly heat to 50°C;

[0062] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0063] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0064] 4. Mix 1.5 g of emulsifier RS710, 10 g of deionized water, 20 g of acrylamide, 60 g of methyl methacrylate (MMA) and 25 g of tetrahydrofuran acrylate (THFA) evenly, and then add them dropwise to the reactor for 3 hours; at the same time, add 40 g of 1% sodium persulfate for 3 hours, and then keep it at 80°C for 2 hours;

[0065] 5. After the insulation is completed, the reactor is cooled to 50° C., the material is discharged, filtered with a 400-mesh filter cloth, and parameters such as solid content, viscosity and pH value are tested to obtain a water-based acrylic emulsion anti-fog resin 1.

[0066] Comparative Example 1

[0067] Compared with Example 1, without adding SVS

[0068] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0069] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 22.5 g of methyl methacrylate, 10 g of hydroxyethyl methacrylate, and 7.5 g of N-hydroxymethyl acrylamide into the reactor, start stirring, and slowly heat to 50°C;

[0070] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0071] When the temperature was raised to 80°C, resin precipitated in the reactor and the reaction could not proceed further;

[0072] Comparative Example 2

[0073] Compared with Example 1, no N-hydroxymethyl acrylamide was added.

[0074] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0075] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 27.5 g of methyl methacrylate, 10 g of hydroxyethyl methacrylate, and 2.5 g of hydrophilic monomer SVS into the reactor, start stirring, and slowly heat to 50°C;

[0076] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0077] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0078] 4. Mix 1.5g of emulsifier RS710, 10g of deionized water, 20g of acrylamide, 60g of MMA and 25g of THFA, and add them dropwise to the reactor for 3 hours. At the same time, add 40g of 1% sodium persulfate for 3 hours, and then keep it at 80°C for 2 hours.

[0079] 5. After the insulation is completed, the reactor is cooled to 50°C, the material is discharged, filtered with a 400-mesh filter cloth, and the solid content, viscosity, pH value and other parameters are tested to obtain a water-based acrylic emulsion anti-fog resin 2.

[0080] Comparative Example 3

[0081] Compared with Example 1, RS710 did not react to the resin molecular weight.

[0082] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0083] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 7.5 g of N-hydroxymethyl acrylamide, 10 g of hydroxyethyl methacrylate, and 2.5 g of hydrophilic monomer SVS into the reactor, start stirring, and slowly heat to 50°C;

[0084] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0085] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0086] 4. Mix 10g deionized water, 20g acrylamide, 60g MMA and 25g THFA evenly, and then add them to the reactor dropwise for 3 hours. At the same time, add 40g 1% sodium persulfate dropwise for 3 hours, and then keep it at 80℃ for 2 hours.

[0087] 5. After the insulation is completed, the reactor is cooled to 50°C, 1.5 g of emulsifier RS710 is added, and the mixture is dispersed for 30 minutes. The mixture is discharged and filtered with a 400-mesh filter cloth, and parameters such as solid content, viscosity and pH value are tested to obtain a water-based acrylic acid.

[0088] Emulsion anti-fog resin 3

[0089] Comparative Example 4

[0090] Compared with Example 1, the non-reactive emulsifier sodium dodecylbenzene sulfonate is used.

[0091] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0092] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 7.5 g of N-hydroxymethyl acrylamide, 10 g of hydroxyethyl methacrylate, and 2.5 g of sodium dodecylbenzene sulfonate into the reactor, start stirring, and slowly heat to 50°C;

[0093] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0094] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0095] 4. Mix 1.5g of emulsifier sodium dodecylbenzene sulfonate, 10g of deionized water, 20g of acrylamide, 60g of MMA and 25g of THFA, and add them dropwise to the reactor over a period of 3 hours. At the same time, add 40g of 1% sodium persulfate over a period of 3 hours, and then keep the mixture at 80°C for 2 hours.

[0096] 5. After the insulation is completed, the reactor is cooled to 50° C., the material is discharged, filtered with a 400-mesh filter cloth, and parameters such as solid content, viscosity and pH value are tested to obtain a water-based acrylic emulsion anti-fog resin 4.

[0097] The water-based acrylic emulsion anti-fog resin was tested according to the following formula and performance, and the results are shown in the following table:

[0098] Table 1 Anti-fog coating formulation and performance test results

[0099]

[0100] The test methods in the table are as follows:

[0101] Repeated fumigation test: The water surface is 10cm away from the anti-fog coating. After the coating is subjected to 80℃ steam test for 15s, the sample / sample piece is placed in a standard environment until it is fully dried. This is one cycle. Perform 60 cycles. Open the water bath lid before fumigation and close it after fumigation. After 60 cycles, observe whether there is fogging or sagging.

[0102] Anti-fog effectiveness: The water surface is 10 cm away from the anti-fog coating. After the coating is subjected to 80°C steam test for 30 seconds, the sample / sample is placed in a standard environment until it is fully dried. This is one cycle. Perform two cycles to observe whether sagging occurs.

[0103] Sagging test: The water surface is 10cm away from the anti-fog coating, and the coating is subjected to a 60℃ steam test. The coating is fumigated for 2 minutes, 5 minutes and 10 minutes respectively. After fumigation, the sample / sample is placed in a standard environment until it is fully dried and observed for sagging.

[0104] Water resistance test: Immerse the lens in (40±2)℃ water for 240h, then store it vertically in a standard environment for 1h, immediately conduct an exhalation performance test, and after storing it in a standard environment for 24h, conduct an adhesion performance test to observe whether fogging occurs and whether the adhesion decreases.

[0105] Data analysis: In Example 1, the emulsifiers SVS and RS710 are both reacted to the main chain of the resin to provide good anti-fog performance, and N-hydroxymethyl acrylamide is used as a cross-linking monomer to improve the physical properties of the paint film after cross-linking and curing; in Comparative Example 1, there is a lack of hydrophilic monomers, and the resin cannot synthesize an aqueous acrylic emulsion; in Comparative Example 2, there is no cross-linking monomer, the paint film cannot be cross-linked during the later curing, the coating has poor physical properties and is very easy to dissolve; in Comparative Example 3, RS710 is not reacted to the main chain of the molecule, and the surfactant will dissolve in the water film during the fumigation process, resulting in a decrease in the water resistance of the anti-fog coating and sagging; in Comparative Example 4, all sodium dodecylbenzene sulfonate that does not participate in the reaction is used as an emulsifier, and the emulsifier will exist in the paint film in a free form, which also results in NG in the water resistance test and the generation of sagging.

[0106] Example 2

[0107] Compared with Example 1, hydroxyethyl methacrylate was replaced with hydroxypropyl acrylate.

[0108] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0109] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 10 g of hydroxypropyl methacrylate, 7.5 g of N-hydroxymethyl acrylamide, and 2.5 g of hydrophilic monomer SVS into the reactor, start stirring, and slowly heat to 50°C;

[0110] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0111] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0112] 4. Mix 1.5g RS710, 10g deionized water, 20g acrylamide, 60g MMA and 25g THFA, and add them to the reactor dropwise for 3 hours. At the same time, add 40g 1% sodium persulfate dropwise for 3 hours, and then keep it at 80℃ for 2 hours.

[0113] 5. After the insulation is completed, the reactor is cooled to 50°C, the material is discharged, filtered with a 400-mesh filter cloth, and the parameters such as solid content, viscosity and pH value are tested to obtain a water-based acrylic emulsion anti-fog resin 5.

[0114] Example 3

[0115] Compared with Example 1, hydroxyethyl methacrylate was replaced with hydroxyethyl acrylate

[0116] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0117] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 10 g of hydroxypropyl acrylate, 7.5 g of N-hydroxymethyl acrylamide, and 2.5 g of hydrophilic monomer SVS into the reactor, start stirring, and slowly heat to 50°C;

[0118] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0119] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0120] 4. Mix 1.5g RS710, 10g deionized water, 20g acrylamide, 60g MMA and 25g THFA, and add them to the reactor dropwise for 3 hours. At the same time, add 40g 1% sodium persulfate dropwise for 3 hours, and then keep it at 80℃ for 2 hours.

[0121] 5. After the insulation is completed, the reactor is cooled to 50°C, the material is discharged, filtered with a 400-mesh filter cloth, and the parameters such as solid content, viscosity and pH value are tested to obtain a water-based acrylic emulsion anti-fog resin 6.

[0122] Example 4

[0123] Compared with Example 1, hydroxyethyl methacrylate was replaced with hydroxypropyl methacrylate.

[0124] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0125] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 10 g of hydroxypropyl methacrylate, 7.5 g of N-hydroxymethyl acrylamide, and 2.5 g of hydrophilic monomer SVS into the reactor, start stirring, and slowly heat to 50°C;

[0126] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0127] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0128] 4. Mix 1.5g RS710, 10g deionized water, 20g acrylamide, 60g MMA and 25g THFA, and add them to the reactor dropwise for 3 hours. At the same time, add 40g 1% sodium persulfate dropwise for 3 hours, and then keep it at 80℃ for 2 hours.

[0129] 5. After the insulation is completed, the reactor is cooled to 50°C, the material is discharged, filtered with a 400-mesh filter cloth, and the parameters such as solid content, viscosity and pH value are tested to obtain a water-based acrylic emulsion anti-fog resin 7.

[0130] Comparative Example 5

[0131] Compared with Example 1, hydroxyethyl methacrylate was replaced with butyl methacrylate without hydroxyl group.

[0132] 1. Pass a certain amount of nitrogen into the four-necked flask for protection;

[0133] 2. Add 790 g of deionized water into a four-necked flask, weigh 5 g of methacrylic acid, 20 g of methyl methacrylate, 10 g of butyl methacrylate, 7.5 g of N-hydroxymethyl acrylamide, and 2.5 g of hydrophilic monomer SVS into the reactor, start stirring, and slowly heat to 50°C;

[0134] 3. After 30 minutes of dispersion and uniform mixing, add 10g of 1% sodium persulfate solution into the reactor and slowly

[0135] The temperature was raised to 80°C and the reaction was continued for 30 minutes to obtain a milky white emulsion with blue light;

[0136] 4. Mix 1.5g RS710, 10g deionized water, 20g acrylamide, 60g MMA and 25g THFA, and add them to the reactor dropwise for 3 hours. At the same time, add 40g 1% sodium persulfate dropwise for 3 hours, and then keep it at 80℃ for 2 hours.

[0137] 5. After the insulation is completed, the reactor is cooled to 50°C, the material is discharged, filtered with a 400-mesh filter cloth, and the solid content, viscosity, pH value and other parameters are tested to obtain a water-based acrylic emulsion anti-fog resin 8.

[0138] The water-based acrylic emulsion anti-fog resin was tested according to the following formula and performance, and the results are shown in the following table:

[0139] Table 2 Anti-fog coating formulation and performance test results

[0140]

[0141]

[0142] Data analysis: In Examples 2-4, replacing different hydroxyl acrylic acid esters has little effect on the anti-fog performance of the coating, while in Comparative Example 5, which does not contain hydroxyl acrylic acid ester monomers, the water resistance of the anti-fog coating decreases slightly, which is mainly because the hydroxyl group also provides a certain hydrophilic effect.

[0143] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0144] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A water-based acrylic emulsion, characterized in that: The raw materials include, by weight, 3-7 parts of acrylic acid, 60-100 parts of methyl methacrylate, 5-15 parts of hydroxyethyl methacrylate, 5-20 parts of N-hydroxyacrylamide, 1-4 parts of sodium vinyl sulfonate, 1-2 parts of emulsifier, 5-15 parts of water, 10-3 parts of acrylamide and 20-30 parts of tetrahydrofuran acrylate.

2. The aqueous acrylic emulsion according to claim 1, characterized in that The raw materials of the aqueous acrylic emulsion include, by weight, 5 parts of acrylic acid, 80 parts of methyl methacrylate, 10 parts of hydroxyethyl methacrylate, 7.5 parts of N-hydroxyacrylamide, 2.5 parts of sodium vinyl sulfonate, 1.5 parts of emulsifier, 10 parts of water, 20 parts of acrylamide and 25 parts of tetrahydrofuran acrylate.

3. The aqueous acrylic emulsion according to claim 1, characterized in that The acrylic acid is one or both of acrylic acid and methacrylic acid; the N-hydroxyacrylamide is one or both of N-hydroxymethylacrylamide and N-hydroxyethylacrylamide; and the acrylamide is one or both of acrylamide and methacrylamide.

4. The aqueous acrylic emulsion according to claim 1, characterized in that The emulsifier is a phosphate surfactant; preferably, the phosphate surfactant is a phosphate ester of aliphatic ethoxyethanol with a double bond.

5. The method for preparing the aqueous acrylic emulsion according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. In a protective gas atmosphere, add water, sodium vinyl sulfonate, acrylic acid, part of methyl methacrylate, hydroxyethyl methacrylate, and N-hydroxymethyl acrylamide, mix well, and heat to 40-60°C; S2, adding part of the initiator, reacting at 75-85°C for 20-40 minutes to obtain emulsion 1; S3, dropping an emulsifier, acrylamide, a mixed solution of the remaining methyl methacrylate and tetrahydrofuran acrylate into emulsion 1, and simultaneously dropping the remaining initiator; and then reacting at 75-85° C. for 2-3 hours to obtain the aqueous acrylic emulsion.

6. The preparation method according to claim 5, characterized in that: The protective gas is nitrogen.

7. The preparation method according to claim 5, characterized in that: The part of methyl methacrylate is 20-30wt% of methyl methacrylate.

8. The preparation method according to claim 5, characterized in that: The initiator is a sodium persulfate solution; the partial initiator is 15-25wt% of the initiator.

9. An anti-fog coating for vehicle lights, characterized in that: The invention comprises the aqueous acrylic emulsion according to any one of claims 1 to 4.

10. The anti-fog coating for vehicle lamps according to claim 9, characterized in that: The anti-fog coating for vehicle lamps further comprises, by weight: 0.05-0.15 parts of a wetting agent and 0.05-0.15 parts of a leveling agent.